Transparent wood production equipment and production process thereof
By using gas-liquid filling tubes and centrifugal force in transparent wood production equipment to simplify the wood processing process, it solves the problems of complex and long preparation processes in the existing technology, achieves efficient and continuous transparent wood production, and improves the permeability of the material. Light rate and tensile strength, suitable for industrial applications.
Patent Information
- Application Number
- CN202410314225.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-22
AI Technical Summary
The preparation process of transparent wood in the prior art is complex, time-consuming, and not suitable for industrial production. It is difficult to quickly and continuously prepare wood composite materials with high haze and high light transmittance.
A transparent wood production equipment including a storage barrel, a motor, a rotating shaft and a material room is used to perform multi-step processing through a gas-liquid filling tube, including drying, bleaching, cleaning and resin impregnation. The centrifugal force is used to push the gas and liquid through the gaps in the wood for physical and chemical processes. reaction, simplifying the lignin removal and resin penetration process.
It achieves efficient and continuous production of transparent wood, reduces production costs and time, improves the light transmittance and tensile strength of the material, and is suitable for industrial applications.
Smart Images

Figure CN118809753A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical production, in particular to transparent wood production equipment and a production process thereof. Background Art
[0002] With the introduction of the national "dual carbon" strategy, people's demands for green, low-carbon and environmentally friendly materials are constantly escalating. Transparent wood is a new type of wood composite material that has emerged in recent years. This material has expanded the boundaries of people's understanding of wood. In 2016, Chinese media reported on transparent wood prepared by Lars Berglund's team, a researcher at the Royal Institute of Technology in Sweden, and Liangbing Hu's team at the University of Maryland. Studies have shown that this new type of transparent wood has a strength 4 to 6 times greater than that of untreated wood. Compared with glass, it has better strength, higher insulation, and more light can enter. Compared with plastic materials, it is easier to degrade. In particular, transparent wood fiber materials can be used in transparent electronic components and even flexible electronic components; and adding other materials such as fluorescence, magnetism, and conductivity can be applied to more fields. In short, transparent wood has the characteristics of high light transmittance, adjustable haze, good thermal insulation, natural renewable raw materials, and carbon fixation. It has received widespread attention in the fields of solar cells, building energy-saving windows, optoelectronic devices, smart wearable devices, etc., and has gradually become a hot spot in the fields of wood science and materials science.
[0003] However, the current preparation technology still has certain limitations. The conventional laboratory preparation method is as follows: Use hypochlorite oxidation method to delignify poplar flakes. First, bake the poplar flakes required for the test to an absolutely dry state, immerse the dried poplar wood in a mixed solution of 5% NaClO2 solution and 65% CH3COOH by mass fraction, and heat at 85°C for 5 hours until the poplar wood chips are white. Take out the treated poplar wood and wash it several times to remove the residual chemicals and store it in anhydrous ethanol to replace the moisture in the cellulose skeleton. Place the prepared delignified poplar wood in a photosensitive resin solution and vacuum impregnate it for 30 minutes. When the poplar wood flakes become transparent, take out the poplar wood; place it under a UV lamp (3kw) for curing for 3 minutes to obtain transparent wood. (Gan Jian, et al.: Preparation and properties of fluorescent transparent wood based on carbon quantum dots, Journal of Forestry Engineering, 2022, 7(4): 31-37) Or another process: After preparing a bleaching solution with H2O2, NaOH and Na2SiO3 in a certain proportion, soak a 1m long birch veneer in the above solution. Heat the solution to 90°C and keep it for 1 hour. After the color of the birch veneer turns completely white, take it out and wash the bleached veneer with deionized water several times until the washing solution becomes neutral. Place the bleached veneer at room temperature for 12 hours and wait for the water to evaporate freely until the moisture content is about 100%. The decolorized wood veneer with a moisture content of about 100% was soaked in acetone for 2 hours to replace the water in the cell pore structure. Then the decolorized wood veneer containing acetone was laid flat on the surface of the epoxy resin and curing agent mixture. As the acetone slowly evaporated, the epoxy resin mixture gradually penetrated into the decolorized wood veneer. After about 2 hours, it was taken out and a transparent wood veneer with a length of 1m was obtained after curing. (Tang Qiheng, Zou Miao, Zhang Lei, et al. Preparation and properties of meter-level transparent wood veneer [J]. Wood Science and Technology, 2023, 37(05): 47-52.) In this study, after cleaning, solvent replacement was used instead of drying, which can effectively inhibit the collapse of the skeleton and facilitate the subsequent resin penetration.
