Continuous production method and equipment for high-temperature-resistant polyamide

Through the process of salt formation-low-pressure prepolymerization-high-pressure prepolymerization-flash evaporation-final polymerization, the problem of degradation and high energy consumption of high-temperature-resistant polyamide in high-temperature environments is solved, and the production of high-quality products is achieved, which is suitable for a variety of applications. Application scenarios expand the application scope of the product.

CN118812840APending Publication Date: 2024-10-22CATHAY BIOTECH INC +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310410026.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing continuous polymerization process of high-temperature-resistant polyamide has problems such as high-temperature degradation, high energy consumption, and poor product performance. In particular, it is difficult to maintain the melting point and appearance quality of the material in high-temperature environments.

Method used

Adopting a continuous production method of salt formation-low pressure prepolymerization-high pressure prepolymerization-flash evaporation-final polymerization, the degree of polymerization is gradually increased through low-pressure and high-pressure prepolymerization, the moisture content is reduced, high-temperature degradation is avoided, and the process is carried out at a temperature higher than the melting point Flash evaporation and final polymerization to form high quality, high temperature resistant polyamide.

Benefits of technology

It simplifies the process flow, reduces energy consumption, avoids high-temperature degradation of polyamide, improves the yellow index, molecular weight distribution and crystallization ability of the product, is suitable for a variety of application scenarios, and expands the production and application scope of high-temperature resistant polyamide products. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812840A_ABST
    Figure CN118812840A_ABST
Patent Text Reader

Abstract

The invention discloses a continuous production method and equipment for high-temperature-resistant polyamide. The continuous production method comprises the steps of salifying, low-pressure prepolymerization, high-pressure prepolymerization, flash evaporation and final polymerization. By optimizing the existing continuous polymerization process, high-temperature degradation of polyamide is effectively avoided, and the obtained high-temperature-resistant polyamide resin slice is lower in yellow index, narrower in molecular weight distribution and more uniform in product distribution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention specifically relates to a continuous production method and equipment for high temperature resistant polyamide. Background Art

[0002] High temperature polyamide (HTPA) is a type of polymer material with a melting point above 280°C and can be used in an environment above 200°C for a long time. It is widely used in electronic appliances, automobiles, military industry, aviation and other industries. Currently, the commercialized HTPA includes: PA46, 6T, 9T and 10T. HTPA is mainly produced by prepolymerization-solid phase viscosity enhancement method and intermittent high pressure melt polymerization method. The prepolymerization-solid phase viscosity enhancement method requires large investment, large equipment and long production cycle; the intermittent high pressure melt polymerization method has high reaction temperature, poor batch reproducibility, low production efficiency, high energy consumption, easy to produce gel and black spots, and affects product performance and appearance. Polyamide with 1,5-pentanediamine as raw material has excellent melt fluidity, which provides the basic conditions for the continuous polymerization of HTPA.

[0003] At present, the continuous polymerization of polyamide is mainly used for the production of PA66. The process mainly includes: salt formation → concentration → high pressure precondensation → flash evaporation → prepolymerization → final polymerization. When the above process is directly used for the continuous polymerization of HTPA, on the one hand, since the flash evaporation, prepolymerization and final polymerization processes all need to be carried out at a temperature higher than the melting point of HTPA, the long high temperature residence time will cause HTPA to degrade, and then the product appearance will turn yellow and the performance will deteriorate. On the other hand, since the concentration of the polyamide salt solution (PA66) is about 50%, a large amount of water needs to be discharged during the concentration and prepolymerization process, which consumes a lot of energy.

[0004] Therefore, the existing continuous polymerization process is not suitable for the continuous preparation of high temperature resistant polyamide. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a continuous production method and equipment for high temperature resistant polyamide.

[0006] The present invention solves the above technical problems through the following technical solutions:

[0007] The present invention provides a continuous production method of high temperature resistant polyamide, comprising the following steps:

[0008] S1, mixing the polymerization monomer of the high temperature resistant polyamide with water to prepare a salt solution;

[0009] S2, prepolymerizing the salt solution under low pressure to obtain a first polyamide melt;

[0010] S3, subjecting the first polyamide melt to high pressure prepolymerization to obtain a second polyamide melt;

[0011] S4, flashing and final polymerizing the second polyamide melt to obtain a high temperature resistant polyamide;

[0012] The polymer monomers of the high temperature resistant polyamide include diamines and dibasic acids, wherein the diamines are selected from one or more terminal diamines having carbon atoms of 1 to 15; the dibasic acids include dibasic acid A1 and dibasic acid A2, wherein the dibasic acid A1 is selected from aromatic dicarboxylic acids and their derivatives, and the dibasic acid A2 is selected from one or more aliphatic dicarboxylic acids having carbon atoms of 4 to 18.

