Solid welding wire, high-wear-resistance composite stepping plate and manufacturing methods of solid welding wire and high-wear-resistance composite stepping plate

Through modified solid core welding wire and tungsten inert gas shielded welding technology, the problem of difficulty in welding base materials with high alloy element content and high carbon equivalent is solved, a wear-resistant surface is formed, the comprehensive performance of the stepper plate is improved, and the surface problems are solved Problems such as pits, edge pressure feed and cracks are eliminated and the service life is improved.

CN118809092AActive Publication Date: 2024-10-22TAIER HEAVY INDUSTRY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410855138.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-22
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively solve the problems of difficult welding and poor welding performance of base materials with high alloy element content and high carbon equivalent. Especially when the carbon equivalent is greater than 0.6%, cracks are prone to occur during welding and the toughness of the weld metal decreases. question.

Method used

Modified solid core welding wire is used, modified by nano-rare earth oxide, combined with tungsten inert gas shielded welding method, layered surfacing is formed to form a wear-resistant surface, and the welding parameters are controlled to form a 'rigid and soft' composite structure to improve welding. performance.

Benefits of technology

It significantly improves the anti-wear, anti-corrosion, impact resistance and anti-fatigue properties of the stepping plate, solves the problems of pits, edge pressure and cracks on the surface of the traditional stepping plate, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118809092A_ABST
    Figure CN118809092A_ABST
Patent Text Reader

Abstract

The invention discloses a solid welding wire, a high-wear-resistance composite stepping plate and manufacturing methods of the solid welding wire and the high-wear-resistance composite stepping plate, and belongs to the technical field of composite stepping plates. The high-wear-resistant composite stepping plate is composed of a base body part and a wear-resistant composite surfacing surface, the wear-resistant surface adopts a solid welding wire containing nano rare earth oxide particles, and the solid welding wire is compounded on the base body material in a surfacing manner, so that a composite structure combining hardness and softness is formed. In order to solve the problems of high alloy element content, high carbon equivalent, high grain sensitivity and high welding difficulty of a base material, the wear-resistant surface meeting the comprehensive performance requirement is prepared by modifying a welding wire, selecting a proper welding mode and regulating and controlling welding parameters.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite stepping plates, and more specifically, relates to a solid welding wire, a highly wear-resistant composite stepping plate and a manufacturing method thereof. Background Art

[0002] With the increasing market demand for product quality and the continuous development of the steel industry, steel rolling technology has been continuously updated and upgraded, and the requirements for the performance of stepping plates have become increasingly higher.

[0003] During the strip rolling process, the energy generated by dynamic pressure, static pressure and impact will be transmitted to the roll neck through the roller body, from the roll neck to the bearing seat, and then from the bearing seat to the mill stepping plate; limited by the size of the support roller bearing box, the contact area between the stepping plate and the arc pad under the support roller bearing seat is small, the force is large, the impact force is large, and the contact stress is large; in addition, the corrosion of cooling water and the abrasive wear and friction caused by the oxidation scales on the steel plate surface cause the stepping plate to be subjected to the sliding friction of the bearing seat and the impact from the bearing seat during operation. These factors will cause pits, edge pressure feedback and cracks on the surface of the stepping plate, and even fracture. Deterioration such as pits and cracks on the surface of the stepping plate will cause the difference in stiffness values ​​on both sides of the mill to exceed the standard. Under a certain rolling pressure, the elastic deformation of the mill is different, resulting in a certain deviation in the roll gap on both sides, affecting the shape of the intermediate slab. Therefore, the safety and stability of the stepping plate plays a decisive role in the stability of the four-roll mill and the shape quality of the intermediate slab.

[0004] After searching, patent CN105149810A discloses a welding method for preventing high carbon equivalent strip weld breakage. The welds between the strips are welded by laser welding. The welding wire composition used in the laser welding is: C 0.08-0.09%, Si0.7-0.88%, Mn 1.3-1.47%, P≤0.011%, S≤0.008%, Cu 0.11-0.14%, Ni0.004-0.007%, Cr0.040-0.046%, and the balance is Fe; the welding machine power used is 9000-11000W, the welding speed of the welding machine is 2-6m / min, the wire feeding speed is 2-7m / min, the annealing current is 100-160A, and the annealing temperature is 500-900℃. The laser welding method for preventing the high carbon equivalent strip weld from breaking provided by the present invention solves the technical problem that the weld of the high carbon equivalent strip steel with a carbon equivalent greater than 0.5% is prone to breaking. The patent is used for connecting and welding between strip steels, and uses a high energy density laser beam as a heat source for welding. The use of high energy density for surfacing welding of small diameter welding wires is prone to uneven distribution of welding materials.

[0005] Patent CN104923935A discloses a welding method for high alloy content and large thickness continuous casting slabs, including the following steps: a. Using at least two high alloy content continuous casting slabs as raw materials, mechanical milling is used to remove the oxide layer on the surface to be joined of the continuous casting slabs, and an L-shaped step is processed on the edge of the joint surface of the continuous casting slabs; b. Stainless steel transition layer is surfacing on the L-shaped step by stainless steel strip surfacing, and the continuous casting slabs are processed into rectangular blocks of the same size by mechanical milling; c. The continuous casting slabs are aligned and stacked, and the continuous casting slabs are positioned and welded by arc welding; d. The continuous casting slabs are placed in a vacuum chamber, and the side seams between the continuous casting slabs are welded by electron beam under high vacuum. The continuous casting slabs of this patent use stainless steel welding materials with low welding crack tendency for submerged arc welding transition, and vacuum electron beam welding is performed after spot welding positioning.

