Lightweight modified asphalt waterproof coiled material
By using materials such as polyester cloth, polypropylene film, hard asphalt and ultra-fine fly ash in asphalt waterproofing membranes, combined with polymer additives to form a multi-layer structure, the problems of heavy weight and poor performance of existing asphalt waterproofing membranes are solved. problem, achieving lightweight, high-strength, heat-resistant, and corrosion-resistant waterproofing effects.
Patent Information
- Application Number
- CN202411145272.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-10-22
AI Technical Summary
Existing asphalt waterproofing membranes are heavy in weight, have low tensile strength, low tear resistance, poor heat resistance, poor low-temperature flexibility, are not corrosion-resistant, and are prone to aging, making it difficult to meet the waterproofing needs of building roofs and underground structures.
Using lightweight modified asphalt waterproofing membrane, polyester cloth, polypropylene film, polyethylene film, hard asphalt, ultra-fine fly ash, styrene-butadiene rubber, graphene and other materials are used, combined with polymer additives to form multiple layers structure, improving flexibility and weather resistance, and replacing heavy calcium with fly ash to reduce weight.
It achieves lightweight, high-strength, heat-resistant, corrosion-resistant, and anti-aging waterproof properties, reduces the weight of the membrane, and improves the durability and crack resistance of the waterproof layer.
Smart Images

Figure BDA0005002029490000061 
Figure BDA0005002029490000062 
Figure BDA0005002029490000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of asphalt waterproofing coiled material, and in particular to a light modified asphalt waterproofing coiled material. Background Art
[0002] Waterproofing membrane is a rollable sheet-like waterproofing material. The choice of waterproofing membrane has a great impact on the quality and durability of the waterproof layer. Correct selection and reasonable use of waterproofing membrane is the key to the success of roof waterproofing design. Ordinary waterproofing membranes have the disadvantages of low tensile strength, low tear strength, small elongation at break, poor heat resistance, poor low temperature flexibility, corrosion resistance, and easy aging.
[0003] Lightweight modified asphalt waterproofing membrane is a material used for waterproofing building roofs and underground structures. Current asphalt waterproofing membranes are often made of heavy calcium or mineral powder materials. Generally, the overall weight of asphalt waterproofing membranes is heavy, and fly ash can be used as a replacement material for production, and the cost is lower than heavy calcium or mineral powder.
[0004] To solve the above problems, we proposed a lightweight modified asphalt waterproof membrane. Summary of the invention
[0005] The purpose of the present invention is to solve the problems in the background technology and to propose a lightweight modified asphalt waterproofing membrane.
[0006] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a light modified asphalt waterproofing coiled material, comprising a waterproofing coiled material, the waterproofing coiled material comprising an upper surface layer 1, a lower surface layer 1, an upper surface layer 2, a lower surface layer 2, and an intermediate layer, the intermediate layer is located between the upper surface layer 2 and the lower surface layer 2, the upper surface layer 2 is located between the upper surface layer 1 and the intermediate layer, the lower surface layer 2 is located between the lower surface layer 1 and the intermediate layer, the upper surface layer 1 and the upper surface layer 2 are located above the intermediate layer, the lower surface layer 1 and the lower surface layer 2 are located below the intermediate layer, the intermediate layer is made of polyester cloth, polypropylene film, polyethylene film, the upper surface layer 2 and the lower surface layer 2 are made of asphalt, heavy calcium, ultrafine fly ash, polyester tire cloth, mineral powder, styrene-butadiene rubber, styrene-butadiene copolymer, rubber powder, and graphene;
[0007] The asphalt is hard asphalt, and the formula of the hard asphalt is: asphalt with a needle penetration of 1mm, dehydrogenated asphalt and asphalt with a needle penetration of 10mm, the asphalt is mixed in a ratio of 1:0.2-0.5:4.5-5.5, the asphalt is lighter than water, and the asphalt density is less than 1.
[0008] In the above-mentioned lightweight modified asphalt waterproofing membrane, the upper surface layer 1 and the lower surface layer 1 are both made of polyethylene film, paraffin, coating resin, and adhesive material.