[0013] In one embodiment of the present invention, the molar ratio of the diamine to the dibasic acid may be conventional in the art, preferably (0.9-1.2):1, more preferably (1-1.08):1, for example 1.01:1, 1.02:1, 1.03:1, 1.04:1, 1.06:1 or 1.07:1.

[0014] In one embodiment of the present invention, the molar ratio of the dibasic acid A1 to the dibasic acid A2 is (0.5-4):1.

[0015] In one embodiment of the present invention, the diamine includes one or more of 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine and 1,14-tetradecanediamine; preferably 1,5-pentanediamine, 1,6-hexanediamine, 1,10-decanediamine or 1,12-dodecanediamine.

[0016] In one embodiment of the present invention, the dibasic acid A1 includes terephthalic acid and its derivatives and / or isophthalic acid and its derivatives, preferably terephthalic acid.

[0017] In one embodiment of the present invention, the dibasic acid A2 includes one or more of adipic acid, 1,8-octanedioic acid, 1,10-decanedioic acid, 1,11-undecanedioic acid, 1,12-dodecanedioic acid, 1,13-tridecanedioic acid, 1,14-tetradecanedioic acid and 1,16-hexadecanedioic acid; preferably adipic acid, 1,10-decanedioic acid or 1,12-dodecanedioic acid.

[0018] In one embodiment of the present invention, in step S1, the temperature at which the polymerization monomer of the high temperature resistant polyamide is mixed with water is 70-170°C, more preferably 90-165°C.

[0019] In one embodiment of the present invention, in step S1, the concentration of the salt solution is 40-80wt%, more preferably 45-75wt%, such as 50wt%, 55wt%, 60wt%, 65wt%, 70wt%. The present invention uses a high concentration of salt solution to reduce the water content therein, thereby reducing the energy consumption required to discharge the water during the concentration and prepolymerization process.

[0020] In one embodiment of the present invention, in step S1, the pH value of the salt solution is 7.2-9.8, preferably 7.35-9.65. The pH value is a parameter reflecting the ratio of the dibasic acid to the diamine. To facilitate comparison with the sample parameters, the pH values ​​of the polyamide salt solution of the present invention are all values ​​measured when the polyamide salt solution is diluted to 10% with water.

[0021] In one embodiment of the present invention, the method comprises adding an auxiliary agent in step S1, wherein the amount of the auxiliary agent added is 500-7000 ppm of the total weight of the dibasic acid and the diamine. The auxiliary agent may be any one or a combination of catalysts, antioxidants, heat stabilizers, weathering agents, pigments, gloss enhancers, dyes, crystal nucleating agents, matting agents, plasticizers, antistatic agents, flame retardants, metals and metal salts.

[0022] In one embodiment of the present invention, in step S2, the low-pressure prepolymerization includes low-pressure prepolymerization 1 and low-pressure prepolymerization 2.

[0023] In the present invention, the low-pressure prepolymerization 1 is carried out at a relatively low pressure and a relatively low temperature to form a high-temperature resistant polyamide melt with a relatively low degree of polymerization. The low-pressure prepolymerization 2 is carried out at a certain pressure and a relatively low temperature to form a high-temperature resistant polyamide melt with a certain degree of polymerization.

[0024] In one specific embodiment of the present invention, the temperature of the low-pressure prepolymerization 1 is below 180-215°C.

[0025] In a specific embodiment of the present invention, the pressure of the low-pressure prepolymerization 1 is 0.5-1.1 MPa, more preferably 0.8-1.1 MPa.

[0026] In one specific embodiment of the present invention, the time of the low-pressure prepolymerization 1 is 30-120 min.

[0027] In one specific embodiment of the present invention, the temperature of the low-pressure prepolymerization 2 is below 215-235°C.