[0006] Patent CN109868342A discloses a method for improving the toughness of the heat affected zone of high carbon equivalent steel plate welding by using rare earth. The method comprises a converter smelting step, a LF refining step, a RH refining step, a continuous casting step, a hot rolling step and a heat treatment step in sequence. A certain amount of rare earth Ce alloy is added to the molten steel during the RH refining process, and the inclusions in the molten steel are modified by rare earth to be rare earth inclusions, while fine new rare earth inclusions are generated in the molten steel, and the dispersion distribution of the rare earth inclusions is controlled. The newly generated fine and dispersed rare earth Ce-containing inclusions in the molten steel and the original inclusions modified by rare earth inhibit the growth of the original austenite grains in the heat affected zone during welding. At the same time, the addition of rare earth also delays the bainite transformation of the welding heat affected zone and inhibits the formation of upper bainite, thereby greatly improving the toughness of the heat affected zone of the high carbon equivalent thick plate welding. This patent adds rare earth alloys when smelting raw materials to form original inclusions, but the original rare earth inclusions in the molten steel have low specific gravity and are easy to float, poor wettability, and are easy to agglomerate due to their small particle size, which affects the uniformity of the inclusion distribution and thus affects the quality stability of the welding heat affected zone. Summary of the invention

[0007] 1. Problem to be solved

[0008] In view of the difficulty in welding existing substrates with high alloy element content and high carbon equivalent, the present invention provides a method for manufacturing a composite stepping plate, which can prepare a wear-resistant surface that meets comprehensive performance requirements by modifying solid welding wire, selecting a suitable welding method, and adjusting welding parameters. The prepared composite stepping plate forms a composite structure that is both rigid and flexible, effectively improving the performance of the stepping plate during use.

[0009] The solid welding wire used for welding is modified with nano rare earth oxides, which is beneficial to improving the comprehensive mechanical properties of the solid welding wire and the wear-resistant surface.

[0010] 2. Technical solution

[0011] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0012] A method for manufacturing a composite stepping plate, the specific steps are as follows:

[0013] S1. Making the base part of the stepping plate: making the base part by forging and rough machining;

[0014] S2. Heat treatment of the base part: Improve the organization and mechanical properties of the base part through heat treatment to facilitate welding and mechanical processing;

[0015] S3. Opening the wear-resistant surface groove of the stepping plate: the wear-resistant surface groove is processed by CNC milling;

[0016] S4, surfacing wear-resistant composite surfacing surface: surfacing the solid welding wire to the surfacing groove of the wear-resistant surface, and then performing post-weld heat treatment;

[0017] S5, finishing: processing the stepping plate after surfacing welding to the finished product size by milling and grinding;

[0018] S6. Testing: Conduct hardness and metallographic structure testing on the finished composite stepping plate.

[0019] Furthermore, the components and weight percentages of the matrix in step S1 are: C: 0.18%-0.24%, Si: 0.10%-0.50%, Mn: 0.40%-0.90%, Cr: 11.00%-12.50%, Mo: 0.80%-1.20%, Ni: 0.30%-0.80%, V: 0.25%-0.35%, S≤0.025%, P≤0.025%, and the rest is Fe.

[0020] Furthermore, in step S2, after the base part is manufactured, the base part is heat treated, and the heat treatment process adopts quenching and tempering to adjust the hardness of the base part so that the hardness of the base part reaches HB240-260.

[0021] The specific process of heat treatment is as follows:

[0022] Quenching: slowly heat to the quenching temperature of 1010-1040℃, then put into the oil pool for quenching treatment, and quench and cool to below 200℃;

[0023] Tempering: After quenching, it needs to be put back into the furnace and heated to 670-690℃ within 20-30min, and kept warm for 10-12 hours, then oil-cooled to 200℃, and then air-cooled to room temperature, so that the hardness of the treated matrix reaches HB240-260.

[0024] Furthermore, the wear-resistant surface surfacing area in step S3 is a groove of 810 mm×210 mm×10 mm to ensure that sufficient wear-resistant surface material can be surfacing-welded.

[0025] Furthermore, in step S4, the solid welding wire selected is a modified solid welding wire treated with a modifier, the diameter of the solid welding wire is 1.2 mm, and it is built-up welded in the built-up welding groove opened in step S3.

[0026] The surfacing method is tungsten inert gas shielded welding.

[0027] During post-weld heat treatment, the stepping plate after surfacing is loaded into the furnace, the furnace temperature is ensured to be 200℃ or above, and then uniformly heated to 380±10℃ at a rate of ≤200℃ / hour, kept warm for 4 hours, and then cooled to ≤100℃ at a rate of ≤50℃ / hour before being taken out of the furnace.

[0028] The step of surfacing the wear-resistant composite surface in step S4 specifically includes:

[0029] S4.1. Preheating: Use a preheating furnace to preheat the stepping plate body at a temperature of 200-250°C and keep it warm during the surfacing process;

[0030] S4.2. Preparation of base layer: high chromium stainless steel solid welding wire containing nano rare earth oxide particles is welded to the wear-resistant composite surface surfacing groove by tungsten inert gas shielded welding. To avoid welding cracks, a smaller heat input is used. The first layer of base parameters are current of 120-150A, arc voltage of 13-17V, pure argon gas, and flow rate of 12-16L / min;

[0031] S4.3. Preparation of filling layer: filling layer parameters current 130-160A, arc voltage 14-19V, gas flow 12-16L / min;

[0032] S4.4. Preparation of cover layer: To ensure the appearance quality and smooth surface for subsequent processing, the cover layer parameters are current 110-150A, arc voltage 12-17V, gas flow 12-15L / min, and a processing allowance of 3mm is required for the surfacing height. Post-weld heat treatment is then performed to eliminate welding residual stress and remove diffused hydrogen in the joint, which can also improve the structure and performance of the joint.

[0033] If the base material has a high alloy element content and a high carbon equivalent, the crack sensitivity is high and the welding difficulty is great. The welding performance of steel can be determined by the carbon equivalent. The larger the carbon equivalent, the worse the welding performance. When the carbon equivalent is less than 0.4%, the weldability is good; when it is 0.4%-0.6%, the hardening tendency of the strip gradually increases, and the weldability is poor. Preheating and other measures are required to prevent cracks during welding; if the carbon equivalent is greater than 0.6%, a higher preheating temperature (or annealing temperature) and strict process measures are required during welding. The present application is aimed at welding a substrate with a carbon equivalent greater than 0.6%. Preferably, the carbon equivalent of the substrate is greater than 2.0%.