[0009] In the above-mentioned lightweight modified asphalt waterproofing membrane, the upper surface layer 2 and the lower surface layer 2 are composed of 35%-41% asphalt, 5%-10% heavy calcium carbonate, 35%-45% ultrafine fly ash, 1%-5% polyester tire cloth, 2% mineral powder, 1%-5% styrene-butadiene rubber, 2% tire rubber powder, and 1%-3% graphene.
[0010] In the above-mentioned lightweight modified asphalt waterproofing membrane, the upper surface layer 2 and the lower surface layer 2 are composed of 36%-42% asphalt, 6%-9% heavy calcium carbonate, 35%-45% ultrafine fly ash, 1%-5% polyester tire cloth, 3% mineral powder, 1%-5% styrene-butadiene rubber, 1%-5% tire rubber powder, and 1%-3% graphene.
[0011] In the above-mentioned lightweight modified asphalt waterproofing membrane, the upper surface layer 2 and the lower surface layer 2 are composed of 38%-40% asphalt, 5%-10% heavy calcium carbonate, 38%-43% ultrafine fly ash, 1%-6% polyester tire cloth, 2% mineral powder, 2%-7% styrene-butadiene rubber, 1% tire rubber powder, and 1%-3% graphene.
[0012] In the above-mentioned lightweight modified asphalt waterproof membrane, the asphalt layer is composed of the following proportions: the upper surface layer two and the lower surface layer two are composed of the following proportions: the upper surface layer two and the lower surface layer two are composed of the following proportions: asphalt 40%-45%, heavy calcium 8%-11%, ultrafine fly ash 36%-45%, polyester tire cloth 2%-4%, mineral powder 2%, styrene-butadiene rubber 3%-5%, tire rubber powder 1%, and graphene 1%-3%.
[0013] Compared with the existing technology, the advantages of this lightweight modified asphalt waterproof membrane are:
[0014] 1. Fly ash is a gray fine powder, a byproduct of coal combustion, which can improve durability and crack resistance. Ultrafine fly ash is lighter than ordinary fly ash, which can reduce the weight of the coil;
[0015] 2. The asphalt is hard asphalt. The formula of hard asphalt is: asphalt with a needle penetration of 1mm, dehydrogenated asphalt and a needle penetration of 10mm. The asphalt is mixed in a ratio of 1:0.2-0.5:4.5-5.5. The asphalt is lighter than water and has a density of less than 1. Asphalt is one of the main components of waterproof membranes. It provides the main protective function of the waterproof layer. Modified asphalt has polymers or other additives added to it to improve its flexibility, weather resistance and anti-aging properties. Asphalt with a density of less than 1 is lighter than water, which can also greatly reduce the weight of the membrane. DETAILED DESCRIPTION
[0016] The following examples are for illustrative purposes only and are not intended to limit the scope of the present invention.
[0017] A lightweight modified asphalt waterproofing coiled material, comprising a waterproofing coiled material, the waterproofing coiled material comprising an upper surface layer 1, a lower surface layer 1, an upper surface layer 2, a lower surface layer 2, and an intermediate layer, wherein the intermediate layer is located between the upper surface layer 2 and the lower surface layer 2, the upper surface layer 2 is located between the upper surface layer 1 and the intermediate layer, the lower surface layer 2 is located between the lower surface layer 1 and the intermediate layer, the upper surface layer 1 and the upper surface layer 2 are located above the intermediate layer, the lower surface layer 1 and the lower surface layer 2 are located below the intermediate layer, the intermediate layer is made of polyester cloth, polypropylene film, and polyethylene film, and the upper surface layer 2 and the lower surface layer 2 are made of asphalt, heavy calcium, ultrafine fly ash, polyester tire cloth, mineral powder, styrene-butadiene rubber, styrene-butadiene copolymer, rubber powder, and graphene;
[0018] The asphalt is hard asphalt. The formula of hard asphalt is: asphalt with a needle penetration of 1mm, dehydrogenated asphalt and 10mm needle penetration. The asphalt is mixed in a ratio of 1:0.2-0.5:4.5-5.5. The asphalt is lighter than water and has a density of less than 1. Asphalt is one of the main components of waterproof membranes. It provides the main protective function of the waterproof layer. Modified asphalt is added with polymers or other additives to improve its flexibility, weather resistance and anti-aging properties. Asphalt with a density of less than 1 is lighter than water, which can also greatly reduce the weight of the membrane. Fly ash is a gray fine powder that is produced by coal combustion. The by-products produced in the process can improve durability and crack resistance. The weight of ultrafine fly ash is lower than that of general fly ash, which can reduce the weight of the coil. Styrene-butadiene rubber is a synthetic rubber, also known as SBR, which can improve the heat resistance, cold resistance and oil resistance of rubber. Tire rubber powder can be recycled and mixed with asphalt to improve elasticity and durability. Graphene is a two-dimensional crystal structure composed of a single layer of carbon atoms with many unique physical and chemical properties. Graphene has good chemical stability and exhibits excellent corrosion resistance in many environments.