[0028] In a specific embodiment of the present invention, the pressure of the low-pressure prepolymerization 2 is 1.1-1.5 MPa.

[0029] In one specific embodiment of the present invention, the time of the low-pressure prepolymerization 2 is 40-90 minutes.

[0030] In a preferred embodiment of the present invention, the temperature of the low-pressure prepolymerization 2 is greater than the temperature of the low-pressure prepolymerization 1.

[0031] In a preferred embodiment of the present invention, the pressure of the low-pressure prepolymerization 2 is greater than the pressure of the low-pressure prepolymerization 1.

[0032] The high temperature resistant polyamide melt after low pressure prepolymerization has a low polymerization degree and a high water content, and is further polymerized under high pressure at a relatively high temperature and pressure, and the water is gradually removed to form a high temperature resistant polyamide melt with a certain polymerization degree.

[0033] In one embodiment of the present invention, in step S3, the pressure of the high-pressure prepolymerization is below 3.2 MPa, preferably 1.7-2.5 MPa.

[0034] In one embodiment of the present invention, in step S3, the time of the high pressure prepolymerization is 60-420 min, preferably 100-400 min.

[0035] In one embodiment of the present invention, in step S3, the mass percentage content of the second polyamide melt obtained is 85-95%.

[0036] In one embodiment of the present invention, in step S3, the temperature of the high pressure prepolymerization is 240-310°C.

[0037] In a preferred embodiment of the present invention, in step S3, the temperature of the high pressure prepolymerization is controlled in stages, preferably in 2-6 stages. The inventors of the present invention have found in their research that too many stages make the temperature difficult to control, which is not conducive to the continuous polymerization reaction.

[0038] In a preferred embodiment of the present invention, the temperature of the latter stage is controlled to be greater than or equal to the temperature of the former stage.

[0039] In a preferred embodiment of the present invention, the temperature difference between the latter stage and the former stage is controlled to be 0-50°C, preferably 2-20°C.

[0040] In a preferred embodiment of the present invention, the temperature of the first stage is controlled to be 240-255°C.

[0041] In a preferred embodiment of the present invention, the temperature of the last stage is controlled to be 280-310°C.

[0042] In one specific embodiment of the present invention, when the high pressure prepolymerization temperature is controlled in two stages, the temperature of the first stage is 240-255°C, and the temperature of the second stage is 280-310°C.

[0043] In one specific embodiment of the present invention, when the high pressure prepolymerization temperature is controlled in three stages, the temperature of the first stage is 240-255°C, the temperature of the second stage is 260-275°C, and the temperature of the third stage is 280-310°C.

[0044] In a specific embodiment of the present invention, when the high pressure prepolymerization temperature is controlled in 4 stages, the temperature of the first stage is 240-255°C, the temperature of the second stage is 250-260°C, the temperature of the third stage is 255-275°C, and the temperature of the fourth stage is 280-310°C.

[0045] In a specific embodiment of the present invention, when the high pressure prepolymerization temperature is controlled in 5 stages, the temperature of the first stage is 240-255°C, the temperature of the second stage is 250-265°C, the temperature of the third stage is 260-270°C, the temperature of the fourth stage is 265-280°C, and the temperature of the fifth stage is 280-310°C.

[0046] In a specific embodiment of the present invention, when the high-pressure prepolymerization temperature is controlled in 6 stages, the temperature of the first stage is 240-255°C, the temperature of the second stage is 250-265°C, the temperature of the third stage is 260-270°C, the temperature of the fourth stage is 265-275°C, the temperature of the fifth stage is 270-285°C, and the temperature of the sixth stage is 280-310°C.

[0047] In the present invention, the high temperature resistant polyamide melt after high pressure prepolymerization is flash evaporated at a temperature higher than the melting point to remove most of the water and obtain a melt with a lower water content.

[0048] In one embodiment of the present invention, in step S4, the flash evaporation temperature is 290-340°C.

[0049] In one embodiment of the present invention, in step S4, the material pressure after flash evaporation is 0-50 KPa.

[0050] In one embodiment of the present invention, in step S4, the material temperature after flash evaporation is 290-320°C.

[0051] In the present invention, the melt with a lower water content is further polymerized under a certain negative pressure and temperature to obtain a high temperature resistant polyamide with a higher degree of polymerization.

