Preparation method of catalyst solid component for olefin polymerization and catalyst

By dissolving magnesium alkoxide in the presence of a dispersant and using a precipitation aid to precipitate solid components, combined with an internal electron donor, the problem of inappropriate particle morphology and size in the prior art is solved, and a high-activity and low-toxicity catalyst is achieved. preparation, reducing resource waste and preparation complexity.

CN118812751AActive Publication Date: 2024-10-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310423132.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-22
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

When preparing magnesium alkoxide catalysts in the prior art, there is a problem of inappropriate particle morphology and size leading to waste of resources, and commonly used dissolving agents such as o-cresol are physiologically irritating, and the dissolution process is complex and inefficient.

Method used

A non-toxic substance system is used to dissolve the magnesium alkoxide, the solid component is precipitated through a precipitation aid, and the internal electron donor is loaded to prepare a catalyst with good particle shape and high polymerization activity. Specific steps include contacting magnesium alkoxide, alcohol compounds and titanium halide in the presence of a dispersant, adding organic epoxy compounds and phosphorus compounds to form a uniform solution, and then adding titanium halide and a precipitation aid for the third contact. Reaction, forming a suspension and solid-liquid separation, and finally reacting with the internal electron donor.

Benefits of technology

It realizes the preparation of catalysts that are not limited by particle morphology, reduces waste of resources, avoids the use of toxic substances, improves the activity of the catalyst and particle morphology, and simplifies the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004190493980000061
    Figure BDA0004190493980000061
  • Figure BDA0004190493980000201
    Figure BDA0004190493980000201
  • Figure FDA0004190493970000021
    Figure FDA0004190493970000021
Patent Text Reader

Abstract

The invention relates to a preparation method of a catalyst solid component for olefin polymerization and a catalyst. According to the method, alkoxy magnesium which is not limited by particle morphology is used as an initial raw material, the alkoxy magnesium dissolving solution is prepared by adopting a non-toxic substance system, then solid components are separated out by virtue of a separation aid, and an internal electron donor is loaded, so that the catalyst which is good in particle morphology and high in polymerization activity and is used for olefin polymerization is finally prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalysts, and more specifically, to a method for preparing a solid component of a catalyst for olefin polymerization and a catalyst. The olefin polymerization catalyst is an olefin polymerization main catalyst prepared by dissolving and precipitating alkoxy magnesium as an initial substance. The main catalyst is converted into an olefin polymerization catalyst by contacting with a co-catalyst and an optional external electron donor. Background Art

[0002] At present, countries around the world have been using a large number of polymers and copolymers of low-level α-olefins to meet the needs of various aspects of social life. These polymer products have the characteristics of low manufacturing cost and wide range of industrial applications. The most common form of these polymers is highly crystalline solids. In the polymerization process, whether it is through liquid phase, gas phase, slurry polymerization or any other common polymerization method, the morphology of the catalyst particles and the polymer particles is required to be in the required shape and size to varying degrees, among which the morphology of the catalyst carrier particles plays a decisive role. Therefore, the preparation process of the main catalyst is crucial for producing polymer particles of qualified shape and size.

[0003] As is well known, there are mainly two ways to prepare Ziegler-Natta catalysts using alkoxymagnesium as initial material. The way to prepare Ziegler-Natta catalysts using alkoxymagnesium as initial material published by Chinese patents CN101906017A and CN102399326 A is to first use metal magnesium, alcohols and halogenating agents to react under specific conditions to prepare alkoxymagnesium carrier particles, then use alkoxymagnesium particles to control a certain temperature to contact with titanium halide, then react with as an internal electron donor compound, then treat with titanium halide to obtain a solid catalyst component. The catalyst prepared by the method has a higher bulk density and good particle morphology, and has high activity during polymerization, and the obtained polymer has the characteristics of good stereoregularity, good particle morphology, and less fine powder content. However, when preparing alkoxymagnesium particle carriers, a part of the carrier particles will be treated as hazardous waste because of the form or size that is not suitable for subsequent catalyst preparation, increasing the processing cost and causing waste of resources.

[0004] U.S. Patents No. 5,082,907, No. 5,151,399, No. 5,229,342, No. 5,106,806, No. 5,146,028, No. 5,066,737, No. 5,124,298 and No. 5,077,357 disclose various catalyst precursors containing magnesium and titanium, some of which are prepared using the above-mentioned magnesium alkoxide as the initial material. These precursors have no polymerization catalyst activity and do not contain any effective electron donor, but these precursors are used as starting materials in the subsequent conversion into active procatalysts. The magnesium and titanium procatalyst is either formed by direct chlorination of the magnesium and titanium precursor or by reacting the magnesium and titanium precursor with a tetravalent titanium halide, an optional hydrocarbon and an optional electron donor. The prepared procatalyst solid is then separated from the reaction slurry (by filtering, precipitation, crystallization, etc.), and then these main catalysts are reacted with cocatalysts and selectivity control agents to be converted into polymerization catalysts. US Pat. No. 5,034,361 discloses dissolving alkoxymagnesium in an alkanol solvent by allowing the alkoxymagnesium compound to interact with certain acidic substances. Then, the magnesium-containing catalyst precursor is reacted with various titanium compounds to prepare a catalyst precursor containing magnesium and titanium.

[0005] When alkoxymagnesium such as ethoxymagnesium is used as a starting material to form a procatalyst precursor, a truncating agent is often required to break the aggregated ethoxymagnesium and react it with other components. As disclosed in U.S. Pat. Nos. 5,124,298 and 5,077,357, the precursor is made with chlorobenzene as a solvent and o-cresol as a truncating agent to chemically break the aggregated ethoxymagnesium. A small amount of o-cresol (1-3%) is retained in the precursor product. In addition to being physiologically irritating, it will still become a polymerization catalyst poison if it is not effectively filtered out in the catalyst preparation step. In addition to the truncating agents including physiologically irritating phenolic compounds such as p-cresol, 3-methoxyphenol, 4-dimethylaminophenol introduced in the above patents, there are many methods that use borate-containing solubilizing agents to complete the dissolution of alkoxymagnesium so that the reaction of the magnesium compound can be carried out in the liquid phase. This method is relatively complicated because a precipitant is required to precipitate the solid product, and because some raw materials are lost during the dissolution process, the cost is high and the efficiency is low.

[0006] Therefore, it is of great significance to find a substance or material system that will not irritate the personnel who prepare the catalyst and will not be toxic to the polymerization catalyst to promote the dissolution of alkoxymagnesium. On this basis, a method for preparing the final catalyst using the solution after dissolving alkoxymagnesium can be found to get rid of the limitation of the morphology of alkoxymagnesium carrier particles on catalyst preparation.

