Method for removing organic pollutants on surface of steel grit by heating

By heating the steel grit at a constant temperature of 180°C for 3 hours in the curing chamber, the problem of removing organic pollutants on the surface of the steel grit is solved, the recycling rate of the steel grit and the cost-effectiveness of the treatment are improved, and the cleaning quality of the coated oil pipe is ensured. stability.

CN118809457APending Publication Date: 2024-10-22KARAMAY CITY KENENG ANTI CORROSION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410901140.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing technology cannot effectively remove organic pollutants on the surface of steel grit, causing pollutants to produce new contamination in the process purge process on the workpiece surface, affecting product quality. There is also a lack of technical determination and removal methods for the content of organic pollutants on the surface of steel grit.

Method used

Heating method is used to heat up the steel grit through the curing chamber, and the temperature and time are selected to volatilize organic pollutants and clean the surface of the steel grit. The specific steps include welding the sand tray, filling the steel grit, and maintaining a constant temperature of 180°C in the curing chamber. Heating treatment for 3 hours, and recording the constant temperature time, followed by cooling and recycling.

Benefits of technology

It can effectively remove organic pollutants on the surface of steel grit, improve the recycling rate of steel grit, save the cost of steel surface treatment, and determine the technical and economic points through experiments to ensure the stability of the cleaning quality of coated oil pipes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118809457A_ABST
    Figure CN118809457A_ABST
Patent Text Reader

Abstract

The invention discloses a method for removing organic pollutants on the surface of steel grit by heating, which adopts a steel grit laboratory heat removal method to eliminate a volatilization curve for removing the organic pollutants attached to the steel grit and technically judge the content of the organic pollutants on the surface of the steel grit. Technical economic points of heat treatment of the steel grit in mass production are determined according to a volatilization curve of removal of organic pollutants of the steel grit touched in a laboratory, then the used steel grit is pulled into a curing chamber through a transfer cart of the curing chamber, and the cleaning quality of the coating oil pipe is more stable through the technical economic points determined by a heat removal method in the laboratory. The used steel grit is pulled into the curing chamber through the curing chamber transfer cart and is heated at the constant temperature of 180 DEG C for 3 hours, so that organic pollutants on the steel grit can be quickly volatilized, the effect of removing the organic pollutants attached to the surface of the steel grit is achieved, the original clean state of the steel grit is recovered, and the recycling rate of the steel grit is effectively increased; the steel surface treatment cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a metal surface treatment technology, in particular to a method for removing organic pollutants on the surface of steel sand by heating. Background Art

[0002] When the metal surface needs to be sandblasted (shot blasted) for cleaning on the production line, the abrasive used is generally steel sand (steel shot). The steel sand (steel shot) is recycled on the production line. The metal surface being treated is sometimes contaminated by organic pollutants. When using physical cleaning processes such as sandblasting (shot blasting), the principle followed is that the steel sand (steel shot) impacts and cuts the steel surface at a certain speed to achieve the process of cleaning the attachments on the steel surface. In the process of impacting and cutting the steel surface, some of the steel sand (steel shot) will be contaminated by organic matter attached to the steel surface. With recycling, the degree of contamination of the steel sand (steel shot) in the cleaning system will become more and more serious until it does not meet the standard requirements, and the steel sand (steel shot) in the system needs to be replaced and disposed of.

[0003] Existing technology

[0004] 1. In the invention patent 1 [A method for manufacturing nano anti-corrosion coating for oil pipe ZL200910113349.5] of Karamay Keneng Anti-corrosion Technology Co., Ltd. as the patentee, the sandblasting process is used for the inner wall of the oil pipe:

[0005] The inner and outer wall surfaces of the oil pipe are treated by sandblasting, so that the sandblasting grade of the inner and outer wall surfaces of the oil pipe reaches Sa2.5 or above, and the surface anchor grain reaches 10-40 microns;

[0006] 1) Treatment of the inner surface of the oil pipe:

[0007] Use the sandblasting gun with loose sand head to blast the inner wall of the oil pipe. The steel sand from the inner sandblasting gun head is directly shot onto the inner surface of the steel pipe to clean the oxide scale, paint and dirt on it. The sandblasting grade reaches Sa2.0-Sa3.0, and the anchor pattern roughness reaches 10-40 microns;

[0008] 2) Treatment of the outer wall of the oil pipe:

[0009] Use a direct-jet sandblasting gun to sandblast the outer wall of the oil pipe. The pipe rotates and sprays 360 degrees to clean the oxide scale, paint and dirt on it. The sandblasting level reaches Sa2.0-Sa3.0, and the anchor pattern roughness reaches 10-40 microns;

[0010] 3) Technical parameters:

[0011] Air pressure: 5.0-6.0kg / cm 2

[0012] Spherical steel sand particle size: 0.1-2.0mm

[0013] Granular steel sand particle size: 0.1-2.0mm

[0014] Spherical steel sand: granular steel sand = 1:1

[0015] 4) Put on sheaths on the inner and outer threads of the oil pipe to protect the threads during sandblasting to avoid damage to the threads.