[0034] Among them, the matrix part has different materials and different carbon equivalents, and its treatment methods are different. First of all, the heat treatment process parameters are different. The reason is that the matrix material is different, the carbon equivalent is different, and the difficulty of controlling the welding quality is different. The matrix material with high carbon equivalent has high difficulty in controlling the welding quality, high alloy element content, and high hardening tendency, which leads to decreased toughness of the weld metal and easy cracking. Generally, it is necessary to increase the preheating temperature before welding and adopt low heat input welding method and parameters for welding. The matrix material with low carbon equivalent has lower difficulty in controlling the welding quality and better welding performance.

[0035] Secondly, the surfacing method is different. The carbon equivalent of the X22CrMoV12-1 matrix is ​​high, and the welding temperature requirement is high, which is difficult to maintain in actual production. Therefore, the tungsten inert gas shielded welding process with good welding stability, strong material adaptability and high weld purity is selected for welding.

[0036] Furthermore, the welding process parameters of high-chromium stainless steel solid welding wire are different. The reason is that the base material high-temperature resistant stainless steel X22CrMoV12-1 has good high-temperature resistance, better oxidation resistance, ductility and mechanical strength at high temperatures, but its high alloy element content and high carbon equivalent make it highly sensitive to cracks. It is necessary to use tungsten inert gas shielded welding with high welding quality, stable process and low heat input. The welding shielding gas pure argon can effectively reduce the burnout of alloy elements and oxide particles in the weld, and fully guarantee the comprehensive performance of the deposited metal.

[0037] Therefore, by selecting a suitable welding method and adjusting welding parameters, the comprehensive performance of the wear-resistant surface can be effectively improved. The wear-resistant surface is formed by layering the solid welding wire on the substrate surface by surfacing welding. The lower welding layer is heated again during the surfacing process. The near-seam area is very likely to grow grains and form harmful structures such as Widmanstätten structure, resulting in the performance degradation of the second heat-affected zone (first weld).

[0038] The present invention further modifies the solid welding wire, and the modified solid welding wire comprises an iron base material and a modifier, wherein the chemical components of the iron base material are: C: 0.47%-0.55%, Si: 0.30%-0.50%, Mn: 0.50%-0.80%, Cr: 12.00%-14.00%, S≤0.03%, P≤0.03%, and the rest is Fe; the modifier is a nano rare earth oxide, wherein the nano rare earth oxide comprises CeO 2 ,La 2 O 3 The particle size of the nano rare earth oxide is 501100nm, preferably, the average particle size is 50nm. The ratio of the modifier to the iron base material is (2-3): (15-20).

[0039] The method for preparing the above solid welding wire comprises the steps of:

[0040] a. Mechanically grinding a modifier with iron powder to obtain a homogenized ceramic phase powder; the size of the modifier is 501100 nm;

[0041] b. ball-milling the ceramic phase powder obtained in step a for 8115 h to obtain a ceramic phase toughening agent;

[0042] c. Continue to add sodium water glass binder to the ceramic phase toughening agent obtained in step b, and roll it into a spherical material;

[0043] d. Finally, according to the raw material ratio of solid welding wire, raw materials of required elements are added into the smelting furnace, and the spherical material obtained in step c is added at the same time, and solid welding wire is obtained through forging, rolling and cold drawing. The ratio of the modifier to the iron base material is (2-3): (15-20).

[0044] The preparation method of the solid welding wire of the present application is applicable to multiple types of steel, such as 5Cr13 and H13.

[0045] The wear-resistant surface is made by surfacing the solid welding wire in layers on the substrate surface. The lower welding layer is continuously heated and solidified during the surfacing process. The addition of rare earth oxides can improve the crystal phase structure of the coating during secondary solidification, produce eutectic solution, and enhance the adhesion and wear resistance of the wear-resistant layer. The added rare earth oxides can serve as "anchor points" and pin in the heat-affected zone, effectively inhibiting the abnormal growth of grains, thereby ensuring the mechanical properties of the heat-affected zone (weld layer).

[0046] Moreover, the fine grain strengthening of the weld metal by the modifier is beneficial to improving the comprehensive mechanical properties of the solid welding wire and the wear-resistant surface.

[0047] Compared with adding rare earth alloys to form original inclusions for modification during smelting of raw materials, this patent adds rare earth alloy synthetic oxide modifiers to the smelted molten steel to avoid the problems of original rare earth inclusions in the molten steel having low specific gravity and easy floating, poor wettability, and easy agglomeration due to small particle size. Appropriate welding methods and process methods are then used according to product requirements to effectively improve the performance of solid welding wire and wear-resistant surface.

[0048] The solid welding wire of the present application is welded in the groove on the surface of the stepping plate. The traditional stepping plate generally adopts an integral structure, so the surface is prone to pits, edge pressure feedback, cracks, and even breakage during use. The present application adopts a composite stepping plate to form a wear-resistant layer with higher hardness on the substrate of the stepping plate, forming a "hard and flexible" composite structure. This composite structure greatly improves the wear resistance, corrosion resistance, impact resistance, and fatigue resistance of the stepping plate during use.

[0049] The invention also discloses a composite stepping plate made by the above method. The composite stepping plate comprises a substrate, a groove is provided on the substrate, and a solid welding wire is used to perform surfacing welding in the groove to form a wear-resistant layer.

[0050] In the wear-resistant surface, the martensite structure accounts for 85% to 90% and the hardness is HRC50-57;

[0051] The metallographic structure of the matrix is ​​tempered troostite;

[0052] There is a heat-affected zone of 2-4 mm between the wear-resistant surface and the substrate. The metallographic structure of the heat-affected zone is bainite, and there is no structural embrittlement caused by MA components, upper bainite, and coarse Widmanstatten structure.

[0053] The matrix is ​​selected from a material with a hardness of HB240-260 and an impact energy Akv (J) ≥ 34, such as X22CrMoV12-1. In addition, other materials that meet the comprehensive mechanical properties can also be applied to the composite stepping plate of the present application.