[0004] It can be seen that the preparation of transparent wood includes log cutting, drying, bleaching, cleaning, re-drying, dipping and curing, etc. Each process requires different sites, different equipment and takes a long time. How to quickly and continuously prepare a new type of transparent wood composite material with a certain thickness, high dimensional stability, high haze and high light transmittance is a very worthy research topic for the industrial production of transparent wood. Summary of the invention
[0005] The object of the present invention is to provide a transparent wood production device and a production process thereof to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: a transparent wood production device and a production process thereof, comprising a storage barrel, a motor, a rotating shaft and a material room, wherein the rotating shaft is a hollow structure, a hole is provided on the rotating shaft, and a gas-liquid filler adding port is provided at the top of the rotating shaft.
[0007] Preferably, a transparent wood production device and a production process thereof include a storage barrel, a motor, a rotating shaft and a material room, wherein the rotating shaft is a hollow structure, a hole is provided on the rotating shaft, and a gas-liquid filler adding port is provided at the top of the rotating shaft.
[0008] Preferably, the material rooms are radially symmetrically distributed around the rotating shaft, the material rooms are connected to the channels of the side walls of the rotating shaft, and at least one of the upper side surface and the left, right and top outer side surfaces of the material room are made of transparent material.
[0009] Preferably, the lower end of the rotating shaft is connected to the transmission shaft of the motor and is separated from the hollow part.
[0010] Preferably, the gas-liquid filler addition port is connected to a gas-liquid filler pipe through a bearing, and the gas-liquid filler pipe is connected to an external device for supplying gas or liquid.
[0011] Preferably, the interior of the storage barrel accommodates the rotating shaft and the material space, the top or side wall of the storage barrel is partially or entirely made of a transparent material, and a liquid discharge and exhaust port is provided at the lower end.
[0012] Preferably, the liquid discharge and exhaust holes are connected to a vacuum suction device.
[0013] Preferably, the material room is barrel-shaped and surrounds the rotating shaft, the outer wall of the material room corresponding to the rotating shaft is covered with sieve holes, a switch plate is provided on the top of the material room, a card ball is fixedly connected to the bottom of the switch plate, a card slot is opened on the top of the material room, and a card seat that is engaged with the card ball is fixedly connected inside the card slot.
[0014] A process for producing transparent wood using a transparent wood production device comprises the following steps:
[0015] S1 Take poplar or other wood and peel it, then cut it to a thickness of 0.5-3CM, keeping the direction of the wood fiber vascular bundle at a nearly 90-degree angle to the axis;
[0016] S2 is put into the material room, and after it is closely contacted and placed symmetrically, air with a temperature of 10-400 degrees Celsius is introduced into the gas-liquid filling pipe, and motor 2 is started to maintain a speed of 500-1500 rpm to dry the wet wood;
[0017] S3 After drying is completed, the gas-liquid filling pipe is fed with a bleaching solution, preferably 1-10% sodium hydroxide, 2-20% sodium hypochlorite, 5-30% hydrogen peroxide, or a mixture of other materials, etc., and the speed is adjusted to 100-500 rpm, and the waste liquid collected at the discharge and exhaust port is filtered through a 2000-3000 mesh screen and then re-enters the gas-liquid filling pipe for 30-90 minutes or until the material in the material room turns white;
[0018] Change the S4 gas-liquid filling pipe to water, adjust the speed to 100-1500 rpm, maintain for 3-10 minutes, and then clean it;
[0019] S5 then inputs air at a temperature of 10-200 degrees Celsius, adjusts the speed to 500-2000 rpm, and maintains it for 5-20 minutes to dry it;
[0020] S6 gas-liquid filling pipe inputs transparent resin or its precursor material such as epoxy resin, methyl methacrylate PMMA, polystyrene, etc., adjusts the speed to 500-3000 rpm, and filters the waste liquid collected at the discharge and exhaust port through a 2000-3000 mesh screen, centrifuges and vibrates to defoam, and then re-enters the gas-liquid filling pipe for 5-10 minutes, until all the liquid enters the gaps in the wood and the air is driven away, then the process ends;
[0021] S7 material is transferred to the reaction plate frame for curing.