[0007] The precipitation preparation process of the solid component of the catalyst requires the addition of a specific precipitation aid to improve the particle morphology of the precipitated solid component. For this reason, the inventors have disclosed a series of precipitation aid systems containing 1,3-diol esters, and olefin polymerization catalysts prepared therefrom (CN102276765A, CN101993506A, CN101864009A, CN101643519A, CN103012627A, CN103012625A, CN103012626A). The olefin polymerization catalyst prepared by the precipitation aid system containing 1,3-diol esters contains a small amount of 1,3-diol ester compounds, and the presence of these diol ester compounds greatly improves the particle morphology of the catalyst and increases the activity of the catalyst. Summary of the invention

[0008] The purpose of the present invention is to use alkoxy magnesium which is not restricted by particle morphology as an initial raw material, complete the preparation of alkoxy magnesium solution by adopting a non-toxic material system, then precipitate solid components through a precipitation aid, and then load an internal electron donor, and finally prepare a polyolefin catalyst with good particle morphology and high polymerization activity.

[0009] One of the purposes of the present invention is to provide a method for preparing a solid component of a catalyst, using alkoxymagnesium as a starting material, comprising the following steps:

[0010] (1) subjecting alkoxymagnesium, an alcohol compound and a titanium halide to a first contact reaction in the presence of a dispersant to form a uniformly dispersed slurry;

[0011] (2) Adding a solvent system of an organic epoxy compound and an organic phosphorus compound to the uniform slurry obtained in step (1) to carry out a second contact reaction to form a uniform solution.

[0012] (3) adding a titanium halide to the uniform solution obtained in step (2) in the presence of a precipitation aid to carry out a third contact reaction to precipitate a solid precipitate mixture containing magnesium / titanium;

[0013] (4) subjecting the mixture obtained in step (3) to a fourth contact reaction with an internal electron donor compound to obtain a suspension;

[0014] (5) separating the suspension obtained in step (4) into solid and liquid, and subjecting the solid component obtained by the solid-liquid separation to a fifth contact reaction with a titanium halide to obtain the catalyst solid component.

[0015] According to the present invention, the alkoxy magnesium described in step (1) has the structural formula Mg(OR9)2, and R9 is C1-C 10The hydrocarbon group (such as hydrocarbon group or aromatic hydrocarbon group) is preferably a hydrocarbon group of C2 to C4. The alkoxy magnesium can be any alkoxy magnesium, preferably dialkoxy magnesium, wherein each alkoxy group can be the same or different, and each alkoxy group can contain 1 to 10 carbon atoms, preferably 1 to 5, such as ethoxy magnesium, propoxy magnesium, butoxy magnesium, phenoxy magnesium, etc.

[0016] The alcohol compound in step (1) is C1-C 10 One or more of the straight-chain or branched alcohols, preferably C2 to C 10 The straight-chain alcohol is preferably a C2-C4 straight-chain alcohol, such as methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, isopentanol, hexanol, heptanol, octanol, isooctyl alcohol, nonanol, decanol, etc.

[0017] The titanium halide described in step (1) may be any titanium compound commonly used in the art, for example, a titanium halide having the general formula Ti(OR 10 ) m X 4-m The titanium compound shown in the general formula, R 10 It can be an alkyl group, preferably C1 to C 10 wherein X is a halogen, such as Cl, Br or I, 0≤m≤3, and m is an integer. Preferably, the titanium compound is one or more of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, alkoxy titanium trihalide, dialkoxy titanium dihalide, and trialkoxy titanium halide, preferably titanium tetrachloride.

[0018] The dispersant described in step (1) can be at least one of various alkane compounds, aromatic hydrocarbon compounds or mineral oils commonly used in the art that do not chemically interact with alkoxy magnesium and alcohol compounds. Specific examples can be one or more of alkanes, cycloalkanes, aromatic hydrocarbons, kerosene, vaseline oil, and white oil, preferably one or more of decane, benzene, toluene, and xylene, and more preferably toluene.

[0019] According to the present invention, in step (1), the molar ratio of the alcohol compound to the alkoxymagnesium is controlled at (0.01-2):1, more preferably (0.02-0.8):1, specifically 0.01:1, 0.02:1, 0.05:1, 0.08:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 1:1, 1.5:1, 2:1, etc.; the molar ratio of the titanium halide to the alkoxymagnesium is (0.45-1):1, preferably The molar ratio of the dispersant to the magnesium alkoxide should be (0.5-0.8):1, specifically 0.45:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, etc.; the molar ratio of the dispersant to the magnesium alkoxide should be controlled at (5-50):1, preferably (5-20):1, specifically 5:1, 8:1, 10:1, 13:1, 15:1, 18:1, 20:1, 25:1, 30:1, 35:1, 40:1, 45:1, 50:1, etc.

[0020] According to the present invention, in step (1), the purpose of the first contact reaction is to react the alkoxymagnesium, the alcohol compound and the titanium halide in the presence of a dispersant to form a uniform slurry. The present invention does not specifically limit the conditions for the first contact reaction to form a uniform slurry, which can be determined according to the specific alkoxymagnesium used. Preferably, the reaction conditions can generally include a temperature of 10 to 150°C, preferably 60 to 120°C; a time of 1 to 10 hours, preferably 2 to 6 hours.

[0021] According to the present invention, in step (1), the order of adding the alkoxy magnesium, the alcohol compound, the titanium halide and the dispersant is not specifically limited. Preferably, the order of adding is to first add the alkoxy magnesium, then add the dispersant and stir to achieve uniform dispersion, and then add the titanium halide and the alcohol compound for contact reaction.

[0022] According to the present invention, the organic epoxy compound in step (2) is selected from at least one of the compounds including oxides, glycidyl ethers, and internal ethers of C2-C8 aliphatic monoolefins, dienes, or halogenated aliphatic olefins or dienes. Specifically, it is selected from at least one of ethylene oxide, propylene oxide, butylene oxide, butadiene oxide, butadiene dioxide, epichlorohydrin, methyl glycidyl ether, and diglycidyl ether.

[0023] According to the present invention, in step (2), the organic phosphorus compound is selected from hydrocarbon esters of orthophosphoric acid or phosphorous acid, halogenated hydrocarbon esters of orthophosphoric acid or phosphorous acid, for example, at least one of trimethyl orthophosphate, triethyl orthophosphate, tributyl orthophosphate, triphenyl orthophosphate, trimethyl phosphite, triethyl phosphite, tributyl phosphite, benzyl phosphite, etc.

[0024] According to the present invention, in step (2), relative to 1 mol of alkoxymagnesium calculated as magnesium element, the organic epoxy compound is 0.2 to 10 mol, preferably 0.5 to 4 mol, for example, 0.2 mol, 0.5 mol, 1 mol, 2 mol, 3 mol, 4 mol, 5 mol, 6 mol, 7 mol, 8 mol, 9 mol, 10 mol, etc.; the organic phosphorus compound is 0.1 to 3 mol, preferably 0.3 to 1 mol, for example, 0.1 mol, 0.2 mol, 0.3 mol, 0.4 mol, 0.5 mol, 0.6 mol, 0.7 mol, 0.8 mol, 0.9 mol, 1 mol, 1.5 mol, 2 mol, 3 mol, etc.

