Method for preparing rock wool by using red mud base through three-step method

Through a three-step process of red mud treatment, including dealkalization, iron removal and composition conditioning, rock wool products suitable for construction purposes are prepared, which solves the problem of shortage of traditional rock wool production resources and environmental pollution, and realizes the resource utilization of red mud. Demand for wall materials for reuse and construction.

CN118812166APending Publication Date: 2024-10-22LIAOCHENG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410709833.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The production of traditional basalt mineral rock wool requires a large amount of mineral raw materials, resulting in resource shortages and environmental pollution. Red mud, as a solid waste from alumina production, has complex composition and is not suitable for direct use in the production of rock wool. In addition, organic insulation materials have poor fire protection levels and have problems in buildings. Application problems.

Method used

A three-step process is used to treat red mud, including dealkalization, iron removal and component conditioning. Rock wool fibers are formed through melting in an electric furnace and spinning processes to prepare rock wool products suitable for construction purposes.

Benefits of technology

It has realized the low-cost production of rock wool, reduced the problem of red mud pollution, reused mineral resources, met the demand for building wall materials, and solved the problem of red mud occupying cultivated land and pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812166A_ABST
    Figure CN118812166A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of rock wool production, in particular to a method for preparing rock wool from a red mud base through a three-step method. The method comprises the following steps: carrying out one-step dealkalization and two-step deironing on red mud to realize component hardening and tempering, carrying out mixing hardening and tempering, pressing into blocks, melting in an electric melting furnace, forming rock wool fibers through a thread throwing process, and carrying out post-treatment to prepare a rock wool product. The red mud-based rock wool production technology has the beneficial effects that low-cost rock wool production can be realized, the pollution problem of red mud can be reduced, resource reutilization can be realized, and compared with common rock wool products, mineral resources can be saved, and the use of building wall materials can be met; the red mud can be consumed in a large amount, the problems of land use and pollution of the red mud are solved, resource reutilization of the red mud can be achieved, and waste is turned into wealth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rock wool production, and in particular to a three-step method for preparing rock wool using red mud. Background Art

[0002] At present, the widely used building wall insulation materials mainly include organic insulation materials such as polystyrene foam and polyurethane foam, and basalt mineral rock wool and other material systems. However, organic insulation materials have poor fire resistance and there are many problems in their application in the construction field. Rock wool for exterior walls is a multifunctional building insulation material. Its function is not limited to energy saving and heat preservation, but also includes sound insulation and noise reduction, fire prevention, moisture prevention, earthquake resistance and crack prevention. In building insulation and decoration, choosing rock wool for exterior walls is a wise choice, which can create a more comfortable, safe and environmentally friendly living space for us. However, the production of traditional basalt mineral rock wool requires a large amount of mineral raw materials. As mineral mining is greatly restricted in terms of policy and resource reserves, it is extremely urgent to seek a substitute for mineral raw materials.

[0003] As a solid waste in alumina production, red mud has long been a problem of pollution and occupation of arable land, which has long been a pain point hindering the sustainable development of the aluminum industry. At the same time, red mud has complex components and is not suitable for direct use in the production of rock wool, which is also one of the main technical problems in this field today. Summary of the invention

[0004] The invention discloses a three-step method for preparing rock wool using red mud as a base, so as to solve any of the above-mentioned technical problems and other potential problems in the prior art.

[0005] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a three-step method for preparing rock wool using red mud as a base, which realizes component tempering through one-step dealkalization and two-step iron removal, and then mixes and tempers, presses into blocks, and then melts in an electric furnace, forms rock wool fibers through a spinning process, and then undergoes post-processing to form rock wool products.

[0006] Furthermore, the method specifically comprises the following steps:

[0007] S1) the selected raw material red mud is treated by soaking and washing to complete the dealkalization, and then set aside;

[0008] S2) removing iron from the raw red mud treated in S1) by a magnetic roasting-magnetic separation method and setting aside;

[0009] S3) mixing the raw red mud treated in S2) with a certain amount of solid waste, completing component conditioning, pressing into blocks, then melting in an electric furnace, forming rock wool fibers through a spinning process, and then post-processing to form rock wool products;

[0010] The order of the above steps cannot be adjusted.

[0011] Furthermore, in said S1), after mixing the raw red mud with the solvent, the mixture is heated to 70-90° C., soaked for 3-5 hours, and the obtained slag is rinsed at least 3 times.