[0054] 3. Beneficial effects

[0055] Compared with the prior art, the present invention has the following beneficial effects:

[0056] (1) A preparation method of a composite stepping plate of the present invention aims at the problem that the base material has high alloy element content, high carbon equivalent, and high grain sensitivity, which makes welding difficult. By modifying the welding wire, selecting a suitable welding method, and adjusting the welding parameters, a wear-resistant surface that meets the comprehensive performance requirements is prepared;

[0057] (2) The solid welding wire used in the welding of the present invention adopts nano rare earth oxide as a modifier to modify the solid welding wire. The nano rare earth oxide has a low melting point and forms nuclei earlier than general ceramic oxides during solidification and crystallization. The number of heterogeneous nucleation cores is larger and the distribution is more uniform. The modifier strengthens the fine grains of the weld metal, which is beneficial to improving the comprehensive mechanical properties of the solid welding wire and the wear-resistant surface.

[0058] (3) In the solid welding wire of the present invention, the nucleation distribution of the nano rare earth oxide is more uniform during solidification and crystallization, which is conducive to forming a solid welding wire with a more uniform structure during the cold drawing process, thereby improving the drawing performance of the solid welding wire;

[0059] (4) A composite stepping plate of the present invention adopts modified solid welding wire to form a wear-resistant surface, forming a "hard and flexible" composite structure with the substrate. The composite stepping plate has both the impact resistance of the substrate material and the wear resistance of the cladding material, which solves the problems of pits, edge pressure feedback and cracks, and even breakage on the surface of traditional stepping plates, thereby improving the service life of the stepping plates. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but it should be understood that these drawings are designed only for explanation purposes and are not intended to limit the scope of the present invention. In addition, unless otherwise specified, these drawings are intended only to conceptually illustrate the structural configurations described herein and are not necessarily drawn to scale.

[0061] Figure 1 and Figure 2 It is a schematic diagram of the base part of the composite stepping plate of the present invention;

[0062] Figure 3 This is a schematic diagram of wear-resistant surface surfacing of the present invention;

[0063] Figure 4 This is a process diagram of heat treatment after welding of the composite stepping plate of the present invention. DETAILED DESCRIPTION

[0064] The following detailed description of exemplary embodiments of the present invention refers to the accompanying drawings, which form a part of the description, and in which exemplary embodiments of the present invention that can be implemented are shown as examples. Although these exemplary embodiments are described in sufficient detail to enable those skilled in the art to implement the present invention, it should be understood that other embodiments can be implemented and various changes can be made to the present invention without departing from the spirit and scope of the present invention. The following more detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but is only for the purpose of illustrating and not limiting the description of the characteristics and features of the present invention, so as to propose the best mode for performing the present invention and to enable those skilled in the art to implement the present invention. Therefore, the scope of the present invention is limited only by the appended claims.

[0065] The wear resistance of each sample in the embodiment is characterized by a wear test, and the test is a wear test on a UMT Tribolab large load reciprocating friction tester. The grinding material is Al2O3 with a diameter of 6.35 mm. 2 O 3 ball.

[0066] The wear specimen is first processed into a prefabricated specimen by wire cutting, and then the surface to be worn is polished to a mirror surface by a metallographic polishing machine. 2 O 3 The ball is in direct contact, the wear time is 30 minutes, the speed of the test machine is set to 150r / min, and the load is 50N. The test uses an analytical balance with a sensitivity of 0.00001g for weighing. After the wear process is completed, the sample is purged and weighed, and the weight loss is used to characterize the wear resistance. At the same time, the friction coefficient of each sample is compared. The test results are shown in Table 1.

[0067] The calculation formula of carbon equivalent is CE=[C+Mn / 6+(Cu+Ni) / 15+(Cr+Mo+V) / 5]×100%.

[0068] Example 1

[0069] A method for manufacturing a composite stepping plate in this embodiment uses high temperature resistant stainless steel X22CrMoV12-1 as a matrix, and the carbon equivalent of the matrix is ​​2.94. The specific steps are as follows:

[0070] Step S1, making the base part: making high temperature resistant stainless steel X22CrMoV12-1, the components and weight percentage of X22CrMoV12-1 are: C: 0.20%, Si: 0.45%, Mn: 0.78%, Cr: 11.5%, Mo: 1.06%, V: 0.31%, Ni: 0.55%, S≤0.035%, P≤0.035%, and the rest is Fe; square ingot billet or continuous casting billet is used for forging. Sufficient cutting head and sufficient processing allowance are left at both ends of the billet to avoid harmful defects in the forging. The forging is forged with a hammer of more than 8 tons, the entire cross section is forged through, and the structure of the forging is ensured to be uniform, and the forging ratio is ≥3. The forging billet is placed in the gas furnace according to the process or specification requirements to ensure uniform heating, and the insulation time shall not be less than the minimum insulation time required for each forging fire. The initial forging temperature is 1220℃-1250℃, and the final forging temperature is ≥880℃. The forgings are quickly solution treated after forging.

[0071] Step S2, heat treatment of the substrate:

[0072] Quenching: slowly heat to the quenching temperature of 1030℃ and then put into the oil pool for quenching treatment, and quench and cool to below 200℃;

[0073] Tempering: After quenching, it needs to be put back into the furnace and heated to 680℃ within 30min, and then kept warm for 10 hours, oil cooled to 200℃, and then air cooled to room temperature, so that the hardness of the treated X22CrMoV12-1 matrix reaches HB240-260, the microstructure of the X22CrMoV12-1 forging blank is coarse martensite + alloy carbide + residual austenite, and the microstructure after quenching and tempering is tempered troostite. The mechanical properties are tensile strength σb (MPa) ≥ 800, yield strength σs (MPa) ≥ 600, elongation δ5 (%) ≥ 14, and impact energy Akv (J) ≥ 34.

[0074] Step S3, making the wear-resistant composite surface of the stepping plate surfacing groove:

[0075] Mill out a groove with a size of 810mm×210mm×10mm, such as Figure 1 and Figure 2 As shown;

[0076] Step S4, surfacing welding of wear-resistant composite surfacing surface:

[0077] like Figure 3 As shown, the wear-resistant composite surface is clad by tungsten inert gas shielded welding, which specifically includes the following steps:

[0078] S4.1 Preheating: Use a preheating furnace to preheat the stepping plate body, the preheating temperature is 280℃, and keep it warm during the surfacing process;

[0079] S4.2 Overlay welding: A high chromium stainless steel solid welding wire containing nano rare earth oxide particles is overlaid into the overlay groove of the wear-resistant composite surface by tungsten inert gas shielded welding.