[0025] According to the present invention, in step (2), in a preferred case, the second contact reaction conditions may generally include a temperature of 10 to 150° C., preferably 50 to 140° C.; and a time of 0.1 to 10 hours, preferably 0.5 to 6 hours.

[0026] According to the present invention, the precipitation aid in step (3) is a diol ester compound represented by formula (I),

[0027]

[0028] In formula (I), R1 to R2 are the same or different and are each independently a substituted or unsubstituted linear C1 to C 20 Alkyl, substituted or unsubstituted branched C3~C 20 Alkyl, substituted or unsubstituted C3~C 20 Cycloalkyl, substituted or unsubstituted C6~C 20 Aryl, substituted or unsubstituted C7~C 20 Alkyl, substituted or unsubstituted C7~C 20 Arylalkyl, substituted or unsubstituted C2~C 10 Alkenyl, substituted or unsubstituted C 10 ~C 20 R3 to R8 are the same or different and are independently hydrogen, halogen, substituted or unsubstituted straight-chain C1 to C 20 Alkyl, substituted or unsubstituted branched C3~C 20 Alkyl, substituted or unsubstituted C3~C 20 Cycloalkyl, substituted or unsubstituted C6~C 20 Aryl, substituted or unsubstituted C7~C 20 Alkyl, substituted or unsubstituted C7~C 20 Arylalkyl, substituted or unsubstituted C2~C 10 Alkenyl, substituted or unsubstituted C 10 ~C 20 A condensed ring aromatic group; or at least one of R3 to R6 forms a ring with at least one of R7 to R8.

[0029] Preferably, the precipitation aid can be 2-ethyl-1,3-propylene glycol dibenzoate, 2-propyl-1,3-propylene glycol dibenzoate, 2-isopropyl-2-isopentyl-1,3-propylene glycol dibenzoate, 1,3-butylene glycol dimethyl benzoate, 2-methyl-1,3-butylene glycol di-m-chlorobenzoate, 2,3-dimethyl-1,3-butylene glycol dibenzoate, 1,3-pentanediol dipivalate, 2,4-pentanediol dibenzoate, 2-methyl At least one of 1,3-pentanediol benzoic acid cinnamate, 2,2-dimethyl-1,3-pentanediol dibenzoate, 2,4-heptanediol dibenzoate, 3,5-heptanediol dibenzoate, 4-ethyl-3,5-heptanediol dibenzoate, 2-methyl-3,5-heptanediol dibenzoate, etc., more preferably at least one of 3,5-heptanediol dibenzoate, 4-ethyl-3,5-heptanediol dibenzoate, and 2,4-pentanediol dibenzoate.

[0030] According to the present invention, the titanium halide in step (3) may be the same as or different from the titanium halide in step (1), and may be various titanium compounds conventionally used in the art, for example, each of which may be a general formula of Ti(OR 10 ) m X 4-m The titanium compound shown in the general formula, R 10 It can be an alkyl group, preferably C1 to C 10 wherein X is a halogen such as Cl, Br or I, 0≤m≤3, and m is an integer. Preferably, the titanium compound is one or more of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, alkoxy titanium trihalide, dialkoxy titanium dihalide, and trialkoxy titanium halide, preferably titanium tetrachloride.

[0031] According to the present invention, in step (3), in the presence of a precipitation aid, the homogeneous solution obtained in step (2) is subjected to a third contact reaction with a titanium halide to precipitate a solid precipitate to obtain a mixture containing a solid precipitate. There is no particular limitation and the process can be carried out in accordance with the prior art. For example, the titanium halide in step (3) can be reacted alone with the homogeneous solution obtained in step (2) in the presence of a precipitation aid, or the titanium halide can be mixed with a dispersant and then reacted with the homogeneous solution obtained in step (2) in the presence of a precipitation aid.

[0032] The dispersant in step (3) may be the same as or different from the dispersant in step (1), and may be at least one of various alkane compounds, aromatic hydrocarbon compounds or mineral oils commonly used in the art that do not chemically interact with alkoxy magnesium and alcohol compounds. Specific examples may be one or more of alkanes, cycloalkanes, aromatic hydrocarbons, kerosene, vaseline oil, and white oil, preferably one or more of decane, benzene, toluene, and xylene, and more preferably toluene. In step (3), the molar amount of the dispersant should be controlled at 0.01 to 50 moles, preferably 5 to 20 moles, relative to 1 mole of alkoxy magnesium calculated as magnesium element.

[0033] According to the present invention, in step (3), relative to 1 mol of alkoxy magnesium calculated as magnesium element, the amount of the precipitation aid added can be 0.005-0.1 mol, preferably 0.01-0.1 mol, etc., for example, 0.005 mol, 0.01 mol, 0.02 mol, 0.03 mol, 0.04 mol, 0.05 mol, 0.06 mol, 0.07 mol, 0.08 mol, 0.09 mol, 0.1 mol, etc. In step (3), relative to 1 mol of alkoxy magnesium calculated as magnesium element, the molar amount of the titanium halide should be controlled to be 5-35 mol, preferably 8-25 mol, for example, 5 mol, 8 mol, 10 mol, 15 mol, 20 mol, 25 mol, 30 mol, 35 mol, etc.

[0034] According to the present invention, the conditions of the third contact reaction in step (3) include: in the presence of a precipitation aid, the uniform solution obtained in step (2) is contacted with a titanium halide at a temperature of -40°C to 0°C for 1 to 8 hours, and then the temperature is raised to 40 to 150°C; preferably, in the presence of a precipitation aid, the uniform solution obtained in step (2) is contacted with a titanium halide at a temperature of -30°C to -20°C for 1 to 5 hours, and then the temperature is raised to 50 to 110°C to obtain a mixture containing a solid precipitate.

[0035] Generally, according to the needs of practical applications, in particular, for catalyst solid components used for propylene polymerization, in order to obtain highly isotactic propylene polymers, at least one internal electron donor compound needs to be added during the preparation of the catalyst solid component. The internal electron donor compound in step (4) of the present invention can be any internal electron donor compound in the art, including but not limited to one or more of phthalate internal electron donor compounds, glycol ester compounds, diether compounds, succinate compounds and cyanosuccinate compounds.

[0036] According to the present invention, the internal electron donor compound and the precipitation aid in step (4) may be the same or different.

[0037] According to the present invention, the mass ratio of the total amount of the internal electron donor compound to the precipitation aid should be controlled at (1-8):1, preferably (3-5):1, and specifically can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, etc.