[0022] The implementation principle of the present invention is: after the wood is cut, the wood is placed in a storage barrel, and the wood fiber is placed at an angle of nearly 90 degrees to the rotating shaft, so that the gas and liquid can smoothly pass through the natural gaps of the wood under the centrifugal force to carry out various physical and chemical reactions. After the wood is peeled, its wood fiber and vascular bundle are well preserved, and its longitudinal tensile strength is high; while the wood grain obtained by cutting in other directions is good, and the direction of high tensile strength varies with the cutting direction. As long as the direction of the wood fiber vascular bundle is kept at a 90-degree angle to the rotating shaft, under the centrifugal force, the air passes through the fiber gaps and channels and can take away water molecules relatively quickly; similarly, the floating solution can also dissolve lignin well through the gaps and push it out, and clean water can also wash the solvent residue well; after drying again, the transparent resin liquid completely penetrates the wood gaps under the centrifugal force and can be used for direct polymerization. Under experimental conditions, it avoids the natural immersion to remove lignin, which takes too long, the effect is not thorough, and it is not easy to clean; better, it avoids the process of using an expensive vacuum degassing machine to remove bubbles when the resin is soaked. It only takes 1 / 5 of the original time and can be produced continuously.
[0023] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0024] The whole device of the present invention takes the centrifuge as the core, has high structural integrity, is easy to operate, has high efficiency, occupies a small area, and has continuous industrial production capacity. When processing wood, various materials required are easy to obtain and highly interchangeable, thereby greatly reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the overall structure of the present invention;
[0026] Figure 2 It is a cutaway schematic diagram of the present invention;
[0027] Figure 3 It is a schematic cross-sectional view of the rotating shaft of the present invention;
[0028] Figure 4 It is a partial cross-sectional schematic diagram of the material space of the present invention;
[0029] Figure 5 Schematic diagram comparing bleached poplar and transparent poplar.
[0030] Among them: 1. Storage bucket; 2. Motor; 3. Rotating shaft; 31; 4. Material room; 41. Sieve hole; 5. Gas-liquid filler adding port; 6. Switch plate; 61. Card ball; 62. Card slot; 63. Card seat; 7. Liquid discharge and exhaust port. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] The present invention provides the following technical solutions:
[0033] Embodiment 1
[0034] See also Figure 1 , Figure 2 , Figure 3 and Figure 4A transparent wood production device and a production process thereof, comprising a storage barrel 1, a motor 2, a rotating shaft 3 and a material room 4, the rotating shaft 3 is a hollow structure, a hole 31 is provided on the rotating shaft 3, a gas-liquid filler adding port 5 is provided at the top of the rotating shaft 3, the material room 4 is radially symmetrically distributed around the rotating shaft 3, the material room 4 is connected with the hole 31 on the side wall of the rotating shaft 3, the upper side surface of the material room 4 and at least one side of the left, right and top outer side surfaces are made of transparent material, the lower end of the rotating shaft 3 is connected to the transmission shaft of the motor 2 and is separated from the hollow part, and the gas-liquid filler adding port 5 is connected to the gas-liquid filler through a bearing. The pipes are connected, the gas-liquid filling pipe is connected to the external gas or liquid supply equipment, the interior of the storage barrel 1 accommodates the rotating shaft 3 and the material room 4, the top or side wall of the storage barrel 1 is partially or entirely made of transparent material, and the lower end is provided with a discharge and exhaust port 7, the material room 4 is barrel-shaped and surrounds the rotating shaft 3, the outer wall of the material room 4 corresponding to the rotating shaft 3 is covered with sieve holes 41, the top of the material room 4 is provided with a switch plate 6, the bottom of the switch plate 6 is fixedly connected to a card ball 61, the top of the material room 4 is provided with a card slot 62, the inside of the card slot 62 is fixedly connected to a card seat 63 that is engaged with the card ball 61.