[0080] The solid welding wire of this embodiment includes an iron base material and a modifier, wherein the components of the iron base material are C: 0.49%, Si: 0.45%, Mn: 0.60%, Cr: 12.51%, S: 0.003%, P: 0.003%, and the rest is Fe; the modifier is a nano rare earth oxide including CeO 2 , the CeO 2 The average particle size of CeO is 50 mm. 2 The mass ratio to the iron base material is 2:15.

[0081] The method for preparing the above solid welding wire comprises the steps of:

[0082] a. Mechanically grinding the modifier and iron powder to obtain a homogenized ceramic phase powder;

[0083] b. ball-milling the ceramic phase powder obtained in step a for 9 hours to obtain a ceramic phase toughening agent;

[0084] c. Continue to add sodium water glass binder to the ceramic phase toughening agent obtained in step b, and roll it into a spherical material;

[0085] d. Finally, according to the raw material ratio of the solid welding wire, the raw materials of the required elements are added into the smelting furnace, and the spherical material obtained in step c is added at the same time, and the solid welding wire is obtained through forging, rolling and cold drawing.

[0086] By adding ceramic phase to the iron base material, the problems of small specific gravity, easy floating, poor wettability, and small particle size and easy agglomeration in the molten steel are solved. After adding it to the molten steel, it plays the role of fine grain strengthening as a heterogeneous nucleation core and plays the role of dispersion strengthening as a fine second phase, thereby improving the toughness and ductility of the material. However, in the prior art, adding SiO 2 , MgO, and CaO form a ceramic phase (CN116021191A), which has a high melting point and a small specific gravity. This results in a short diffusion time from the melting of the molten pool to the crystallization solidification during welding, making it easy to float, resulting in uneven distribution in the weld, thus affecting performance stability.

[0087] The addition of rare earth oxides in the steel smelting process has the following effects compared to the addition of general ceramic phase oxides: 1. Purify the molten steel: Rare earth elements can react with oxygen and sulfur in inclusions such as manganese sulfide, aluminum oxide and aluminosilicate in the steel to generate non-metallic compounds with high melting points. These compounds float to the slag layer, thereby reducing the content of inclusions in the steel and producing a solid welding wire with higher purity. 2. Microalloying effect. Rare earth elements can refine grains, improve the microstructure of steel, affect the phase change process of steel, change the composition and structure of phase change products, and thus improve the physical and mechanical properties of steel; 3. Improve resistance to hydrogen embrittlement and stress corrosion: Rare earth elements can effectively absorb and diffuse hydrogen atoms, reduce the hydrogen content in steel, and thus improve the hydrogen embrittlement resistance and corrosion resistance of steel. 4. Refine grains to improve the performance of steel: The addition of rare earth elements can improve the mechanical properties of steel such as strength, toughness and plasticity, while improving the wear resistance and corrosion resistance of steel. 5. Control the morphology of inclusions. Rare earth elements can control the morphology of inclusions in steel, avoiding or overcoming the anisotropy of performance caused by the extension and deformation of other types of inclusions during hot pressure processing of steel.

[0088] In order to ensure that the oxides diffuse fully during welding, the heat input has to be increased, and the melting time of the molten pool is prolonged, which will cause the heat affected zone to expand, generate thermal stress and residual stress, and cause large deformation of the weld joint. At the same time, the weld joint structure is coarse, affecting its mechanical properties and corrosion resistance. Therefore, the present application adds nano rare earth oxides. The rare earth oxides have a lower melting point than general ceramic oxides. Whether in the material smelting preparation or welding process, the time for melting and diffusion into the molten steel or molten pool is more sufficient, the distribution is more uniform, and the nucleation is earlier than that of general ceramic oxides during solidification and crystallization. The number of heterogeneous nucleation cores of rare earth oxides is larger and the distribution is more uniform, which is conducive to the formation of a fine grain strengthening mechanism, promotes the toughening of the material, and forms a more uniformly structured solid welding wire during the cold drawing process. The tensile properties of the solid welding wire are improved, so that it can be stretched into a welding wire with a diameter of 1.2 mm.

[0089] During the cladding process, the first layer's base parameters are current 130±10A, arc voltage 15±1V, and flow rate 15L / min; the filling layer's parameters are current 150±10A, arc voltage 16±2V, and gas flow rate 16L / min; the cover layer's parameters are current 130±10A, arc voltage 14±1V, and gas flow rate 15L / min. A 3mm machining allowance is required for the cladding height.

[0090] S4.3 Post-weld heat treatment: Post-weld heat treatment is used to eliminate welding residual stress, remove diffused hydrogen in the joint, and improve the structure and performance of the joint. Figure 4The heat treatment process shown is carried out, the stepping plate after surfacing is loaded into the furnace, the furnace temperature is ensured to be above 200℃, and then it is uniformly heated to 380±10℃ at a speed of ≤200℃ / hour, kept warm for 4 hours, and then cooled to ≤100℃ at a speed of ≤50℃ / hour before being taken out of the furnace.

[0091] The composition of the wear-resistant surface after surfacing is the same as that of solid welding wire.

[0092] Step S5, finishing: processing the stepping plate after surfacing welding to the finished product size by rough grinding, fine grinding, milling and clamping;

[0093] Step S6, detection:

[0094] The finished product is tested for hardness and metallographic structure.

[0095] The hardness test result is 52-56HRC, the metallographic structure of the wear-resistant surface is martensite + δ ferrite, of which the martensite structure accounts for about 85-88%, and the hardness of the area where the martensite structure accounts for 85% is HRC52, and the hardness of the area where the martensite structure accounts for 88% is HRC56; the metallographic structure of the matrix is ​​troostite + bainite, which provides a guarantee for no brittle structure after welding; the thickness of the heat-affected zone is 2mm, and the metallographic structure of the heat-affected zone is bainite. There is no structural embrittlement caused by MA components, upper bainite, and coarse Widmanstatten structure. The test results meet the technical requirements.

[0096] The friction properties of the prepared wear-resistant surface are shown in Table 1.