[0038] According to the present invention, in step (4), the conditions of the fourth contact reaction include a reaction temperature of 20 to 120° C., preferably 70 to 110° C.; and a reaction time of 0.5 to 6 hours, preferably 1 to 4 hours.

[0039] According to the present invention, the fifth contact reaction conditions in step (5) include a reaction temperature of 50 to 150° C., preferably 80 to 120° C., and a reaction time of 0.5 to 6 hours, preferably 1 to 4.5 hours. After the reaction is completed, the liquid in the reactant is filtered off to obtain a solid reaction product, and then the contact reaction is repeated 1 to 3 times, and after washing and drying, a titanium-containing solid catalyst component is obtained.

[0040] In step (5), the molar ratio of alkoxymagnesium to titanium halide can be 1:(3-40), preferably 1:(5-35), specifically 1:3, 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, etc.

[0041] In step (5), the titanium halide is the same as or different from the titanium halide in the aforementioned step (1), and will not be described in detail here.

[0042] The form of the titanium halide used in step (5) is not particularly limited. For example, the titanium halide in step (5) can react alone with the solid product obtained after solid-liquid separation of the suspension obtained in step (4), or the titanium halide can be mixed with a dispersant and reacted with the solid product obtained after solid-liquid separation of the suspension obtained in step (4). The types of the dispersant have been described in detail above and will not be repeated here.

[0043] The second object of the present invention is to provide a catalyst solid component obtained by the preparation method.

[0044] The third object of the present invention is to provide the use of the catalyst solid component obtained by the preparation method in an olefin polymerization catalyst system.

[0045] A fourth object of the present invention is to provide a catalyst for olefin polymerization, comprising the above-mentioned catalyst solid component.

[0046] According to the olefin polymerization catalyst system of the present invention, the catalyst system is used for the polymerization reaction of olefins represented by the general formula CH2=CHR, wherein R is hydrogen or a C1-C6 alkyl group, and the catalyst comprises the reaction product of the following substances: the catalyst solid component, an alkyl aluminum compound, and an optional external electron donor compound.

[0047] In the above-mentioned olefin polymerization catalyst, the alkyl aluminum compound can be various alkyl aluminum compounds commonly used in the field of olefin polymerization that can be used as co-catalysts for Ziegler-Natta type catalysts. In a preferred case, the alkyl aluminum compound can be a compound represented by formula (II),

[0048] AlR' n' X' 3-n' (II)

[0049] In formula (II), R' is hydrogen, C1- 20 Alkyl or C6~ 20 , X' is a halogen, and n' is an integer of 1 to 3. Specific examples of the alkyl aluminum compound may be at least one of trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, trioctylaluminum, diethyl aluminum monohydrogenate, diisobutyl aluminum monohydrogenate, diethyl aluminum monochloride, diisobutyl aluminum monochloride, sesquiethyl aluminum chloride, and ethyl aluminum dichloride.

[0050] In the present invention, the amount of the alkyl aluminum compound can be a conventional amount in the art. Generally, the molar ratio of the aluminum in the alkyl aluminum compound to the titanium in the solid component of the catalyst is (5 to 5000):1. Preferably, the molar ratio of the aluminum in the alkyl aluminum compound to the titanium in the solid component of the catalyst is (20 to 1000):1. More preferably, the molar ratio of the aluminum in the alkyl aluminum compound to the titanium in the solid component of the catalyst is (50 to 500):1.

[0051] Since only the precipitation aid in the preparation process of the olefin polymerization catalyst component is improved in the olefin polymerization catalyst of the present invention, the type and content of the external electron donor compound in the olefin polymerization catalyst of the present invention are not particularly limited. In a preferred case, the molar ratio of the aluminum in the alkyl aluminum compound to the external electron donor compound is (0.1 to 500):1, preferably (1 to 300):1, and more preferably (3 to 100:1).

[0052] In the above olefin polymerization catalyst, the external electron donor component may be an organosilicon compound represented by formula (III),

[0053] R1” m” R2” n” Si(OR3”) 4-m”-n' (III)

[0054] In formula (III), R1" and R2" are the same or different and are independently halogen, hydrogen, C1- 20 Alkyl, C3~ 20 Cycloalkyl, C6~ 20 Aryl, C1~ 20 R3" is C1~ 20 Alkyl, C3~ 20 Cycloalkyl, C6~ 20 Aryl, C1~ 20halogenated alkyl; m" and n" are respectively integers of 0 to 3, and m"+n"<4. Specific examples of the organic silicon compound include trimethylmethoxysilane, trimethylethoxysilane, trimethylphenoxytriethylmethoxysilane, triethylethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, ethylisopropyldimethoxysilane, propylisopropyldimethoxysilane, diisopropyldimethoxysilane, diisobutyldimethoxysilane, isopropylisobutyldimethoxysilane, di-tert-butyldimethoxysilane, tert-butylmethyldimethoxysilane, tert-butylethyldimethoxysilane, tert-butylpropyldimethoxysilane, tert-butylisopropyldimethoxysilane, tert-butyl, tert-Butylbutyldimethoxysilane, tert-Butylisobutyldimethoxysilane, tert-Butyl(sec-butyl)dimethoxysilane, tert-Butylpentyldimethoxysilane, tert-Butylnonyldimethoxysilane, tert-Butylhexyldimethoxysilane, tert-Butylheptyldimethoxysilane, tert-Butyloctyldimethoxysilane, tert-Butyldecyldimethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexylethyldimethoxysilane, cyclohexylpropyldimethoxysilane, cyclohexylisobutyldimethoxysilane, dicyclohexyldimethoxysilane, cyclohexyl-tert-butyldimethoxysilane, cyclopentylmethyldimethoxysilane, cyclopentylethyldimethoxysilane Oxysilane, cyclopentylpropyldimethoxysilane, cyclopentyltert-butyldimethoxysilane, dicyclopentyldimethoxysilane, cyclopentylcyclohexyldimethoxysilane, bis(2-methylcyclopentyl)dimethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, phenyltriethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, isopropyltrimethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, isobutyltrimethoxysilane, tert-butyltrimethoxysilane, sec-butyltrimethoxysilane, pentanediol trimethoxysilane, isopentyltrimethoxysilane, cyclopentyltrimethoxysilane, cyclohexyltrimethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, n-propyltrimethoxysilane, vinyltrimethoxysilane, cyclohexylmethyldimethoxysilane, tetramethoxysilane, tetraethoxysilane, tetrabutoxysilane, 2-ethylpiperidinyl-2-tert-butyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-methyldimethoxysilane, etc. These organosilicon compounds may be used alone or in combination of two or more. More preferably, the compound C as the external electron donor contains at least one of dicyclopentyldimethoxysilane, diisopropyldimethoxysilane, diisobutyldimethoxysilane, cyclohexylmethyldimethoxysilane, methyl-tert-butyldimethoxysilane and tetramethoxysilane.