[0035] When in use, after peeling poplar (or other wood), peeling is performed, the thickness is 0.5-3CM, and the cylindrical shape is formed, and the direction of the wood fiber vascular bundle is kept at a 90 degree angle with the rotating shaft; put into the material room 4, after close contact and symmetrical placement, the air-liquid filling pipe is passed into the air at a temperature of 10-400 degrees Celsius, the motor 2 is started, and the speed is maintained at 500-1500 rpm to dry the wet wood. After drying, the air-liquid filling pipe inputs a bleaching solution, preferably sodium hydroxide (1-10%), sodium hypochlorite (2-20%), hydrogen peroxide (5-30%), or a mixed solution composed of other materials, etc., and the speed is adjusted to 100-500 rpm, and the waste liquid collected by the discharge and exhaust port 7 is filtered through a 2000-3000 mesh screen, and then re-enters the air-liquid filling pipe, and is maintained for 30-90 minutes or until the material in the material room turns white. Then, the gas-liquid filling pipe is changed to input clean water, and the speed is adjusted to 100-1500 rpm, and maintained for 3-10 minutes. That is, it is cleaned. Then the air with a temperature of 10-200 degrees Celsius is input, and the speed is adjusted to 500-2000 rpm, and maintained for 5-20 minutes. It is dried. The gas-liquid filling pipe inputs transparent resin or its precursor material (epoxy resin, methyl methacrylate PMMA, polystyrene, etc.), and the speed is adjusted to 500-3000 rpm, and the waste liquid collected by the liquid discharge and exhaust port 7 is filtered through a 2000-3000 mesh screen, centrifugal vibration defoaming, and then re-enters the gas-liquid filling pipe and maintained for 5-10 minutes. When all the liquid enters the gap of the wood and the air is driven away, it ends, and the liquid discharge and exhaust port 7 is connected to a vacuum suction device, and the gas-liquid filling pipe can be respectively switched to connect a hot air generating device, a resin liquid stirring and mixing device, a clean water device, a bleaching liquid device, etc.
[0036] Example 2
[0037] When in use, after peeling poplar (or other wood), longitudinal cutting, cross cutting or beveling cutting are performed, with a thickness of 0.5-5CM, and the wood fiber vascular bundle direction is kept at a nearly 90 degree angle with the rotating shaft around the central rotating shaft (the closer the better, adjusted according to the situation); put it into the material room 4, and after close contact and symmetrical placement, the gas-liquid filling pipe is fed with air at a temperature of 10-400 degrees Celsius, and the motor 2 is started to maintain a rotation speed of 500-1500 rpm to dry the wet wood. After drying, the gas-liquid filling pipe inputs a bleaching solution, preferably sodium hydroxide (1-10%), sodium hypochlorite (2-20%), hydrogen peroxide (5-30%), or a mixed solution composed of other materials, etc., and the rotation speed is adjusted to 100-500 rpm, and the waste liquid collected by the discharge and exhaust port 7 is filtered through a 2000-3000 mesh screen, and then re-enters the gas-liquid filling pipe, and is maintained for 30-90 minutes or until the material in the material room turns white. Then, the gas-liquid filling pipe is changed to input clean water, and the speed is adjusted to 100-1500 rpm, and maintained for 3-10 minutes. That is, it is cleaned. Then the air with a temperature of 10-200 degrees Celsius is input, and the speed is adjusted to 500-2000 rpm, and maintained for 5-20 minutes. It is dried. The gas-liquid filling pipe inputs transparent resin or its precursor material (epoxy resin, methyl methacrylate PMMA, polystyrene, etc.), and the speed is adjusted to 500-3000 rpm, and the waste liquid collected by the liquid discharge and exhaust port 7 is filtered through a 2000-3000 mesh screen, centrifugal vibration defoaming, and then re-enters the gas-liquid filling pipe and maintained for 5-10 minutes. When all the liquid enters the gap of the wood and the air is driven away, it ends, and the liquid discharge and exhaust port 7 is connected to a vacuum suction device, and the gas-liquid filling pipe can be respectively switched to connect a hot air generating device, a resin liquid stirring and mixing device, a clean water device, a bleaching liquid device, etc.
[0038] Experiment 1 observed the light transmittance of peeled poplar wood, produced using equipment modified from a small centrifuge.
[0039] from Figure 5 It can be seen that the poplar veneer is opaque after bleaching, and the pattern on the bottom of the veneer cannot be seen; while the pattern on the bottom of the transparent wood veneer is clearly visible, indicating that the transparent wood veneer has good light transmittance.
[0040] Experiment 2 observed the optical transmittance of the two and found that in the visible light range of 400-780nm, the transmittance of bleached wood was lower, with an average transmittance of about 46%, while the average transmittance of transparent wood was 83% and the average haze was 72%.