[0097] Example 2

[0098] A method for manufacturing a composite stepping plate in this embodiment uses high temperature resistant stainless steel X22CrMoV12-1 as a matrix, the carbon equivalent of the matrix is ​​3.21, and the specific steps are as follows:

[0099] Step S1, making the base part: making high temperature resistant stainless steel X22CrMoV12-1, the components and weight percentage of X22CrMoV12-1 are: C: 0.24%, Si: 0.48%, Mn: 0.80%, Cr: 12.5%, Mo: 1.20%, V: 0.28%, Ni: 0.68%, S≤0.035%, P≤0.035%, and the rest is Fe; square ingot billet or continuous casting billet is used for forging. Sufficient cutting heads and sufficient processing allowance are left at both ends of the billet to avoid harmful defects in the forging. The forging is forged with a hammer of more than 8 tons, the entire cross section is forged through, and the structure of the forging is ensured to be uniform, and the forging ratio is ≥3. The forging billet is placed in the gas furnace according to the process or specification requirements to ensure uniform heating, and the insulation time shall not be less than the minimum insulation time required for each forging fire. The initial forging temperature is 1220℃-1250℃, and the final forging temperature is ≥880℃. The forgings are quickly solution treated after forging.

[0100] Step S2, heat treatment of the substrate:

[0101] Quenching: slowly heat to the quenching temperature of 1030℃ and then put into the oil pool for quenching treatment, and quench and cool to below 200℃;

[0102] Tempering: After quenching, it needs to be put back into the furnace and heated to 680℃ within 30min, and then kept warm for 10 hours, oil cooled to 200℃, and then air cooled to room temperature, so that the hardness of the treated X22CrMoV12-1 matrix reaches HB240-260, the microstructure of the X22CrMoV12-1 forging blank is coarse martensite + alloy carbide + residual austenite, and the microstructure after quenching and tempering is tempered troostite. The mechanical properties are tensile strength σb (MPa) ≥ 800, yield strength σs (MPa) ≥ 600, elongation δ5 (%) ≥ 14, and impact energy Akv (J) ≥ 34.

[0103] Step S3, making the wear-resistant composite surface of the stepping plate surfacing groove:

[0104] Mill out a groove with a size of 810mm×210mm×10mm, such as Figure 1 and Figure 2 As shown;

[0105] Step S4, surfacing welding of wear-resistant composite surfacing surface:

[0106] like Figure 3 As shown, the wear-resistant composite surface is clad by tungsten inert gas shielded welding, which specifically includes the following steps:

[0107] S4.1 Preheating: Use a preheating furnace to preheat the stepping plate body, the preheating temperature is 280℃, and keep it warm during the surfacing process;

[0108] S4.2 Overlay welding: A high chromium stainless steel solid welding wire containing nano rare earth oxide particles is overlaid into the overlay groove of the wear-resistant composite surface by tungsten inert gas shielded welding.

[0109] The solid welding wire of this embodiment includes an iron base material and a modifier, wherein the components of the iron base material are C: 0.49%, Si: 0.45%, Mn: 0.60%, Cr: 12.51%, S: 0.003%, P: 0.003%, and the rest is Fe; the modifier is a nano rare earth oxide including CeO 2 , the CeO 2 The average particle size of CeO is 50 mm. 2 The mass ratio to the iron base material is 2:20.

[0110] The method for preparing the above solid welding wire comprises the steps of:

[0111] a. Mechanically grinding the modifier and iron powder to obtain a homogenized ceramic phase powder;

[0112] b. ball-milling the ceramic phase powder obtained in step a for 9 hours to obtain a ceramic phase toughening agent;

[0113] c. Continue to add sodium water glass binder to the ceramic phase toughening agent obtained in step b, and roll it into a spherical material;

[0114] d. Finally, according to the raw material ratio of the solid welding wire, the raw materials of the required elements are added into the smelting furnace, and the spherical material obtained in step c is added at the same time, and the solid welding wire is obtained through forging, rolling and cold drawing.

[0115] During the cladding process, the first layer's base parameters are current 140±10A, arc voltage 15±1V, pure argon gas with a flow rate of 15L / min; the filling layer's parameters are current 150±10A, arc voltage 17±1V, and gas flow rate 18L / min; the cover layer's parameters are current 140±10A, arc voltage 15±1V, and gas flow rate 14L / min. A 3mm machining allowance is required for the cladding height.

[0116] S4.3 Post-weld heat treatment: Post-weld heat treatment is used to eliminate welding residual stress, remove diffused hydrogen in the joint, and improve the structure and performance of the joint. Figure 4 The heat treatment process shown is carried out, the stepping plate after surfacing is loaded into the furnace, the furnace temperature is ensured to be above 200℃, and then it is uniformly heated to 380±10℃ at a speed of ≤200℃ / hour, kept warm for 4 hours, and then cooled to ≤100℃ at a speed of ≤50℃ / hour before being taken out of the furnace.

[0117] The composition of the wear-resistant surface after surfacing is the same as that of solid welding wire.

[0118] Step S5, finishing: processing the stepping plate after surfacing welding to the finished product size by rough grinding, fine grinding, milling and clamping;

[0119] Step S6, detection:

[0120] The finished product is tested for hardness and metallographic structure.

[0121] The hardness test result is 52-57HRC, the metallographic structure of the wear-resistant surface is martensite + δ ferrite, of which the martensite structure accounts for about 86-90%, and the hardness of the area where the martensite structure accounts for 86% is HRC52, and the hardness of the area where the martensite structure accounts for 90% is HRC57; the metallographic structure of the matrix is ​​troostite + bainite, which provides a guarantee for no brittle structure after welding; the thickness of the heat-affected zone is 2mm, and the metallographic structure of the heat-affected zone is bainite. There is no structural embrittlement caused by MA components, upper bainite, and coarse Widmanstatten structure. The test results meet the technical requirements.

[0122] The friction properties of the prepared wear-resistant surface are shown in Table 1.