[0019] The upper surface layer 1 and the lower surface layer 1 are both made of polyethylene film, paraffin, coating resin and adhesive. Polyethylene film is a common anti-sticking layer material for waterproof membranes, and has good anti-sticking properties, which can effectively prevent the membranes from sticking together during storage and transportation. Paraffin is a commonly used anti-sticking layer material, which has good anti-sticking and waterproof properties, and can ensure that the waterproof membranes will not stick together during storage and transportation. The anti-sticking layers of some waterproof membranes are made of special coating resins. These resins have good adhesion and weather resistance, which can effectively prevent the membranes from sticking together and provide additional protection. The adhesive is a commonly used anti-sticking layer material, which can coat a thin film of adhesive on the bottom of the waterproof membrane to prevent the membrane from sticking together during storage and transportation, and provide good adhesion during construction.
[0020] The upper surface layer 2 and the lower surface layer 2 are composed of 35%-41% asphalt, 5%-10% heavy calcium, 35%-45% ultrafine fly ash, 1%-5% polyester tire cloth, 2% mineral powder, 1%-5% styrene-butadiene rubber, 2% tire rubber powder and 1%-3% graphene.
[0021] The upper surface layer 2 and the lower surface layer 2 are composed of 36%-42% asphalt, 6%-9% heavy calcium, 35%-45% ultrafine fly ash, 1%-5% polyester tire cloth, 3% mineral powder, 1%-5% styrene-butadiene rubber, 1% tire rubber powder, and 1%-3% graphene.
[0022] The upper surface layer 2 and the lower surface layer 2 are composed of 38%-40% asphalt, 5%-10% heavy calcium, 38%-43% ultrafine fly ash, 1%-6% polyester tire cloth, 2% mineral powder, 2%-7% styrene-butadiene rubber, 1% tire rubber powder and 1%-3% graphene.
[0023] The upper surface layer two and the lower surface layer two are made in proportion as follows: the upper surface layer two and the lower surface layer two are made in proportion as follows: 40%-45% asphalt, 8%-11% heavy calcium, 36%-45% ultrafine fly ash, 2%-4% polyester tire cloth, 2% mineral powder, 3%-5% styrene-butadiene rubber, 1% tire rubber powder and 1%-3% graphene.
[0024] A lightweight modified asphalt waterproofing membrane, the ice melting test results are shown in Table 1 and Table 2: HCl-PANI mass content 1%, 1000W ice melting
[0025] Table 1
[0026] Distilled water Tap water Roof waterproof coating 3min 7s 3min 11s Asphalt waterproof membrane 2min 40s 2min 45s
[0027] 1000W ice melting, material size 4×4cm
[0028] Table 2
[0029]
[0030] The results of the test sand drop quantity are shown in Table 3:
[0031] The material size is 4×4cm. Use a steel wool to brush 5 times with the same force. The number of sands dropped is shown in Table 3.