[0016] The oil pipe after sandblasting is placed in a dry environment, and within 24 hours, the inner and outer walls of the oil pipe are coated with the following nano-composite coatings respectively.

[0017] 2. In the invention patent 2 [treatment method for inner and outer walls of oil pipes before anti-corrosion coating ZL201710675698.0] of Karamay Keneng Anti-corrosion Technology Co., Ltd. as the patentee, the inner wall of the oil pipe is cleaned by sandblasting, and the outer wall of the oil pipe is cleaned by shot blasting:

[0018] A. Treatment of the outer wall of the oil pipe:

[0019] Step ①, throwing balls with a diameter of 0.2-3.0mm to the outer wall of the oil pipe and then making the balls physically impact the outer wall of the oil pipe until the anchor grain of the outer wall of the oil pipe reaches 15-20μm; the intact balls thrown are recovered by the ball circulation system, and the dust generated during the shot blasting process, including the dust raised and the powder broken into powder by the balls impacting the outer wall of the oil pipe, is introduced into the flowing gas generated by the induced fan into the dust filter, so that the dust filter blocks the dust in the dust collector and makes the flowing gas flow through it and be filtered to the environmental purity by the dust filter before being discharged to the outdoor atmosphere;

[0020] Step ②, remove the primary pollutants including scale, paint, dust and oil stains attached to the outer wall of the oil pipe by moving the oil pipe in a straight line and rotating, keep the speed of the oil pipe moving in a straight line at 1.2-3.5 m / min and the speed of the oil pipe rotating at 3-8 rpm, until the surface cleanliness of the steel base exposed on the outer wall of the oil pipe reaches Sa1.5-2.5;

[0021] Step ③, use clean compressed air with a pressure of 0.6-0.9MPa to purge the outer wall of the oil pipe, so as to remove the secondary pollutants carried by the balls during the throwing process and attached to the outer wall of the oil pipe by air washing, until the surface cleanliness of the steel base exposed on the outer wall of the oil pipe reaches Sa1.5-2.5 again;

[0022] B. Treatment of the end faces of the oil pipes at both ends:

[0023] Remove pollutants including dust and oil attached to the end faces of both ends of the oil pipe;

[0024] C. Treatment of the inner wall of the oil pipe:

[0025] Step ①, use clean compressed air with a pressure of 0.6-0.9MPa to purge the inner wall of the oil pipe to remove primary pollutants such as oxide scale, paint scale, dust, and oil stains attached to the inner wall of the oil pipe by air washing;

[0026] Step ②, using a pre-prepared total gas sand guide pipe in a straight segment shape, the total gas sand guide pipe is divided into a front gas sand guide pipe located at the front section thereof and a rear gas sand guide pipe located at the rear section thereof, the front gas sand guide pipe and the rear gas sand guide pipe are dynamically sealed and cooperated with each other in a manner of rotating relative to each other around the central axis of the total gas sand guide pipe in the length direction;

[0027] Step ③, extend the total gas sand guide pipe into the horizontally stationary oil pipe, keep the pipe section of the total gas sand guide pipe extending into the oil pipe and the gun nozzle arranged at the front end of the pipe section suspended in the oil pipe without contacting the inner wall of the sandblasting pipe;

[0028] Step ④, keep the front gas sand guide pipe and the rear gas sand guide pipe that are in dynamic sealing cooperation with each other in a state of reciprocating rotation relative to each other around the central axis of the total gas sand guide pipe in the length direction, and keep the gun nozzle moving back and forth along the straight line at a rate of 0.8-1.5 m / min;

[0029] Step ⑤, the clean compressed air with a pressure of 0.65-0.90MPa pressed out by the sandblasting machine drives the sandblasting abrasive to pass through the total air sand guide pipe from the nozzle located at the front end of the front air sand guide pipe and spray it onto the inner wall of the oil pipe in a direction with an angle of 30°-60° with the horizontal line, until the anchor grain of the inner wall of the oil pipe reaches 30-40μm and the surface cleanliness of the steel base exposed on the inner wall of the oil pipe reaches Sa2.5-3.0;