[0052] In one embodiment of the present invention, in step S4, the final polymerization temperature is 290-340°C, preferably 295-330°C.

[0053] In one embodiment of the present invention, in step S4, the final polymerization is carried out under normal pressure or vacuum conditions.

[0054] Preferably, inert gas protection is used when final polymerization is carried out under normal pressure.

[0055] Preferably, the final polymerization pressure under vacuum conditions is -0.095 to 0 MPa, more preferably -0.09 to 0 MPa.

[0056] In one embodiment of the present invention, the method further comprises step S5, that is, performing underwater pelletizing on the high temperature resistant polyamide obtained in step S4 to obtain high temperature resistant polyamide resin slices. Furthermore, the temperature of pelletizing water is controlled to be 55-80°C.

[0057] The present invention also provides a continuous production device for high temperature resistant polyamide, which comprises a salt-forming reaction device, a low-pressure prepolymerization reaction device, a high-pressure prepolymerization reaction device, a flash evaporation device and a final polymerization reaction device connected in sequence;

[0058] The salt-forming reaction device comprises a salt-forming reaction kettle, which is used to mix the polymerized monomer of the high-temperature resistant polyamide with water to perform a salt-forming reaction to obtain a salt solution;

[0059] The low-pressure prepolymerization reaction device comprises a first low-pressure prepolymerization reactor and a second low-pressure prepolymerization reactor; the first low-pressure prepolymerization reactor is used to carry out a first low-pressure prepolymerization reaction on the salt solution; the second low-pressure prepolymerization reactor is used to carry out a second low-pressure prepolymerization reaction on the reaction product of the first low-pressure prepolymerization reaction to obtain a first polyamide melt;

[0060] The high-pressure prepolymerization reaction device comprises at least two high-pressure prepolymerization reactors connected in series, preferably 2-6 high-pressure prepolymerization reactors connected in series, and the high-pressure prepolymerization reactor is used to perform a high-pressure prepolymerization reaction on the first polyamide melt to obtain a second polyamide melt;

[0061] The flash evaporation device comprises a flash evaporator for flash evaporating and dehydrating the second polyamide melt;

[0062] The final polymerization reaction device comprises a post-polymerization reactor, which is used for further polymerizing the reaction product after the flash evaporation.

[0063] In one embodiment of the present invention, the continuous production equipment further comprises a pelletizing device connected to the final polymerization reaction device, for underwater pelletizing the further polymerized product to obtain high temperature resistant polyamide resin chips.

[0064] The present invention also provides a continuous production method of high temperature resistant polyamide, which is carried out in the continuous production equipment as described above.

[0065] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention. The reagents and raw materials used in the present invention are all commercially available.

[0066] The positive and progressive effects of the present invention are:

[0067] (1) The present invention provides a new continuous polymerization process suitable for high temperature resistant polyamide, which includes salt formation-low pressure prepolymerization-high pressure prepolymerization-flash evaporation-post-polymerization, omitting the steps of concentration and pre-polymerization, thereby simplifying the process flow and reducing energy consumption.

[0068] (2) The present invention optimizes the existing continuous polymerization process, effectively avoiding the high-temperature degradation of polyamide, and obtaining high-temperature resistant polyamide resin chips with a lower yellow index, narrower molecular weight distribution, better crystallization ability, and more uniform product distribution.

[0069] (3) The continuous polymerization method provided by the present invention can produce multiple different types of high-temperature resistant polyamide products. Products with different properties obtained by using different monomers are suitable for a variety of application scenarios, which can expand the production and application scope of high-temperature resistant polyamide products and has great industrial value. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] Figure 1 This is a schematic structural diagram of a continuous production device for high temperature resistant polyamide according to Example 1 of the present invention.