[0012] Furthermore, the solvent is water.

[0013] Further, the specific process of S2) is:

[0014] S2.1) heating the raw red mud treated in S1) to a temperature of 700-750°C, introducing a reducing atmosphere, and calcining for 3-5 hours to obtain a block material;

[0015] S2.2) Grinding the block material obtained in S2.1) and performing weak magnetic separation to separate iron from the raw red mud to obtain iron concentrate.

[0016] Furthermore, the reducing atmosphere is CO.

[0017] Further, the specific process of S3) is:

[0018] S3.1) mixing the raw red mud treated in S2) with solid waste and pressing them into blocks, wherein the mass percentage of the raw red mud is 70-75% and the mass percentage of the solid waste is 25-30%;

[0019] S3.2) placing the block obtained in S3.1) in a furnace, melting it at a temperature of 1400-1500°C to obtain a melt, and centrifuging the melt at a speed of not less than 5000 r / m into fibers to obtain a rock wool product.

[0020] Furthermore, the components of the obtained rock wool products are: 45% to 50% SiO2, 15% to 20% Al2O3, 10% to 15% Fe2O3, 15% to 20% CaO, 5-8% MgO, and 5-7% other oxides (TiO2, Na2O).

[0021] Furthermore, the mass percentages of the various components of the solid waste are: silicon powder 8-10%; fly ash: 10-15%; quicklime 2-3%; coal gangue: 3-5%.

[0022] A rock wool is prepared by adopting the above method.

[0023] The beneficial effects of the present invention are as follows: due to the adoption of the above technical scheme, the red mud-based rock wool production technology proposed in the present invention can realize low-cost production of rock wool, which can reduce the pollution problem of red mud and realize resource recycling. Compared with general rock wool products, it can save mineral resources and meet the use of building wall materials;

[0024] It can not only consume a large amount of red mud and solve the problems of red mud land use and pollution, but also realize the resource reuse of red mud and turn waste into treasure. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The present invention is a flowchart of a three-step method for preparing rock wool using red mud as a base. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0027] like Figure 1 As shown, the present invention provides a three-step method for preparing rock wool using red mud, and the method specifically comprises the following steps:

[0028] S1) the selected raw material red mud is treated by soaking and washing to complete the dealkalization, and then set aside;

[0029] The specific process is:

[0030] The raw red mud is mixed with a solvent, heated to 70-90°C, soaked for 3-5 hours, and the obtained slag is rinsed at least 3 times. The solvent is water.

[0031] This step uses soaking and washing to carry out dealkalization, thereby dissolving the free alkali components contained in the red mud, so that the content of Na2O is reduced from 3.641% to 2.215%.

[0032] S2) removing iron from the raw red mud treated in S1) by a magnetic roasting-magnetic separation method and setting aside;

[0033] The specific process is:

[0034] The raw material red mud is heated to a temperature of 700-750°C, introduced into a reducing atmosphere, and roasted for 3-5 hours to obtain a block material; the obtained block material is ground and subjected to weak magnetic separation to separate iron from the raw material red mud to obtain iron concentrate.

[0035] The reducing atmosphere is CO.

[0036] The hematite (Fe2O3) with weaker magnetism in the red mud is converted into magnetite (Fe3O4) with stronger magnetism, and the content of Fe2O3 in the red mud is reduced from 55.981% to 18.651%.

[0037] S3) The raw red mud treated in S2) is mixed with a certain amount of solid waste to complete the component conditioning, pressed into blocks, and then melted in an electric furnace to form rock wool fibers through a spinning process, and then post-processed to form rock wool products.

[0038] S3.1) mixing the raw red mud treated in S2) with solid waste and pressing them into blocks, wherein the mass percentage of the raw red mud is 70-75% and the mass percentage of the solid waste is 25-30%;

[0039] S3.2) placing the block obtained in S3.1) in a furnace, melting it at a temperature of 1400-1500°C to obtain a melt, and centrifuging the melt at a speed of not less than 5000 r / m into fibers to obtain a rock wool product.

[0040] The components of the obtained rock wool products are: 45% to 50% SiO2, 15% to 20% Al2O3, 10% to 15% Fe2O3, 15% to 20% CaO, 5-8% MgO, and 5-7% other oxides (TiO2, Na2O).

[0041] The mass percentages of the various components of the solid waste are: silicon powder 8-10%; fly ash: 10-15%; quicklime: 2-3%; coal gangue: 3-5%.