[0030] Step ⑥, the blasted intact sandblasting abrasive is recovered by the sandblasting abrasive circulation system, and the dust generated during the sandblasting process, including the dust raised and the powder broken into powder by the sandblasting abrasive impacting the inner wall of the oil pipe, is introduced into the flowing gas generated by the induced fan into the dust filter, so that the dust filter blocks the dust in the dust collector and the flowing gas flows through it and is filtered to the environmentally friendly purity by the dust filter and then discharged to the outdoor atmosphere;

[0031] Step ⑦, use clean compressed air with a pressure of 0.6-0.9MPa to purge the inner wall of the oil pipe to remove secondary pollutants carried by the sandblasting abrasive during the spraying process that are secondary attached to the inner wall of the oil pipe by air washing, until the cleanliness of the inner wall of the oil pipe exposed on the steel base surface reaches Sa2.5-3.0 again.

[0032] The above-mentioned existing technologies 1 and 2 disclose the use of sandblasting (shot blasting) to treat the inner and outer wall surfaces of the oil pipe and to remove the secondary pollutants carried by the sandblasting abrasive during the spraying process that are secondary attached to the inner wall surface of the oil pipe by the circulating dust blowing method. However, the above-mentioned existing technologies cannot completely blow away the secondary pollutants on the oil pipe, and the pollutants on the surface of the steel grit cannot be completely blown away during the process blowing link of the workpiece surface. When the pollutants accumulate on the steel grit to a certain extent, new pollution will be generated on the newly treated steel surface when the sandblasting operation is performed, which will affect the quality of the intermediate product. At present, there is no technical determination of the content of organic pollutants on the surface of steel grit and a method for effectively removing the organic pollutants on the surface of steel grit in the industry. Summary of the invention

[0033] The purpose of the present invention is to provide a method for removing organic pollutants on the surface of steel grit by heating, so as to solve the problems raised in the above-mentioned background technology.

[0034] To achieve the above object, the present invention provides the following technical solutions:

[0035] A method for removing organic pollutants from the surface of steel grit by heating, the method comprising the following steps:

[0036] S1. Select 4 steel plates and weld them into four sand trays;

[0037] S2, then load the steel sand onto the four sand trays and place them in parallel on the hoisting rack in the cleaning workshop, and pull the hoisting rack into the curing room through the curing room transport vehicle for heating;

[0038] S3, when the temperature of the three zones of the curing chamber reaches 120-300°C, start constant temperature and record the constant temperature time. After 1-4 hours of constant temperature, the heating treatment ends;

[0039] S4. After the steel sand is heated in the curing room, open the door of the curing room, quickly pull out the sand tray, and close the curing door in time. After the sand tray is cooled in the workshop for 30 minutes, it is hoisted and transported back to the cleaning workshop using a wire rope. The steel sand that has been heated and transported back to the workshop is scattered on the iron sheet laid in the cleaning workshop to cool;

[0040] S5. After all the steel sands have been heated and cooled completely, they are added to the oil pipe inner wall cleaning machine. The inner and outer wall dust removal systems are turned on. After the steel sands have circulated several times and the surface is clean and dust-free, the formal cleaning operation can be carried out.

[0041] As a further solution of the present invention: the inner diameter specifications of the four sand trays in step S1 are all 1.42m×1.18m×0.15cm, the density of steel shot is 7.4g / cm3, the density of steel sand is 7.6g / cm3, each tray is (1.42m×1.18m×0.1m)=0.17m3, each tray is (0.17m3×7.6g / cm3)=1.3 tons.

[0042] As a further solution of the present invention: in step S2, the four sand trays are horizontally filled with 10 cm thick steel sand.

[0043] As a further solution of the present invention: in step S3, the boiler operator heats the curing chamber to 120-300°C one hour in advance, heats it again after the steel sand enters the curing chamber, and the heating treatment is completed after keeping the temperature constant for 1-4 hours, and the curing chamber is kept warm for the next heating.

[0044] As a further solution of the present invention: in the step S2, the steel sand should be placed neatly when entering the curing room, and the placement width should be smaller than the width of the curing room, so that the sand tray is in the center of the curing room.