[0071] Description of reference numerals:

[0072] 1-salt-forming reactor; 2-first low-pressure prepolymerization reactor; 3-second low-pressure prepolymerization reactor; 4-high-pressure prepolymerization reaction device, 41-high-pressure prepolymerization reactor I, 42-high-pressure prepolymerization reactor II, 43-high-pressure prepolymerization reactor III; 5-flash evaporator; 6-post-polymerization reactor. DETAILED DESCRIPTION

[0073] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the embodiments. The experimental methods in the following examples that do not specify specific conditions are selected according to conventional methods and conditions, or according to the product specifications. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0074] This embodiment 1 provides a continuous production device for high temperature resistant polyamide, such as Figure 1 As shown, it includes a salt-forming reaction device, a low-pressure prepolymerization reaction device, a high-pressure prepolymerization reaction device 4, a flash evaporation device and a post-polymerization reaction device connected in sequence;

[0075] The salt-forming reaction device is a salt-forming reaction kettle 1, which is used to mix the polymerization monomer of the high-temperature resistant polyamide with water to perform a salt-forming reaction to obtain a salt solution;

[0076] The low-pressure prepolymerization reaction device comprises a first low-pressure prepolymerization reactor 2 and a second low-pressure prepolymerization reactor 3;

[0077] The first low-pressure prepolymerization reactor 2 is used to carry out a first low-pressure prepolymerization reaction on the salt solution;

[0078] The second low-pressure prepolymerization reactor 3 is used to perform a second low-pressure prepolymerization reaction on the reaction product of the first low-pressure prepolymerization reaction to obtain a first polyamide melt;

[0079] The high-pressure prepolymerization reaction device 4 comprises three high-pressure prepolymerization reactors connected in series, namely, a high-pressure prepolymerization reactor I 41, a high-pressure prepolymerization reactor II 42 and a high-pressure prepolymerization reactor III 43, wherein the high-pressure prepolymerization reactor is used to perform a high-pressure prepolymerization reaction on the first polyamide melt to obtain a second polyamide melt;

[0080] The flash evaporation device is a flash evaporator 5, which is used to flash and dehydrate the second polyamide melt;

[0081] The final polymerization reaction device is a post-polymerization reactor 6, which is used to further polymerize the reaction product after flash evaporation.

[0082] The high temperature resistant polyamide continuous production equipment may further include a pelletizing device connected to the post-polymerization reactor 6 for underwater pelletizing the product of the polymerization reaction to obtain high temperature resistant polyamide resin chips.

[0083] Example 1

[0084] The preparation of the high temperature resistant polyamide of Example 1 is Figure 1 The continuous production method is as follows:

[0085] S1, adding diamine (pentanediamine), dibasic acid (terephthalic acid, adipic acid) and water into a salt-forming reactor 1, mixing at 92°C to prepare a salt solution with a concentration of 48%, adjusting the pH to 8.21 (the salt solution was diluted to 10% test result), controlling the molar ratio of diamine to dibasic acid to be 1.03:1, and the molar ratio of terephthalic acid to adipic acid to be 1.12:1;

[0086] S2, passing the salt solution into the first low-pressure prepolymerization reactor 2 for low-pressure prepolymerization 1, controlling the temperature of the low-pressure prepolymerization 1 to be 215° C., the pressure to be 1.1 MPa, and the time to be 115 min, passing the reaction product obtained by the low-pressure prepolymerization 1 into the second low-pressure prepolymerization reactor 3 for low-pressure prepolymerization 2, controlling the temperature of the low-pressure prepolymerization 2 to be 233° C., the pressure to be 1.5 MPa, and the time to be 90 min, to obtain a first polyamide melt;

[0087] S3, sequentially passing the first polyamide melt into a high-pressure prepolymerization reactor I 41, a high-pressure prepolymerization reactor II 42 and a high-pressure prepolymerization reactor III 43 for three-stage high-pressure prepolymerization, controlling the temperature of the first stage of high-pressure prepolymerization to be 242° C. and the pressure to be 1.7 MPa; the temperature of the second stage of high-pressure prepolymerization to be 262° C. and the pressure to be 1.7 MPa; the temperature of the last stage of high-pressure prepolymerization to be 297° C. and the pressure to be 1.7 MPa; controlling the time of the entire high-pressure prepolymerization to be 140 min, and obtaining a second polyamide melt having a mass percentage content of 92%;

[0088] S4, passing the second polyamide melt into the flash evaporator 5 for flash dehydration, controlling the flash temperature to be 312° C., the material pressure after flash evaporation to be 12 KPa, and the temperature to be 307° C.;

[0089] The flashed material is passed into the post-polymerization reactor 6 for final polymerization reaction, and the temperature of the final polymerization reaction is controlled to be 315° C. and the pressure of the final polymerization reaction is -0.072 MPa;

[0090] S5. Pass the product of the final polymerization reaction into a pelletizing device for underwater pelletizing, and control the temperature of the pelletizing water to be 55° C. to obtain high temperature resistant polyamide resin chips.