[0055] The catalyst system according to the present invention is suitable for use in olefin polymerization reactions.

[0056] According to the olefin polymerization method of the present invention, the method includes contacting one or more olefins with the above-mentioned catalyst system under olefin polymerization conditions, at least one of the olefins is an olefin represented by the general formula CH2=CHR, wherein R is hydrogen or a C1-C6 alkyl group.

[0057] The olefin polymerization method of the present invention can be used for the homopolymerization of olefins, and can also be used for copolymerizing multiple olefins. At least one of the olefins is an olefin represented by the general formula CH2=CHR, wherein R is hydrogen or a C1-C6 alkyl group. Specific examples of the olefin represented by the general formula CH2=CHR include: ethylene, propylene, 1-n-butene, 1-n-pentene, 1-n-hexene, 1-n-octene and 4-methyl-1-pentene. Preferably, the α-olefin CH2=CHR is one or more of ethylene, propylene, 1-butene, 4-methyl-1-pentene and 1-hexene. More preferably, the olefin represented by the general formula CH2=CHR is propylene.

[0058] According to the method for using the solid catalyst component in olefin polymerization described in the present invention, the various components of the olefin polymerization catalyst, i.e., the solid catalyst component described in the present invention, the organic aluminum compound as a co-catalyst and the compound as an external electron donor, can be contacted before contacting the olefin monomer, which is called "pre-contact" or "pre-complexation" in the industry; or the above components can be added to the olefin monomer separately before the polymerization reaction, i.e., no "pre-contact" is performed. Preferably, the reaction of the various components of the olefin polymerization catalyst is carried out by the "pre-contact" method. The time of "pre-contact" is 0.1 to 30 minutes, preferably 1 to 10 minutes; the temperature of "pre-contact" is -20 to +80°C, preferably 10 to 50°C.

[0059] The olefin polymerization catalyst is first polymerized to a certain extent in the presence of a small amount of olefin monomer to obtain a prepolymerized catalyst, and then the prepolymerized catalyst is further contacted with the olefin monomer to react to obtain an olefin polymer. This technology is called the "prepolymerization" process in the industry, which helps to improve the polymerization activity of the catalyst and the bulk density of the polymer. According to the olefin polymerization method of the present invention, the olefin polymerization catalyst can adopt the "prepolymerization" process or not, and preferably adopts the "prepolymerization" process. The ratio of "prepolymerization" is 5 to 1000 gPP / gCat, preferably 10 to 500 gPP / gCat; the temperature of "prepolymerization" is -20 to +80°C, preferably 10 to 50°C.

[0060] According to the olefin polymerization method of the present invention, the olefin polymerization conditions may be conventional conditions in the art, and the amount of the catalyst may be the amount of various catalysts in the prior art.

[0061] The present invention uses alkoxy magnesium which is not restricted by particle shape as the initial raw material, completes the preparation of alkoxy magnesium solution by adopting a non-toxic material system, then precipitates solid components through a precipitation aid, and then loads an internal electron donor, and finally prepares a polyolefin catalyst with good particle shape and high polymerization activity. DETAILED DESCRIPTION

[0062] The following examples are given to illustrate the present invention but not to limit the present invention.

[0063] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0064] (I) Test method:

[0065] 1. Catalyst yield: catalyst yield % = mass of catalyst obtained / mass of magnesium chloride corresponding to the number of moles of alkoxymagnesium used × 100%.

[0066] 2. Titanium content in catalyst: tested by 721 spectrophotometer.

[0067] 3. The internal electron donor content in the olefin polymerization catalyst component is determined using a Waters 600E liquid chromatograph or an Agilent 7890 gas chromatograph.

[0068] 4. Determination of polymer melt index: Determined according to GB / T3682-2000.

[0069] 5. The isotacticity of polymers is determined by the heptane extraction method: 2 grams of dry polymer sample is placed in an extractor and extracted with boiling heptane for 6 hours. The residue is dried to constant weight, and the ratio of the polymer weight (g) to 2 (g) is the isotacticity.

[0070] 6. Activity calculation: Catalyst activity = (mass of prepared polyolefin) / (mass of catalyst solid component) g / g

[0071] 7. Bulk density determination: The prepared polymer powder is allowed to fall freely from a height of 10 cm into a 100 ml container in a funnel. The weight of the polymer powder in the container is weighed as M g. The bulk density of the polymer is M / 100 g / cm 3 .

[0072] (II) Preparation and polymerization of catalyst components:

[0073] Example 1

[0074] Preparation of catalyst component A1:

[0075] In a reactor that has been repeatedly replaced with high-purity nitrogen, 5.7g of diethoxymagnesium, 100ml of toluene, 1mL of ethanol, and 2.75ml of titanium tetrachloride were added in sequence, and the mixture was stirred at 200rpm and 80°C for 4 hours to obtain a stable and uniform magnesium compound slurry; after cooling to 55°C, 4ml of epichlorohydrin and 12.5ml of tributyl phosphate were added, and the mixture was reacted for 1 hour to obtain a magnesium compound solution. 0.7ml of 3,5-heptanediol dibenzoate was added, stirred for 60 minutes, and cooled to room temperature.

[0076] The uniform solution prepared above was added into a reactor fully replaced with nitrogen, and the temperature was lowered to -25°C. 60 ml of titanium tetrachloride was added to allow them to fully contact at low temperature. After 5 hours, the temperature was raised to 110°C. Solid precipitates were precipitated during the heating process. 2.7 g of diisobutyl phthalate was added and the reaction was carried out for 1 hour. After the reaction was completed, the liquid was filtered out; 72 ml of toluene and 48 ml of titanium tetrachloride were added and the mixture was contacted at 110°C for 0.5 hour; this operation was repeated once more, and the mixture was washed 5 times with 120 ml of hexane and dried to obtain a titanium-containing solid catalyst component A1.

[0077] The analysis results of the titanium content, precipitation aid content and electron donor content of the catalyst solid component A1 are shown in Table 1.

[0078] Catalyst polymerization:

[0079] Polymerization evaluation: In a 5-liter autoclave, after sufficient replacement of gaseous propylene, add 5 ml of triethylaluminum hexane solution (the concentration of triethylaluminum is 0.5 mmol / ml), 1 ml of cyclohexylmethyldimethoxysilane (CHMMS) hexane solution (the concentration of CHMMS is 0.1 mmol / ml), 10 ml of anhydrous hexane and 10 mg of solid catalyst component at room temperature. Close the autoclave, introduce 0.18 mol of hydrogen and 1.15 kg of liquid propylene; raise the temperature to 70°C under stirring. Polymerize at 70°C for a certain period of time. After the reaction is completed, stop stirring, remove the unpolymerized propylene monomer, collect the polymer, vacuum dry, weigh and calculate the catalyst activity.