[0123] Example 3

[0124] A method for manufacturing a composite stepping plate in this embodiment uses high temperature resistant stainless steel X22CrMoV12-1 as a matrix, the carbon equivalent of the matrix is ​​2.70, and the specific steps are as follows:

[0125] Step S1, making the base part: making high temperature resistant stainless steel X22CrMoV12-1, the components and weight percentage of X22CrMoV12-1 are: C: 0.18%, Si: 0.10%, Mn: 0.41%, Cr: 11.05%, Mo: 0.82%, Ni: 0.35%, V: 0.25%, S≤0.025%, P≤0.025%, and the rest is Fe; square ingot billet or continuous casting billet is used for forging. Sufficient cutting heads and sufficient processing allowance are left at both ends of the billet to avoid harmful defects in the forging. The forging is forged with a hammer of more than 8 tons, the entire cross section is forged through, and the structure of the forging is ensured to be uniform, and the forging ratio is ≥3. The forging billet is placed in the gas furnace according to the process or specification requirements to ensure uniform heating, and the insulation time shall not be less than the minimum insulation time required for each forging fire. The initial forging temperature is 1220℃-1250℃, and the final forging temperature is ≥880℃. The forgings are quickly solution treated after forging.

[0126] Step S2, heat treatment of the substrate:

[0127] Quenching: slowly heat to the quenching temperature of 1030℃ and then put into the oil pool for quenching treatment, and quench and cool to below 200℃;

[0128] Tempering: After quenching, it needs to be put back into the furnace and heated to 680℃ within 30min, and then kept warm for 10 hours, oil cooled to 200℃, and then air cooled to room temperature, so that the hardness of the treated X22CrMoV12-1 matrix reaches HB240-260, the microstructure of the X22CrMoV12-1 forging blank is coarse martensite + alloy carbide + residual austenite, and the microstructure after quenching and tempering is tempered troostite. The mechanical properties are tensile strength σb (MPa) ≥ 800, yield strength σs (MPa) ≥ 600, elongation δ5 (%) ≥ 14, and impact energy Akv (J) ≥ 34.

[0129] Step S3, making the wear-resistant composite surface of the stepping plate surfacing groove:

[0130] Mill out a groove with a size of 810mm×210mm×10mm, such as Figure 1 and Figure 2 As shown;

[0131] Step S4, surfacing welding of wear-resistant composite surfacing surface:

[0132] like Figure 3 As shown, the wear-resistant composite surface is clad by tungsten inert gas shielded welding, which specifically includes the following steps:

[0133] S4.1 Preheating: Use a preheating furnace to preheat the stepping plate body, the preheating temperature is 280℃, and keep it warm during the surfacing process;

[0134] S4.2 Overlay welding: A high chromium stainless steel solid welding wire containing nano rare earth oxide particles is overlaid into the overlay groove of the wear-resistant composite surface by tungsten inert gas shielded welding.

[0135] The solid welding wire of this embodiment includes an iron base material and a modifier, wherein the components of the iron base material are C: 0.49%, Si: 0.45%, Mn: 0.60%, Cr: 12.51%, S: 0.003%, P: 0.003%, and the rest is Fe; the modifier is a nano rare earth oxide including La 2 O 3 , the La 2 O 3 The average particle size is 50 mm, the La 2 O 3 The mass ratio to the iron base material is 2:20.

[0136] The method for preparing the above solid welding wire comprises the steps of:

[0137] a. Mechanically grinding the modifier and iron powder to obtain a homogenized ceramic phase powder;

[0138] b. ball-milling the ceramic phase powder obtained in step a for 9 hours to obtain a ceramic phase toughening agent;

[0139] c. Continue to add sodium water glass binder to the ceramic phase toughening agent obtained in step b, and roll it into a spherical material;

[0140] d. Finally, according to the raw material ratio of the solid welding wire, the raw materials of the required elements are added into the smelting furnace, and the spherical material obtained in step c is added at the same time, and the solid welding wire is obtained through forging, rolling and cold drawing.

[0141] During the cladding process, the parameters of the first layer base are current 135±10A, arc voltage 14±1V, pure argon gas with a flow rate of 15L / min; the parameters of the filling layer are current 140±10A, arc voltage 15.5±1V, and gas flow rate 16L / min; the parameters of the cover layer are current 125±10A, arc voltage 14±1V, and gas flow rate 13L / min. A processing allowance of 3mm is required for the cladding height.

[0142] S4.3 Post-weld heat treatment: Post-weld heat treatment is used to eliminate welding residual stress, remove diffused hydrogen in the joint, and improve the structure and performance of the joint. Figure 4 The heat treatment process shown is carried out, the stepping plate after surfacing is loaded into the furnace, the furnace temperature is ensured to be above 200℃, and then it is uniformly heated to 380310℃ at a rate of ≤200℃ / hour, kept warm for 4 hours, and then cooled to ≤100℃ at a rate of ≤50℃ / hour and taken out of the furnace.

[0143] The composition of the wear-resistant surface after surfacing is the same as that of solid welding wire.

[0144] Step S5, finishing: processing the stepping plate after surfacing welding to the finished product size by rough grinding, fine grinding, milling and clamping;

[0145] Step S6, detection:

[0146] The finished product is tested for hardness and metallographic structure.

[0147] The hardness test result is 50-55HRC, the metallographic structure of the wear-resistant surface is martensite + δ ferrite, of which the martensite structure accounts for about 85187%, and the hardness of the area where the martensite structure accounts for 85% is HRC50, and the hardness of the area where the martensite structure accounts for 87% is HRC55; the metallographic structure of the matrix is ​​troostite + bainite, which provides a guarantee for no brittle structure after welding; the thickness of the heat-affected zone is 2mm, and the metallographic structure of the heat-affected zone is bainite. There is no structural embrittlement caused by MA components, upper bainite, and coarse Widmanstatten structure. The test results meet the technical requirements.

[0148] The friction properties of the prepared wear-resistant surface are shown in Table 1.

[0149] Table 1 Abrasion weight loss data of each material in Examples 1-3

[0150] Example Hardness / HRC <![CDATA[Original weight M 0 / g]]> <![CDATA[Weight M after wear 1 / g]]> Weight loss ΔM / g Average friction coefficient 1 52-56 2083.52 2083.48 0.04 0.8525 2 52-57 2136.17 2136.09 0.08 0.8402 3 50-55 2163.90 2163.82 0.08 0.8482

[0151] The modified solid welding wire prepared in the present application is used for surfacing to form a wear-resistant surface with higher wear resistance, forming a "rigid and flexible" composite structure with the substrate. The composite stepping plate has both the impact resistance of the substrate material and the wear resistance of the surfacing material, which greatly improves the wear resistance, corrosion resistance, impact resistance and fatigue resistance of the stepping plate during use.