[0091] Example 2

[0092] The high temperature resistant polyamide continuous production equipment of Example 2 is similar to the equipment of Example 1, except that the high pressure prepolymerization reaction device 4 includes four high pressure prepolymerization reactors connected in series.

[0093] The continuous production method of the high temperature resistant polyamide of Example 2 is as follows:

[0094] S1. Add diamine (pentanediamine), dibasic acid (terephthalic acid, 1,12-dodecane dioic acid) and water into a salt-forming reactor, mix at 107°C to prepare a salt solution with a concentration of 55%, adjust the pH to 8.56 (the salt solution is diluted to 10% test result), control the molar ratio of diamine to dibasic acid to be 1.038:1, and the molar ratio of terephthalic acid to 1,12-dodecane dioic acid to be 1.45:1;

[0095] S2, passing the salt solution into the first low-pressure prepolymerization reactor for low-pressure prepolymerization 1, controlling the temperature of the low-pressure prepolymerization 1 to be 198° C., the pressure to be 0.95 MPa, and the time to be 75 min, passing the reaction product obtained by the low-pressure prepolymerization 1 into the second low-pressure prepolymerization reactor for low-pressure prepolymerization 2, controlling the temperature of the low-pressure prepolymerization 2 to be 223° C., the pressure to be 1.35 MPa, and the time to be 57 min, to obtain a first polyamide melt;

[0096] S3, sequentially passing the first polyamide melt into a high-pressure prepolymerization reactor I, a high-pressure prepolymerization reactor II, a high-pressure prepolymerization reactor III and a high-pressure prepolymerization reactor IV for 4 stages of high-pressure prepolymerization, controlling the temperature of the first stage of high-pressure prepolymerization to be 246° C. and the pressure to be 1.95 MPa; the temperature of the second stage of high-pressure prepolymerization to be 251° C. and the pressure to be 1.95 MPa; the temperature of the third stage of high-pressure prepolymerization to be 268° C. and the pressure to be 1.95 MPa; the temperature of the last stage of high-pressure prepolymerization to be 294° C. and the pressure to be 1.95 MPa; controlling the time of the entire high-pressure prepolymerization to be 270 min, and obtaining a second polyamide melt having a mass percentage content of 90%;

[0097] S4, passing the second polyamide melt into a flash evaporator for flash dehydration, controlling the flash temperature to be 305° C., the material pressure after flash evaporation to be 27 KPa, and the temperature to be 302° C.;

[0098] The flashed material was introduced into a post-polymerization reactor for final polymerization reaction, and the temperature of the final polymerization reaction was controlled to be 308°C and the pressure of the final polymerization reaction was -0.06MPa;

[0099] S5. Pass the product of the final polymerization reaction into a pelletizing device for underwater pelletizing, and control the temperature of the pelletizing water to be 68° C. to obtain high temperature resistant polyamide resin chips.

[0100] Example 3

[0101] The high temperature resistant polyamide continuous production equipment of Example 3 is similar to the equipment of Example 1, except that the high pressure prepolymerization reaction device 4 includes two high pressure prepolymerization reactors connected in series.

[0102] The continuous production method of the high temperature resistant polyamide of Example 3 is as follows:

[0103] S1. Add diamine (pentanediamine, hexamethylenediamine), dibasic acid (terephthalic acid, sebacic acid) and water into a salt-forming reactor, mix at 90°C to prepare a salt solution with a concentration of 45%, adjust the pH to 8.37 (the salt solution is diluted to 10% test result), control the molar ratio of diamine to dibasic acid to be 1.033:1, and the molar ratio of terephthalic acid to sebacic acid to be 2.64:1;

[0104] S2, passing the salt solution into the first low-pressure prepolymerization reactor for low-pressure prepolymerization 1, controlling the temperature of the low-pressure prepolymerization 1 to be 210° C., the pressure to be 1.07 MPa, and the time to be 108 min, passing the reaction product obtained by the low-pressure prepolymerization 1 into the second low-pressure prepolymerization reactor for low-pressure prepolymerization 2, controlling the temperature of the low-pressure prepolymerization 2 to be 225° C., the pressure to be 1.45 MPa, and the time to be 86 min, to obtain a first polyamide melt;