[0041] Experiment 3 observed the longitudinal / transverse tensile strength of bleached poplar and transparent wood. The results showed that the tensile strength of transparent wood was improved compared with bleached poplar, with the longitudinal and transverse tensile strengths increasing by 1.56 and 3.34 times, respectively.
[0042] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and alterations may be made to the embodiments without departing from the principles and spirit thereof, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A transparent wood production device and a production process thereof, comprising a storage barrel (1), a motor (2), a rotating shaft (3) and a material room (4), Features: The rotating shaft (3) is a hollow structure, a hole (31) is provided on the rotating shaft (3), and a gas-liquid filler adding port (5) is provided at the top end of the rotating shaft (3).
2. A transparent wood production device and production process according to claim 1, Features: The material rooms (4) are radially symmetrically distributed around the rotating shaft (3); the material rooms (4) are connected to the channels (31) on the side walls of the rotating shaft (3); and the upper side surface and at least one of the left, right and top outer side surfaces of the material room (4) are made of transparent material.
3. A transparent wood production device and production process according to claim 1, Features: The lower end of the rotating shaft (3) is connected to the transmission shaft of the motor (2) and is separated from the hollow part.
4. A transparent wood production device and production process according to claim 1, Features: The gas-liquid filler adding port (5) is connected to a gas-liquid filler pipe via a bearing, and the gas-liquid filler pipe is connected to an external device for supplying gas or liquid.
5. A transparent wood production device and production process according to claim 1, Features: The interior of the storage barrel (1) accommodates the rotating shaft (3) and the material room (4); the top or side wall of the storage barrel (1) is partially or entirely made of a transparent material, and a liquid discharge and exhaust port (7) is provided at the lower end.
6. A transparent wood production device and production process according to claim 1, Features: The material room (4) is barrel-shaped and surrounds the rotating shaft (3); the outer wall of the material room (4) corresponding to the rotating shaft (3) is covered with sieve holes (41); a switch plate (6) is provided on the top of the material room (4); a clamping ball (61) is fixedly connected to the bottom of the switch plate (6); a clamping groove (62) is provided on the top of the material room (4); a clamping seat (63) clamped to the clamping ball (61) is fixedly connected inside the clamping groove (62).
7. A process for producing transparent wood using the transparent wood production device of claim 1, It is characterized in that The following steps are involved: S1 Take poplar (or other wood) and peel it, then cut it to a thickness of 0.5-3CM, keeping the direction of the wood fiber vascular bundle at a nearly 90-degree angle to the axis; S2 is placed in the material room, in close contact and symmetrically, and air at a temperature of 10-400 degrees Celsius is introduced into the gas-liquid filling pipe, and the motor (2) is started and maintained at a speed of 500-1500 rpm to dry the wet wood; S3 After drying is completed, a bleaching solution is input into the gas-liquid filling pipe, preferably sodium hydroxide (1-10%), sodium hypochlorite (2-20%), hydrogen peroxide (5-30%), or a mixture of other materials, and the speed is adjusted to 100-500 rpm. The waste liquid collected by the liquid discharge and exhaust port (7) is filtered through a 2000-3000 mesh screen and then re-enters the gas-liquid filling pipe for 30-90 minutes or until the material in the material room turns white. Change the S4 gas-liquid filling pipe to water, adjust the speed to 100-1500 rpm, maintain for 3-10 minutes, and then clean it; S5 then inputs air at a temperature of 10-200 degrees Celsius, adjusts the speed to 500-2000 rpm, and maintains it for 5-20 minutes to dry it; S6 is a gas-liquid filling pipe that inputs a transparent resin or its precursor material (epoxy resin, methyl methacrylate PMMA, polystyrene, etc.), and the speed is adjusted to 500-3000 rpm. The waste liquid collected by the liquid discharge and exhaust port (7) is filtered through a 2000-3000 mesh screen, centrifuged and vibrated to defoam, and then re-enters the gas-liquid filling pipe for 5-10 minutes. When all the liquid enters the gaps in the wood and all the air is driven away, the process ends. S7 material is transferred to the reaction plate frame for curing.
Citation Information
Patent Citations
Manufacturing method for high-flexibility high-elasticity and high-transparency wood film
CN108312281A
Method of production of modified wood
SU1123229A1
Impregnation of articles by centrifugal means