[0045] As a further solution of the present invention: in step S4, the lifting can only be carried out after the temperature drops to below 40°C.

[0046] As a further solution of the present invention: a dust mask must be worn when filling the sand tray in step S2.

[0047] As a further solution of the present invention: during the operation of steps S1-S4, the operators must wear labor protection suits.

[0048] As a further solution of the present invention: in step S4, a high temperature warning sign needs to be hung next to the steel sand when it is cooled.

[0049] Compared with the prior art, the present invention has the following beneficial effects:

[0050] 1. The present invention pulls the used steel sand (steel shot) into the curing chamber through a curing chamber transport vehicle and heats it at a constant temperature of 180°C for 3 hours, so that the organic pollutants on the steel sand (steel shot) can be quickly volatilized, thereby achieving the effect of removing the organic pollutants attached to the surface of the steel sand (steel shot), effectively improving the recycling rate of the steel sand (steel shot) and saving the cost of steel surface treatment.

[0051] 2. The present invention adopts the laboratory thermal removal method of steel grit to investigate the volatilization curve of the removal of organic pollutants attached to the steel grit. The technical and economic point of the heat treatment of steel grit in large-scale production is determined based on the volatilization curve of the removal of organic pollutants from the steel grit investigated in the laboratory (through comparison of experimental data), so that the cleaning quality of the coated oil pipe is more stable.

[0052] 3. The present invention can make a technical determination on the content of organic pollutants on the surface of steel sand. When the content reaches the regeneration standard, the steel sand on the production line is discharged for regeneration treatment to restore the original clean state of the steel sand. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 This is a comparison chart of steel sand before and after heating at 120°C in Experimental Report 1 of the present invention.

[0054] Figure 2 This is a comparison chart of steel sand before and after heating at 150°C in Experimental Report 1 of the present invention.

[0055] Figure 3 This is a comparison chart of steel sand before and after heating at 180°C in Experimental Report 1 of the present invention.

[0056] Figure 4 This is a comparison chart of steel sand before and after heating at 210°C in Experimental Report 1 of the present invention.

[0057] Figure 5 This is a comparison chart of steel sand before and after heating at 240°C in Experimental Report 1 of the present invention.

[0058] Figure 6 This is a comparison chart of steel sand before and after heating at 270°C in Experimental Report 1 of the present invention.

[0059] Figure 7 This is a curve chart of the experimental results of the steel sand thermal removal method in the experimental report 1 of the present invention.

[0060] Figure 8 This is a comparison chart of the steel sand before and after heating at 150°C in Experimental Report 2 of the present invention.

[0061] Fig. 9 This is a comparison chart of the steel sand before and after heating at 160°C in Experimental Report 2 of the present invention.

[0062] Fig.10 This is a comparison chart of the steel sand before and after heating at 170°C in Experimental Report 2 of the present invention.

[0063] Fig.11 This is a comparison chart of the steel sand before and after heating at 180°C in Experimental Report 2 of the present invention.

[0064] Fig.12 This is a curve chart of the experimental results of the steel sand thermal removal method in Experimental Report 2 of the present invention. DETAILED DESCRIPTION

[0065] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0066] The present invention adopts a laboratory heat treatment method for steel sand, samples steel sand with a full production use cycle of 2 months for laboratory heating treatment, uses an analytical balance to detect the volatile organic matter in the steel sand, and determines the heating time and heating temperature of the large-scale production steel sand based on the statistical results of the laboratory heating experiment.

[0067] Experimental report of the present invention

[0068] 1. Experimental purpose:

[0069] 1.0 The laboratory investigated the volatilization curve of organic pollutants attached to steel grit used in production by heating and removing them.

[0070] 2.0 The technical and economic point of heat treatment of steel grit in large-scale production is determined based on the volatilization curve of organic pollutants removed from steel grit obtained in the laboratory.

[0071] 3.0 Formulate relevant operating procedures for large-scale production of steel grit processing to make the cleaning quality of coated oil pipes more stable.

[0072] 2. Experimental methods:

[0073] Thermal removal method: A method of removing organic pollutants from steel grit using different temperature ranges and time periods under closed heating conditions.

[0074] 3. Experimental process and phenomena:

[0075] 1.0 Experimental Preparation

[0076] 1.1 Instruments and materials used: analytical balance, electric blast constant temperature drying oven, drying dish, desiccant, 50ml beaker, beaker tongs, tweezers, medicine spoon and other instruments.