[0105] S3, passing the first polyamide melt into high-pressure prepolymerization reactor I and high-pressure prepolymerization reactor II in sequence, performing two stages of high-pressure prepolymerization, controlling the temperature of the first stage of high-pressure prepolymerization to 253° C. and the pressure to 1.8 MPa; controlling the temperature of the last stage of high-pressure prepolymerization to 298° C. and the pressure to 1.8 MPa; controlling the time of the entire high-pressure prepolymerization to 180 min, and obtaining a second polyamide melt having a mass percentage content of 95%;

[0106] S4, passing the second polyamide melt into a flash evaporator for flash dehydration, controlling the flash temperature to be 310° C., and the material pressure after flash evaporation to be 0 KPa and the temperature to be 308° C.;

[0107] The flashed material was introduced into a post-polymerization reactor for final polymerization reaction, and the temperature of the final polymerization reaction was controlled to be 313°C and the pressure of the final polymerization reaction was -0.067MPa;

[0108] S5. Pass the product of the final polymerization reaction into a pelletizing device for underwater pelletizing, and control the temperature of the pelletizing water to be 70° C. to obtain high temperature resistant polyamide resin chips.

[0109] Example 4

[0110] The high temperature resistant polyamide continuous production equipment of Example 4 is similar to the equipment of Example 1, except that the high pressure prepolymerization reaction device 4 includes 6 high pressure prepolymerization reactors connected in series.

[0111] The continuous production method of the high temperature resistant polyamide of Example 4 is as follows:

[0112] S1. Add diamine (pentanediamine, decanediamine), dibasic acid (terephthalic acid, adipic acid) and water into a salt-forming reactor, mix at 145°C to prepare a 60% salt solution, adjust the pH to 8.91 (the salt solution is diluted to 10% test result), control the molar ratio of diamine to dibasic acid to be 1.045:1, and the molar ratio of terephthalic acid to adipic acid to be 1.89:1;

[0113] S2, passing the salt solution into the first low-pressure prepolymerization reactor for low-pressure prepolymerization 1, controlling the temperature of the low-pressure prepolymerization 1 to be 182° C., the pressure to be 0.88 MPa, and the time to be 82 min, passing the reaction product obtained by the low-pressure prepolymerization 1 into the second low-pressure prepolymerization reactor for low-pressure prepolymerization 2, controlling the temperature of the low-pressure prepolymerization 2 to be 215° C., the pressure to be 1.2 MPa, and the time to be 65 min, to obtain a first polyamide melt;

[0114] S3, the first polyamide melt is sequentially passed into high-pressure prepolymerization reactor I, high-pressure prepolymerization reactor II, high-pressure prepolymerization reactor III, high-pressure prepolymerization reactor IV, high-pressure prepolymerization reactor V and high-pressure prepolymerization reactor VI for 6 sections of high-pressure prepolymerization, the temperature of the first section of high-pressure prepolymerization is controlled to be 248° C., and the pressure is 2.4 MPa; the temperature of the second section of high-pressure prepolymerization is 257° C., and the pressure is 2.4 MPa; the temperature of the third section of high-pressure prepolymerization is 264° C., and the pressure is 2.4 MPa; the temperature of the fourth section of high-pressure prepolymerization is 268° C., and the pressure is 2.4 MPa; the temperature of the fifth section of high-pressure prepolymerization is 271° C., and the pressure is 2.4 MPa; the temperature of the last section of high-pressure prepolymerization is 283° C., and the pressure is 2.4 MPa; the time of the entire high-pressure prepolymerization is controlled to be 340 min, and a second polyamide melt having a mass percentage content of 87% is obtained;

[0115] S4, passing the second polyamide melt into a flash evaporator for flash dehydration, controlling the flash temperature to be 300° C., the material pressure after flash evaporation to be 41 KPa, and the temperature to be 296° C.;

[0116] The flashed material is passed into a post-polymerization reactor for final polymerization reaction, and the temperature of the final polymerization reaction is controlled to be 304°C and the pressure of the final polymerization reaction is -0.085MPa;

[0117] S5. Pass the product of the final polymerization reaction into a pelletizing device for underwater pelletizing, and control the temperature of the pelletizing water to be 77° C. to obtain high temperature resistant polyamide chips.