[0042] Embodiment 1:

[0043] A three-step method for preparing rock wool using red mud.

[0044] S1) mixing the raw red mud with water, heating to 70° C., soaking for 3.5 hours, and washing the obtained slag with water at least 3 times; this step dissolves the free alkali components contained in the red mud, so that the content of Na2O is reduced from 3.641% to 2.215%, and the obtained soaking liquid can be used as an alkali liquid to temper the acidity and desulfurization process of subsequent production of rock wool.

[0045] After the raw red mud treated by S1) is heated to a temperature of 700°C, CO is introduced and roasted for 3.5 hours to obtain a block material; the obtained block material is ground and weakly magnetically separated from the iron in the raw red mud to obtain iron concentrate and raw red mud, and the magnetite is recovered. This step can not only obtain the refined iron ore directly for ironmaking, but also provide high-quality raw materials for the subsequent red mud-based rock wool production. The content of Fe2O3 in red mud is reduced from 55.981% to 18.651%.

[0046] S3) mixing the raw red mud treated in S2) with solid waste and pressing them into blocks, wherein the mass percentage of the raw red mud is 70% and the mass percentage of the solid waste is 30%; placing the obtained blocks in a furnace, melting them at a temperature of 1400° C. to obtain a melt, and centrifuging the melt at a speed of not less than 5000 r / m to form fibers, thereby obtaining rock wool products.

[0047] The components of the obtained rock wool products are: 45% to 50% SiO2, 15% to 20% Al2O3, 10% to 15% Fe2O3, 15% to 20% CaO, 5-8% MgO, and 5-7% other oxides (TiO2, Na2O).

[0048] The mass percentages of the various components of the solid waste are: silicon powder 8%; fly ash: 10%; quicklime 2%; coal gangue: 3%.

[0049] The components of red mud before and after modification were tested by phase analysis, and the properties of rock wool after production were also tested. The results of the component comparison before and after red mud modification are shown in Table 1, and the properties of rock wool after production are shown in Table 2.

[0050]

[0051] Table 1

[0052]

[0053] Table 2

[0054] Embodiment 2:

[0055] A three-step method for preparing rock wool using red mud.

[0056] S1) mixing the raw red mud with water, heating to 80°C, soaking for 4 hours, and washing the obtained slag with water at least 3 times; this step dissolves the free alkali components contained in the red mud;

[0057] After the raw red mud treated in S1) is heated to a temperature of 750°C, CO is introduced and roasted for 4 hours to obtain a block material; the obtained block material is ground and weakly magnetically separated to obtain iron concentrate and raw red mud, and the magnetite is recovered. This step can not only obtain the iron concentrate for direct ironmaking, but also provide high-quality raw materials for the subsequent red mud-based rock wool production.

[0058] S3) mixing the raw red mud treated in S2) with solid waste and pressing them into blocks, wherein the mass percentage of the raw red mud is 72.5% and the mass percentage of the solid waste is 27.5%; placing the obtained blocks in a furnace, melting them at a temperature of 1450° C. to obtain a melt, and centrifuging the melt at a speed of not less than 5000 r / m to form fibers, thereby obtaining rock wool products.

[0059] The components of the obtained rock wool products are: 45% to 50% SiO2, 15% to 20% Al2O3, 10% to 15% Fe2O3, 15% to 20% CaO, 5-8% MgO, and 5-7% other oxides (TiO2, Na2O).

[0060] The mass percentages of the various components of the solid waste are: silicon powder 9%; fly ash: 12.5%; quicklime: 2.5%; coal gangue: 4%.

[0061] Embodiment 3:

[0062] A three-step method for preparing rock wool using red mud.

[0063] S1) mixing the raw red mud with water, heating to 90°C, soaking for 5 hours, and washing the obtained slag with water at least 3 times; this step dissolves the free alkali components contained in the red mud;

[0064] After the raw red mud treated in S1) is heated to a temperature of 750°C, CO is introduced and roasted for 5 hours to obtain a block material; the obtained block material is ground and weakly magnetically separated from the iron in the raw red mud to obtain iron concentrate and raw red mud, and the magnetite is recovered. This step can not only obtain the iron concentrate for direct use in ironmaking, but also provide high-quality raw materials for the subsequent red mud-based rock wool production.