[0152] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope involved in the present application is not limited to the technical solution formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept, such as a technical solution formed by replacing the above-mentioned features with (but not limited to) technical features with similar functions disclosed in this application.

[0153] Except for the technical features described in the specification, the remaining technical features are known technologies to those skilled in the art. In order to highlight the innovative features of the present invention, the remaining technical features will not be described here in detail.

Claims

1. A method for manufacturing a composite stepping plate, It is characterized in that The method comprises the following steps: opening a wear-resistant surface groove on the surface of a stepping plate substrate, surfacing a solid welding wire into the wear-resistant surface groove to form a wear-resistant surface, wherein the solid welding wire comprises an iron base material and a modifier, wherein the modifier is a nano rare earth oxide, and the carbon equivalent of the substrate portion is greater than 2.0%.

2. The manufacturing method according to claim 1, It is characterized in that The ratio of the modifier to the iron base material is (2-3): (15-20).

3. The manufacturing method according to claim 2, It is characterized in that The nano rare earth oxide includes CeO 2 ,La 2 O 3 One or more of .

4. The manufacturing method according to claim 1, It is characterized in that The steps of surfacing wear-resistant composite surface specifically include: S4.

1. Preheating: The preheating temperature is 200-250℃ and should be kept warm during the surfacing process; S4.

2. Preparation of base layer: 1.2mm diameter solid welding wire containing nano rare earth oxide is welded into the wear-resistant composite surface welding groove. The first layer of base parameters is 120-150A, arc voltage is 13-17V, pure argon gas is used, and the flow rate is 12-16L / min; S4.

3. Preparation of filling layer: filling layer parameters current 130-160A, arc voltage 14-19V, gas flow 12-16L / min; S4.

4. Preparation of cover layer: The cover layer parameters are current 110-150A, arc voltage 12-17V, and gas flow rate 12-15L / min.

5. The manufacturing method according to claim 4, It is characterized in that The surfacing welding method is a tungsten inert gas shielded welding method.

6. The manufacturing method according to claim 5, It is characterized in that Includes steps: S1, making the stepping board base part; S2, heat treatment of the substrate; S3. Opening the wear-resistant surface groove of the stepping plate: the wear-resistant surface groove is processed by CNC milling; S4, cladding wear-resistant composite cladding surface: cladding the solid welding wire to the groove of the wear-resistant surface, and then perform post-weld heat treatment; S5, finishing: the stepping plate after surfacing welding is processed to the finished size by milling and grinding.

7. The manufacturing method according to claim 6, It is characterized in that The step of heat treating the substrate part in step S2 includes: Quenching: slowly heat to the quenching temperature of 1010-1040℃, then put into the oil pool for quenching treatment, and quench and cool to below 200℃; Tempering: After quenching, it needs to be put back into the furnace and heated to 670-690℃ within 20-30 minutes, and kept warm for 10-12 hours, then oil-cooled to 200℃ and then air-cooled to room temperature.

8. A composite stepping plate, made by the manufacturing method according to any one of claims 1 to 7, It is characterized in that The invention comprises a substrate, a groove is provided on the substrate, and a solid welding wire is used to perform overlay welding in the groove to form a wear-resistant layer. The carbon equivalent of the substrate part is greater than 2.0%.

9. The composite stepping board according to claim 8, It is characterized in that In the wear-resistant surface, the martensite structure accounts for 85% to 90%, and the hardness is HRC50-57.

10. The composite stepping board according to claim 9, It is characterized in that The matrix metallographic structure is tempered troostite, the matrix hardness is HB240-260, and the impact energy Akv (J) is ≥34.

11. The composite stepping board according to claim 10, It is characterized in that The components and weight percentages of the matrix are: C: 0.18%-0.24%, Si: 0.10%-0.50%, Mn: 0.40%-0.90%, Cr: 11.00%-12.50%, Mo: 0.80%-1.20%, Ni: 0.30%-0.80%, V: 0.25%-0.35%, S≤0.025%, P≤0.025%, and the rest is Fe.

12. The composite stepping board according to claim 11, It is characterized in that It also includes a heat-affected zone located between the wear-resistant surface and the substrate. The thickness of the heat-affected zone is 2-4 mm, and the metallographic structure of the heat-affected zone is bainite.

13. A solid welding wire for welding the composite stepping plate according to any one of claims 8 to 12, It is characterized in that The invention comprises an iron base material and a modifier, wherein the chemical components of the iron base material are: C: 0.47%-0.55%, Si: 0.30%-0.50%, Mn: 0.50%-0.80%, Cr: 12.00%-14.00%, S≤0.03%, P≤0.03%, and the rest is Fe; and the modifier is nano rare earth oxide.

14. The solid welding wire according to claim 13, It is characterized in that The ratio of the modifier to the iron base material is (2-3): (15-20).

15. The solid welding wire according to claim 14, It is characterized in that The nano rare earth oxide includes CeO 2 ,La 2 O 3 One or more of .

16. A method for manufacturing the solid welding wire according to any one of claims 13 to 15, It is characterized in that Includes steps: a. Mechanically grinding the modifier and iron powder to obtain a homogenized ceramic phase powder; b. ball-milling the ceramic phase powder obtained in step a for 8 to 15 hours to obtain a ceramic phase toughening agent; c. Continue to add sodium water glass binder to the ceramic phase toughening agent obtained in step b, and roll it into a spherical material; d. Finally, according to the raw material ratio of the solid welding wire, the raw materials of the required elements are added into the smelting furnace, and the spherical material obtained in step c is added at the same time, and the solid welding wire is obtained through forging, rolling and cold drawing.

Citation Information

Patent Citations

  • Flux core for nano-modified boron-containing high-chromium iron hardfacing self-protection flux-cored wire

    CN105269183A

  • Low-cost preparation method of ceramic phase modified H13 solid welding wire

    CN116021191A

  • Surfacing composite shear blade and manufacturing method thereof

    CN117817041A

  • Geopolymer foams based on ceramic materials

    US20240199483A1