[0080] The polymerization activity of the catalyst system containing the catalyst solid component A1 in propylene polymerization and the property parameters of the polymer are shown in Table 1.

[0081] Example 2

[0082] Preparation of catalyst component A2:

[0083] The preparation method of the catalyst solid component A2 is the same as the preparation method of A1 in Example 1, except that 2.7 g of diisobutyl phthalate is replaced by 2.7 g of di-n-butyl phthalate.

[0084] The results of the titanium content, the precipitation aid content and the internal electron donor content of the catalyst solid component A2 are shown in Table 1.

[0085] Catalyst polymerization:

[0086] Using A2, polymerization was carried out according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A2 in propylene polymerization and the property parameters of the polymer are shown in Table 1.

[0087] Example 3

[0088] Catalyst component A3 preparation:

[0089] The preparation method of the catalyst solid component A3 is the same as the preparation method of A1 in Example 1, except that 0.7 ml of 3,5-heptanediol dibenzoate is replaced by 0.7 ml of 2,4-pentanediol dibenzoate.

[0090] The results of the titanium content, the precipitation aid content and the internal electron donor content of the catalyst solid component A3 are shown in Table 1.

[0091] Olefin polymerization:

[0092] Using A3, polymerization was carried out according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A3 in propylene polymerization and the property parameters of the polymer are shown in Table 1.

[0093] Example 4

[0094] Preparation of catalyst solid component A4

[0095] The preparation method of the catalyst solid component A4 is the same as the preparation method of A1 in Example 1, except that 0.7 ml of 3,5-heptanediol dibenzoate is replaced by 0.5 ml of 3,5-heptanediol dibenzoate.

[0096] The results of the titanium content, the precipitation aid content and the internal electron donor content of the catalyst solid component A4 are shown in Table 1.

[0097] Olefin polymerization:

[0098] Using A4, polymerization was carried out according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A4 in propylene polymerization and the property parameters of the polymer are shown in Table 1.

[0099] Example 5

[0100] Catalyst component A5 preparation:

[0101] The preparation method of the catalyst solid component A5 is the same as the preparation method of A1 in Example 1, except that 0.7 ml of 3,5-heptanediol dibenzoate is replaced by 0.5 ml of 2,4-pentanediol dibenzoate.

[0102] The results of the titanium content, the precipitation aid content and the internal electron donor content of the catalyst solid component A5 are shown in Table 1.

[0103] Catalyst polymerization:

[0104] Using A5, propylene polymerization was carried out according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A5 in propylene polymerization and the property parameters of the polymer are shown in Table 1.

[0105] Example 6

[0106] Catalyst component A6 preparation:

[0107] The preparation method of the catalyst solid component A6 is the same as the preparation method of A1 in Example 1, except that the internal electron donor is replaced by 2.3 g of 9,9-di(methoxymethyl)fluorene.

[0108] The results of the titanium content, the precipitation aid content and the internal electron donor content of the catalyst solid component A6 are shown in Table 1.

[0109] Olefin polymerization:

[0110] Using A6, propylene polymerization was carried out according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A6 in propylene polymerization and the property parameters of the polymer are shown in Table 1.

[0111] Example 7

[0112] Catalyst component A7 preparation:

[0113] The preparation method of the catalyst solid component A7 is the same as the preparation method of A1 in Example 1, except that the internal electron donor is replaced by 2.3 g of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane.

[0114] The results of the titanium content, the precipitation aid content and the internal electron donor content of the catalyst solid component A7 are shown in Table 1.

[0115] Olefin polymerization:

[0116] Using A7, propylene polymerization was carried out according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A7 in propylene polymerization and the property parameters of the polymer are shown in Table 1.

[0117] Example 8

[0118] Preparation of catalyst solid component A8

[0119] The preparation method of the catalyst solid component A8 is the same as the preparation method of A1 in Example 1, except that the internal electron donor is replaced by 3.1 g of 3,5-heptanediol dibenzoate.

[0120] The results of the titanium content, the precipitation aid content and the internal electron donor content of the catalyst solid component A8 are shown in Table 1.

[0121] Catalyst polymerization:

[0122] Using A8, propylene polymerization was carried out according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A8 in propylene polymerization and the property parameters of the polymer are shown in Table 1.

[0123] Example 9

[0124] Preparation of catalyst solid component A9

[0125] The preparation method of the catalyst solid component A9 is the same as the preparation method of A1 in Example 1, except that the internal electron donor is replaced by 3.1 g of 2,4-pentanediol dibenzoate.

[0126] The results of the titanium content, the precipitation aid content and the internal electron donor content of the catalyst solid component A9 are shown in Table 1.

[0127] Catalyst polymerization:

[0128] Using A9, propylene polymerization was carried out according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A9 in propylene polymerization and the property parameters of the polymer are shown in Table 1.

[0129] Example 10

[0130] Preparation of catalyst solid component A10

[0131] The preparation method of the catalyst solid component A10 is the same as the preparation method of A1 in Example 1, except that the internal electron donor is replaced by 5 mmol of diethyl 2,3-diisopropylsuccinate.

[0132] The results of the titanium content, the precipitation aid content, and the internal electron donor content of the catalyst solid component A10 are shown in Table 1.

[0133] Catalyst polymerization:

[0134] Using A10, propylene polymerization was carried out according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A10 in propylene polymerization and the performance parameters of the polymer are shown in Table 1.

[0135] Embodiment 11

[0136] Preparation of catalyst solid component A11

[0137] The preparation method of the catalyst solid component A11 is the same as the preparation method of A1 in Example 1, except that the internal electron donor is replaced by 2 g of diethyl 2-cyano-2,3-diisopropylsuccinate.

[0138] The results of the titanium content, the precipitation aid content and the internal electron donor content of the catalyst solid component A11 are shown in Table 1.

[0139] Catalyst polymerization:

[0140] Using A11, propylene polymerization was carried out according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A11 in propylene polymerization and the performance parameters of the polymer are shown in Table 1.

[0141] Example 12

[0142] Preparation of catalyst solid component A12

[0143] The preparation method of the catalyst solid component A12 is the same as the preparation method of A1 in Example 1, except that 4 ml of epichlorohydrin and 12.5 ml of tributyl phosphate are replaced by 8 ml of epichlorohydrin and 10 ml of tributyl phosphate.

[0144] The results of the titanium content, the precipitation aid content and the internal electron donor content of the catalyst solid component A12 are shown in Table 1.

[0145] Olefin polymerization:

[0146] Using A12, polymerization was carried out according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A12 in propylene polymerization and the performance parameters of the polymer are shown in Table 1.