[0065] S3) mixing the raw red mud treated in S2) with solid waste and pressing them into blocks, wherein the mass percentage of the raw red mud is 75% and the mass percentage of the solid waste is 25%; placing the obtained blocks in a furnace, melting them at a temperature of 1500° C. to obtain a melt, and centrifuging the melt at a speed of not less than 5000 r / m to form fibers, thereby obtaining rock wool products.

[0066] The components of the obtained rock wool products are: 45% to 50% SiO2, 15% to 20% Al2O3, 10% to 15% Fe2O3, 15% to 20% CaO, 5-8% MgO, and 5-7% other oxides (TiO2, Na2O).

[0067] The mass percentages of the various components of the solid waste are: silicon powder 10%; fly ash: 15%; quicklime: 3%; coal gangue: 5%.

[0068] The above is a detailed introduction to a three-step method for preparing rock wool using red mud provided in the embodiment of the present application. The description of the above embodiment is only used to help understand the method and its core idea of ​​the present application; at the same time, for those skilled in the art, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present application.

[0069] For example, certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that hardware manufacturers may use different nouns to refer to the same component. This specification and claims do not use differences in names as a way to distinguish components, but use differences in the functions of components as the criteria for distinction. As mentioned throughout the specification and claims, "including" and "comprising" are open-ended terms, so they should be interpreted as "including / including but not limited to". "Approximately" means that within an acceptable error range, those skilled in the art can solve the technical problem within a certain error range and basically achieve the technical effect. The subsequent description of the specification is a preferred embodiment of the present application, but the description is for the purpose of illustrating the general principles of the present application, and is not used to limit the scope of the present application. The scope of protection of the present application shall be determined by the definition of the attached claims.

[0070] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such a product or system. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the product or system including the elements.

[0071] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0072] The above description shows and describes several preferred embodiments of the present application, but as mentioned above, it should be understood that the present application is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present application, and should be within the scope of protection of the claims attached to the present application.

Claims

1. A three-step method for preparing rock wool using red mud, characterized in that: The method achieves component conditioning through one-step dealkalization and two-step iron removal, then performs mixed conditioning, presses into blocks, then melts in an electric furnace, forms rock wool fibers through a spinning process, and then produces rock wool products through post-processing.

2. The method according to claim 1, characterized in that The method specifically comprises the following steps: S1) the selected raw material red mud is treated by soaking and washing to complete the dealkalization, and then set aside; S2) removing iron from the raw red mud treated in S1) by a magnetic roasting-magnetic separation method and setting aside; S3) The raw red mud treated in S2) is mixed with a certain amount of solid waste to complete the component conditioning, pressed into blocks, and then melted in an electric furnace to form rock wool fibers through a spinning process, and then post-processed to make rock wool products.

3. The method according to claim 2, characterized in that In the step S1), the raw red mud is mixed with the solvent, heated to 70-90° C., and soaked for 3-5 hours, and the obtained slag is rinsed at least 3 times.

4. The method according to claim 3, characterized in that The solvent is water.

5. The method according to claim 2, characterized in that: The specific process of S2) is: S2.1) heating the raw red mud treated in S1) to a temperature of 700-750°C, introducing a reducing atmosphere, and calcining for 3-5 hours to obtain a block material; S2.2) Grinding the block material obtained in S2.1) and performing weak magnetic separation to separate iron from the raw red mud to obtain iron concentrate.

6. The method according to claim 5, characterized in that The reducing atmosphere in S2.1) is CO.

7. The method according to claim 1, characterized in that The specific process of S3) is: S3.1) mixing the raw red mud treated in S2) with solid waste and pressing them into blocks, wherein the mass percentage of the raw red mud is 70-75% and the mass percentage of the solid waste is 25-30%; S3.2) placing the block obtained in S3.1) in a furnace, melting it at a temperature of 1400-1500°C to obtain a melt, and centrifuging the melt at a speed of not less than 5000 r / m into fibers to obtain a rock wool product.

8. The method according to claim 7, characterized in that The mass percentage of each component of the solid waste is 8-10% silicon powder; 10-15% fly ash; 2-3% quicklime; and 3-5% coal gangue.

9. The method according to claim 7, characterized in that: The various components of the obtained rock wool products are: 45% to 50% SiO2, 15% to 20% Al2O3, 10% to 15% Fe2O3, 15% to 20% CaO, 5-8% MgO, and 5-7% other oxides.

10. A rock wool, characterized in that: The rock wool is prepared by the method as claimed in any one of claims 1 to 9.