[0077] 1.2 Sampling: Take 3000 grams of unprocessed steel sand samples that have been used in the workshop for 2 months and keep them for use in the experiment.

[0078] 1.3 During the experiment, it is strictly forbidden to touch the beaker and samples with your body to avoid affecting the experimental results.

[0079] 2.0 Laboratory heat removal experiment

[0080] 2.1 Use a clean 50ml beaker to take a 50g sample, for a total of 7 groups, take 7 cups of sample in each group, place an appropriate amount of desiccant on the bottom of the drying dish, put the sample steel sand into the drying dish, use vaseline to thinly coat the drying dish, seal it and leave it for more than 6 hours.

[0081] 2.2 Take out the steel sand sample which has been placed in the drying dish for more than 6 hours and place it in an electric heated air blast constant temperature drying oven.

[0082] 2.3 Start timing when the temperature of the steel sand in the electric blast constant temperature drying box reaches the set temperature. Take a sample at 60min, 90min, 120min, 150min, 180min, 210min and 240min respectively, weigh it, and record the weight loss ratio.

[0083] 2.4 Same as the above method, the steel sand samples were heated and weighed at six temperature ranges of 120℃, 150℃, 180℃, 210℃, 240℃ and 270℃ respectively.

[0084] 2.5 Use an analytical balance to weigh and record the amount of steel grit volatilization (mg), and record it as the weight loss ratio. (See the table below for details) 2.5.1.120℃ experiment

[0085]

[0086] 2.5.2 150℃ Experiment

[0087]

[0088] 2.5.3 180℃ experiment

[0089]

[0090]

[0091] 2.5.4 210℃ Experiment

[0092]

[0093] 2.5.5 240℃ experiment

[0094]

[0095] 2.5.6 270℃ Experiment

[0096]

[0097]

[0098] 4. Experimental results statistics:

[0099] Experimental results statistics table

[0100]

[0101] 5. Experimental conclusion:

[0102] 1. During the experiment, the color of the steel sand did not change at 210℃ to 270℃. The color of the steel sand at 210℃ was dark red, the color of the steel sand at 240℃ was azure blue, and the color of the steel sand turned into cyan at 270℃. The steel sand produced two temperings to different degrees. Checking the analysis report of the steel sand, the carbon content of the steel sand was 0.95%, which belongs to the range of high carbon steel (carbon content greater than 0.60%). The low-temperature tempering temperature is between 200℃-400℃. Low-temperature tempering will increase the toughness and plasticity of the steel sand, but reduce the hardness of the steel sand, which is not conducive to cleaning operations.

[0103] 2. During the experiment, the organic matter removal effect was best at a constant temperature of 180°C for 3 hours, reaching a peak of 0.111%.

[0104] 3. After discussion by the experimental team, it was determined that the boiler currently used in large-scale production needs to make the curing chamber temperature reach 180°C. The boiler needs to be heated to above 210°C to effectively remove organic pollutants attached to steel sand.

[0105] Experimental report 2 of the present invention

[0106] 1. Experimental purpose:

[0107] 1.0 Based on the first experiment, the laboratory refined the temperature range to investigate the volatilization curve of organic pollutants attached to steel sand at 150℃-180℃.

[0108] 2.0 Compound and determine the technical and economic points of heat treatment of steel sand in large-scale production.

[0109] 2. Experimental methods:

[0110] Thermal removal method: A method of removing organic pollutants from steel grit using different temperature ranges and time periods under closed heating conditions.

[0111] 3. Experimental process and phenomena:

[0112] 1.0 Experimental Preparation

[0113] 1.1 Instruments and materials used: analytical balance, electric blast constant temperature drying oven, drying dish, desiccant, 50ml beaker, beaker tongs, tweezers, medicine spoon and other instruments.

[0114] 1.2 Sampling: Take 1000 grams of unprocessed steel sand sample that has been used in the workshop for 2 months at a time.

[0115] 1.3 During the experiment, it is strictly forbidden to touch the beaker and samples with your body to avoid affecting the experimental results.

[0116] 2.0 Laboratory heat removal experiment

[0117] 2.1 Use a clean 50ml beaker to take about 50 grams of steel sand sample, a total of 4 groups, 4 cups of sample in each group, put an appropriate amount of desiccant on the bottom of the drying dish, put the sample steel sand into the drying dish, use vaseline to thinly coat the drying dish, cover it and leave it for more than 6 hours.

[0118] 2.2 Take out the steel sand sample which has been placed in the drying dish for more than 6 hours and place it in an electric heated air blast constant temperature drying oven.