[0032] raw materials HCl-PANI PFOA-PANI Red Sand 16 20 16 Fine sand 35 30 15 Shale 22 18 13 Emery 25 22 26
[0033] The application of new materials in waterproof membranes is shown in Table 4:
[0034] Table 4
[0035]
[0036]
[0037]
[0038] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A lightweight modified asphalt waterproofing membrane, a lightweight modified asphalt waterproofing membrane, comprising a waterproofing membrane, characterized in that: The waterproof coiled material comprises an upper surface layer 1, a lower surface layer 1, an upper surface layer 2, a lower surface layer 2, and an intermediate layer, wherein the intermediate layer is located between the upper surface layer 2 and the lower surface layer 2, the upper surface layer 2 is located between the upper surface layer 1 and the intermediate layer, the lower surface layer 2 is located between the lower surface layer 1 and the intermediate layer, the upper surface layer 1 and the upper surface layer 2 are located above the intermediate layer, the lower surface layer 1 and the lower surface layer 2 are located below the intermediate layer, the intermediate layer is made of polyester cloth, polypropylene film, and polyethylene film, and the upper surface layer 2 and the lower surface layer 2 are made of asphalt, heavy calcium, ultrafine fly ash, polyester tire cloth, mineral powder, styrene-butadiene rubber, styrene-butadiene copolymer, rubber powder, and graphene; The asphalt is hard asphalt, and the formula of the hard asphalt is: asphalt with a needle penetration of 1mm, dehydrogenated asphalt and asphalt with a needle penetration of 10mm, the asphalt is mixed in a ratio of 1:0.2-0.5:4.5-5.5, the asphalt is lighter than water, and the asphalt density is less than 1.
2. A lightweight modified asphalt waterproofing membrane according to claim 1, characterized in that: The upper surface layer 1 and the lower surface layer 1 are both made of polyethylene film, paraffin, coating resin and adhesive.
3. A lightweight modified asphalt waterproofing membrane according to claim 1, characterized in that: The upper surface layer 2 and the lower surface layer 2 are made of the following proportions: 35%-41% asphalt, 5%-10% heavy calcium, 35%-45% ultrafine fly ash, 1%-5% polyester tire cloth, 2% mineral powder, 1%-5% styrene-butadiene rubber, 2% tire rubber powder, and 1%-3% graphene.
4. The lightweight modified asphalt waterproofing membrane according to claim 1, characterized in that: The upper surface layer 2 and the lower surface layer 2 are composed of 36%-42% asphalt, 6%-9% heavy calcium, 35%-45% ultrafine fly ash, 1%-5% polyester tire cloth, 3% mineral powder, 1%-5% styrene-butadiene rubber, 1% tire rubber powder, and 1%-3% graphene.
5. The lightweight modified asphalt waterproofing membrane according to claim 1, characterized in that: The upper surface layer 2 and the lower surface layer 2 are made of the following proportions: 38%-40% asphalt, 5%-10% heavy calcium, 38%-43% ultrafine fly ash, 1%-6% polyester tire cloth, 2% mineral powder, 2%-7% styrene-butadiene rubber, 1% tire rubber powder, and 1%-3% graphene.
6. The lightweight modified asphalt waterproofing membrane according to claim 1, characterized in that: The upper surface layer 2 and the lower surface layer 2 are made in the following proportions: 40%-45% asphalt, 8%-11% heavy calcium carbonate, 36%-45% ultrafine fly ash, 2%-4% polyester tire cloth, 2% mineral powder, 3%-5% styrene-butadiene rubber, 1% tire rubber powder, and 1%-3% graphene.
Citation Information
Patent Citations
Flame-retardant polymer modified asphalt waterproof roll and preparation method thereof
CN102134810A
Modified asphalt waterproof coiled material with heat insulation function and preparation method thereof
CN102409812A
Asphalt modified waterproof rolled material
CN102852235A
Modified asphalt of waterproof roll and preparation method of modified asphalt
CN107739519A
Low-temperature anti-cracking self-adhesive modified bituminous waterproof roll material and preparation method
CN110001174A
Cited By
Asphalt coating material for waterproof coiled material, preparation method of asphalt coating material and asphalt waterproof coiled material
CN122105881A