[0147] Embodiment 13

[0148] Preparation of catalyst solid component A13

[0149] The preparation method of the catalyst solid component A13 is the same as the preparation method of A1 in Example 1, except that 1 ml of ethanol is replaced by 2 ml of ethanol.

[0150] The titanium content and internal electron donor content of the catalyst solid component A13 are shown in Table 1.

[0151] Olefin polymerization:

[0152] A13 was used to carry out polymerization according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A13 in propylene polymerization and the performance parameters of the polymer are shown in Table 1.

[0153] Embodiment 14

[0154] Preparation of catalyst solid component A14

[0155] The preparation method of the catalyst solid component A14 is the same as the preparation method of A1 in Example 1, except that 2.75 ml of titanium tetrachloride is replaced by 3 ml of titanium tetrachloride.

[0156] The titanium content and internal electron donor content of the catalyst solid component A14 are shown in Table 1.

[0157] Olefin polymerization:

[0158] Using A14, polymerization was carried out according to the polymerization method of Example 1. The polymerization activity of the catalyst system containing the catalyst solid component A14 in propylene polymerization and the property parameters of the polymer are shown in Table 1.

[0159] Comparative Example 1

[0160] Preparation of catalyst solid component D1

[0161] The catalyst solid component D1 was prepared according to Example 1 except that 1 ml of ethanol was not added.

[0162] The results of the titanium content, the precipitation aid content, and the internal electron donor content of the catalyst solid component D1 are shown in Table 1.

[0163] Using D1, propylene polymerization was carried out according to the method of Example 1. The polymerization activity of the catalyst system prepared by the catalyst component in propylene polymerization and the performance parameters of the prepared propylene polymer are shown in Table 1.

[0164] Comparative Example 2

[0165] Preparation of catalyst solid component D2

[0166] Catalyst solid component D2 was prepared as in Example 1, except that 2.75 ml of titanium tetrachloride was replaced by 2 ml of titanium tetrachloride.

[0167] The results of the titanium content, the precipitation aid content, and the internal electron donor content of the catalyst solid component D2 are shown in Table 1.

[0168] Using D2, propylene polymerization was carried out according to the method of Example 1. The polymerization activity of the catalyst system prepared by the catalyst component in propylene polymerization and the performance parameters of the prepared propylene polymer are shown in Table 1.

[0169] Comparative Example 3

[0170] Preparation of catalyst solid component D3

[0171] The catalyst solid component D3 was prepared according to Example 1, except that the reaction time in step 1 was adjusted from 4 hours to 0.5 hours.

[0172] The results of the titanium content, the precipitation aid content and the internal electron donor content of the catalyst solid component D3 are shown in Table 1.

[0173] Using D3, propylene polymerization was carried out according to the method of Example 1. The polymerization activity of the catalyst system prepared by the catalyst component in propylene polymerization and the performance parameters of the prepared propylene polymer are shown in Table 1.

[0174] (III) Test results:

[0175] Table 1 Catalyst component results

[0176]

[0177] It can be seen from the data in the table that the catalyst prepared by the present invention has good performance in terms of composition and polymerization performance.

[0178] Compared with Comparative Example 1 (no ethanol added in step 1), Comparative Example 2 (insufficient amount of titanium tetrachloride in step 1) and Comparative Example 3 (insufficient reaction time in step 1), the solid catalyst component prepared in the embodiment has the characteristics of high yield and high activity. In the comparative examples, no addition of ethanol, insufficient titanium tetrachloride and insufficient reaction time in step 1 will lead to insufficient dissolution process in step (2), thereby greatly reducing the yield of the precipitated solid component and affecting the overall performance of the catalyst.

[0179] The results of Example (6) and Example (7) show that the catalyst activity is significantly higher than that of other catalysts, indicating that diol ester is a precipitation aid and compounding with a diether internal electron donor can significantly improve the catalyst activity of the system.

Claims

1. A method for preparing a solid component of a catalyst for olefin polymerization, comprising the following steps: (1) subjecting alkoxymagnesium, an alcohol compound and a titanium halide to a first contact reaction in the presence of a dispersant to form a uniformly dispersed slurry; (2) adding a solvent system of an organic epoxy compound and an organic phosphorus compound to the uniform slurry obtained in step (1) to carry out a second contact reaction to form a uniform solution; (3) adding a titanium halide to the uniform solution obtained in step (2) in the presence of a precipitation aid to carry out a third contact reaction to precipitate a solid precipitate mixture containing magnesium / titanium; (4) subjecting the mixture obtained in step (3) to a fourth contact reaction with an internal electron donor compound to obtain a suspension; (5) separating the suspension obtained in step (4) into solid and liquid, and subjecting the solid component obtained by the solid-liquid separation to a fifth contact reaction with a titanium halide to obtain the catalyst solid component.

2. The preparation method according to claim 1, characterized in that In step (1): The structural formula of the magnesium alkoxide is Mg(OR9)2, R9 is C1~C 10 Preferably, the alkoxy magnesium is at least one of ethoxy magnesium, propoxy magnesium, butoxy magnesium, and phenoxy magnesium; The alcohol compound is C1~C 10 At least one of the linear or branched alcohols; and / or, The general formula of the titanium halide is Ti(OR 10 ) m X 4-m The titanium compound shown, wherein R 10 is an alkyl group, X is a halogen, 0≤m≤3, m is an integer, and is preferably at least one of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, alkoxy titanium trihalide, dialkoxy titanium dihalide, and trialkoxy titanium halide; The dispersant is at least one of alkane compounds, aromatic hydrocarbon compounds or mineral oils that do not chemically interact with alkoxy magnesium and alcohol compounds, preferably at least one of alkanes, cycloalkanes, aromatic hydrocarbons, kerosene, vaseline oil, and white oil, and more preferably at least one of decane, benzene, toluene, and xylene.

3. The preparation method according to claim 1, characterized in that In step (1): The molar ratio of the alcohol compound to the alkoxy magnesium is (0.01-2):1, preferably (0.02-0.8):1; and / or, The molar ratio of the titanium halide to the alkoxymagnesium is (0.45-1):1, preferably (0.5-0.8):1; and / or, The molar ratio of the dispersant to the magnesium alkoxide is (5-50):1, preferably (5-20):1; and / or, The first contact reaction conditions include a temperature of 10 to 150° C., preferably 60 to 120° C., and a time of 1 to 10 hours, preferably 2 to 6 hours.

4. The preparation method according to claim 1, characterized in that In step (2): The organic epoxy compound is selected from at least one of oxides, glycidyl ethers, and internal ethers of C2-C8 aliphatic monoolefins, dienes, or halogenated aliphatic olefins or dienes, preferably at least one of ethylene oxide, propylene oxide, butylene oxide, butadiene oxide, butadiene dioxide, epichlorohydrin, methyl glycidyl ether, and diglycidyl ether; and / or, The organophosphorus compound is a hydrocarbon ester of orthophosphoric acid or phosphorous acid, or a halogenated hydrocarbon ester of orthophosphoric acid or phosphorous acid, preferably at least one of trimethyl orthophosphate, triethyl orthophosphate, tributyl orthophosphate, triphenyl orthophosphate, trimethyl phosphite, triethyl phosphite, tributyl phosphite, and benzyl phosphite.