[0119] 2.3 Start timing when the temperature of the steel sand in the electric blast constant temperature drying box reaches the set temperature. Take a sample at 60min, 120min, 180min and 240min respectively, weigh it, and record the weight loss ratio.

[0120] 2.4 The method is the same as above. The steel sand samples are heated and weighed at four temperature ranges of 150°C, 160°C, 170°C and 180°C. During the heating process, it is found that although the marked temperature of the electric blast drying oven is 300°C, the actual oven can reach a maximum of 274°C, so the 300°C temperature range is cancelled.

[0121] 2.5 Use an analytical balance to weigh and record the amount of steel grit volatilization (mg), and record it as the weight loss ratio. (See the table below for details)

[0122] 2.5.1.150℃ Experiment

[0123]

[0124]

[0125] 2.5.2 160℃ experiment

[0126]

[0127] 2.5.3 170℃ Experiment

[0128]

[0129] 2.5.4 180℃ Experiment

[0130]

[0131]

[0132] 4. Experimental results statistics:

[0133] 1.0 Statistical table of steel sand heating test results

[0134]

[0135] 5. Experimental conclusion:

[0136] 1. During the experiment, the organic matter removal effect was the best at 170℃ constant temperature for 4 hours, which was basically the same as the organic matter removal effect at 180℃ constant temperature for 3 hours. The organic matter removal effect at 150℃ and 160℃ was second.

[0137] 2. Judging from the appearance of the steel grit, there is no tempering phenomenon.

[0138] 3. Considering the heating temperature and heating time, it is more economical and appropriate to heat to 180℃ and keep it at a constant temperature for 3 hours.

[0139] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for removing organic pollutants from the surface of steel grit by heating. Features: The method comprises the following steps: S1. Select 4 steel plates and weld them into four sand trays; S2, then load the steel sand onto the four sand trays and place them in parallel on the hoisting rack in the cleaning workshop, and pull the hoisting rack into the curing room through the curing room transport vehicle for heating; S3, when the temperature of the three zones of the curing chamber reaches 120-300°C, start constant temperature and record the constant temperature time. After 1-4 hours of constant temperature, the heating treatment ends; S4. After the steel sand is heated in the curing room, open the door of the curing room, quickly pull out the sand tray, and close the curing door in time. After the sand tray is cooled in the workshop for 30 minutes, it is hoisted and transported back to the cleaning workshop using a wire rope. The steel sand that has been heated and transported back to the workshop is scattered on the iron sheet laid in the cleaning workshop to cool; S5. After all the steel sands have been heated and cooled completely, they are added to the oil pipe inner wall cleaning machine. The inner and outer wall dust removal systems are turned on. After the steel sands have circulated several times and the surface is clean and dust-free, the formal cleaning operation can be carried out.

2. The method for removing organic pollutants from the surface of steel grit by heating according to claim 1, Features: In step S1, the inner diameter specifications of the four sand trays are all 1.42m×1.18m×0.15cm.

3. The method for removing organic pollutants from the surface of steel grit by heating according to claim 1, Features: In step S2, four sand trays are horizontally loaded with 10 cm thick steel sand.

4. The method for removing organic pollutants from the surface of steel grit by heating according to claim 1, Features: In step S3, the boiler operator raises the temperature of the curing chamber to 120-300° C. 1 hour in advance, and raises the temperature again after the steel sand enters the curing chamber. After the temperature is kept constant for 1-4 hours, the heating process is completed, and the curing chamber is kept warm to prepare for the next heating.

5. The method for removing organic pollutants from the surface of steel grit by heating according to claim 1, Features: In step S2, the steel sand should be placed neatly when entering the curing room, and the placement width should be smaller than the width of the curing room, so that the sand tray is in the center of the curing room.

6. The method for removing organic pollutants from the surface of steel grit by heating according to claim 1, Features: In step S4, the lifting can only be carried out after the temperature drops below 40°C.

7. The method for removing organic pollutants from the surface of steel grit by heating according to claim 1, Features: A dust mask must be worn when filling the sand tray in step S2.

8. The method for removing organic pollutants from the surface of steel grit by heating according to claim 1, Features: During the operation of steps S1-S4, the operator must wear a labor protection suit.

9. The method for removing organic pollutants from the surface of steel grit by heating according to claim 1, Features: In step S4, a high temperature warning sign needs to be hung next to the steel sand when the steel sand is cooled.