5. The preparation method according to claim 1, characterized in that In step (2): With respect to 1 mol of magnesium alkoxide calculated as magnesium element, the organic epoxy compound is 0.2 to 10 mol, preferably 0.5 to 4 mol; the organic phosphorus compound is 0.1 to 3 mol, preferably 0.3 to 1 mol; and / or, The second contact reaction conditions include a temperature of 10 to 150° C., preferably 50 to 140° C., and a time of 0.1 to 10 hours, preferably 0.5 to 6 hours.

6. The preparation method according to claim 1, characterized in that In step (3): The precipitation aid is a diol ester compound represented by formula (I): In formula (I), R1 to R2 are the same or different and are each independently a substituted or unsubstituted linear C1 to C 20 Alkyl, substituted or unsubstituted branched C3~C 20 Alkyl, substituted or unsubstituted C3~C 20 Cycloalkyl, substituted or unsubstituted C6~C 20 Aryl, substituted or unsubstituted C7~C 20 Alkyl, substituted or unsubstituted C7~C 20 Arylalkyl, substituted or unsubstituted C2~C 10 Alkenyl, substituted or unsubstituted C 10 ~C 20 R3 to R8 are the same or different and are independently hydrogen, halogen, substituted or unsubstituted straight-chain C1 to C 20 Alkyl, substituted or unsubstituted branched C3~C 20 Alkyl, substituted or unsubstituted C3~C 20 Cycloalkyl, substituted or unsubstituted C6~C 20 Aryl, substituted or unsubstituted C7~C 20 Alkyl, substituted or unsubstituted C7~C 20 Arylalkyl, substituted or unsubstituted C2~C 10 Alkenyl, substituted or unsubstituted C 10 ~C 20 condensed ring aromatic group; or at least one of R3 to R6 forms a ring with at least one of R7 to R8; preferably, the precipitation aid is 2-ethyl-1,3-propylene glycol dibenzoate, 2-propyl-1,3-propylene glycol dibenzoate, 2-isopropyl-2-isopentyl-1,3-propylene glycol dibenzoate, 1,3-butylene glycol dimethyl benzoate, 2-methyl-1,3-butylene glycol dichlorobenzoate, 2,3-dimethyl- At least one of 1,3-butanediol dibenzoate, 1,3-pentanediol dipivalate, 2,4-pentanediol dibenzoate, 2-methyl-1,3-pentanediol benzoic acid cinnamate, 2,2-dimethyl-1,3-pentanediol dibenzoate, 2,4-heptanediol dibenzoate, 3,5-heptanediol dibenzoate, 4-ethyl-3,5-heptanediol dibenzoate, and 2-methyl-3,5-heptanediol dibenzoate.

7. The preparation method according to claim 1, characterized in that In step (3): Relative to 1 mol of alkoxymagnesium calculated as magnesium element, the precipitation aid is 0.005 to 0.1 mol, preferably 0.01 to 0.1 mol; the titanium halide is 5 to 35 mol, preferably 8 to 25 mol; and / or, The third contact reaction conditions include contacting at a temperature of -40°C to 0°C for 1 to 8 hours, and then heating to 40 to 150°C; preferably, contacting at a temperature of -30°C to -20°C for 1 to 5 hours, and then heating to 50 to 110°C.

8. The preparation method according to claim 1, characterized in that In step (4): The internal electron donor compound is selected from at least one of phthalate compounds, glycol ester compounds, diether compounds, succinate compounds, and cyanosuccinate compounds; and / or, The mass ratio of the internal electron donor compound to the precipitation aid is (1-8):1, preferably (3-5):1; and / or, The fourth contact reaction conditions include a reaction temperature of 20 to 120° C., preferably 70 to 110° C.; and a reaction time of 0.5 to 6 hours, preferably 1 to 4 hours.

9. The preparation method according to claim 1, characterized in that In step (5): The molar ratio of the magnesium alkoxide to the titanium halide is 1:(3-40), preferably 1:(5-35); and / or, The fifth contact reaction conditions include a reaction temperature of 50 to 150° C., preferably 80 to 120° C.; and a reaction time of 0.5 to 6 hours, preferably 1 to 4.5 hours.

10. The catalyst solid component obtained according to the preparation method according to any one of claims 1 to 9.

11. Use of the catalyst solid component obtained by the preparation method according to any one of claims 1 to 9 in an olefin polymerization catalyst system.

12. A catalyst for olefin polymerization, comprising a reaction product of a catalyst solid component obtained by the preparation method according to any one of claims 1 to 9, an alkyl aluminum compound and an optional external electron donor compound.

13. The catalyst according to claim 12, characterized in that: The alkyl aluminum compound is a compound represented by formula (II), AlR' n' X' 3-n' (II), In formula (II), R' is hydrogen, C1- 20 Alkyl or C6~ 20 aryl, X' is halogen, n' is an integer from 1 to 3; and / or, The external electron donor compound is an organosilicon compound represented by formula (III), R1” m” R2” n” Si(OR3”) 4-m”-n” (III), In formula (III), R1" and R2" are the same or different and are independently halogen, hydrogen, C1- 20 Alkyl, C3~ 20 Cycloalkyl, C6~ 20 Aryl, C1~ 20 R3" is C1~ 20 Alkyl, C3~ 20 Cycloalkyl, C6~ 20 Aryl, C1~ 20 m" and n" are integers of 0 to 3 respectively, and m"+n"<4.

14. The catalyst according to claim 13, characterized in that: The molar ratio of aluminum in the alkyl aluminum compound to titanium in the solid component of the catalyst is (5-5000):1, preferably (20-1000):1; and / or, The molar ratio of aluminum in the alkyl aluminum compound to the external electron donor compound is (0.1-500):1, preferably (1-300):1.

Citation Information

Patent Citations

  • Preparation method of catalyst component for polymerization reaction of olefins and catalyst thereof

    CN101864009A

  • Catalyst component for olefin polymerization and catalyst thereof

    CN101885789A

  • Catalyst component for preparing fiber polyolefin, preparation method and application thereof, catalyst system, application of catalyst system, and olefin polymerization method

    CN106317275A

  • Alkoxy magnesium carrier, Ziegler-Natta catalyst, catalyst for olefin polymerization and preparation method and application thereof

    CN114456281A

  • Solid catalyst component for polymerizing olefins, catalyst for polymerizing olefins, and production method for polymerized olefins