[0118] Example 5

[0119] The high temperature resistant polyamide continuous production equipment of Example 5 is similar to the equipment of Example 1, except that the high pressure prepolymerization reaction device 4 includes 5 high pressure prepolymerization reactors connected in series.

[0120] The continuous production method of the high temperature resistant polyamide of Example 4 is as follows:

[0121] S1. Add diamine (pentanediamine, hexamethylenediamine), dibasic acid (terephthalic acid, adipic acid) and water into a salt-forming reactor, mix at 157°C to prepare a salt solution with a concentration of 75%, adjust the pH to 9.24 (the salt solution is diluted to 10% test result), control the molar ratio of diamine to dibasic acid to be 1.06:1, and the molar ratio of terephthalic acid to adipic acid to be 3.27:1;

[0122] S2, passing the salt solution into the first low-pressure prepolymerization reactor for low-pressure prepolymerization 1, controlling the temperature of the low-pressure prepolymerization 1 to be 193° C., the pressure to be 0.8 MPa, and the time to be 55 min, passing the reaction product obtained by the low-pressure prepolymerization 1 into the second low-pressure prepolymerization reactor for low-pressure prepolymerization 2, controlling the temperature of the low-pressure prepolymerization 2 to be 218° C., the pressure to be 1.1 MPa, and the time to be 40 min, to obtain a first polyamide melt;

[0123] S3, sequentially passing the first polyamide melt into a high-pressure prepolymerization reactor I, a high-pressure prepolymerization reactor II, a high-pressure prepolymerization reactor III, a high-pressure prepolymerization reactor IV and a high-pressure prepolymerization reactor V for 5 stages of high-pressure prepolymerization, controlling the temperature of the first stage of high-pressure prepolymerization to be 240° C. and the pressure to be 2.2 MPa; the temperature of the second stage of high-pressure prepolymerization to be 261° C. and the pressure to be 2.2 MPa; the temperature of the third stage of high-pressure prepolymerization to be 267° C. and the pressure to be 2.2 MPa; the temperature of the fourth stage of high-pressure prepolymerization to be 278° C. and the pressure to be 2.2 MPa; the temperature of the last stage of high-pressure prepolymerization to be 285° C. and the pressure to be 2.2 MPa; controlling the time of the entire high-pressure prepolymerization to be 380 min, and obtaining a second polyamide melt having a mass percentage content of 85%;

[0124] S4, passing the second polyamide melt into a flash evaporator for flash dehydration, controlling the flash temperature to be 295° C., and the material pressure after flash evaporation to be 50 KPa and the temperature to be 290° C.;

[0125] The flashed material was introduced into a post-polymerization reactor for final polymerization reaction, and the temperature of the final polymerization reaction was controlled to be 301°C and the pressure of the final polymerization reaction was -0.09MPa;

[0126] S5. Pass the product of the final polymerization reaction into a pelletizing device for underwater pelletizing, and control the temperature of the pelletizing water to be 80° C. to obtain high temperature resistant polyamide chips.

[0127] Comparative Example 1

[0128] In this example, steps S1, S3-S5 are the same as those in Example 1, except that step S2 is not performed, and step S3 is performed after the salt solution is preheated to 233° C. using a preheater.

[0129] The second polyamide melt with a mass percentage of 83% is obtained through high-temperature prepolymerization in step S3.

[0130] The material pressure after flash evaporation in step S4 is 18 KPa and the temperature is 305°C.

[0131] Comparative Example 2

[0132] In this example, steps S1-S2 and S4-S5 are the same as those in Example 3, with the only difference being that step S3 does not perform segmented temperature control, and only the first polyamide melt is passed into the high-pressure prepolymerization reactor, and the high-temperature prepolymerization temperature is controlled to be 298° C., the pressure to be 1.8 MPa, and the time to be 180 min, to obtain a second polyamide melt with a mass percentage content of 97%.

[0133] The material pressure after flash evaporation in step S4 is 0 KPa and the temperature is 309°C.

[0134] Effect Example

[0135] The high temperature resistant polyamide resin slices obtained in the above examples 1-5 and comparative examples 1-2 were tested as follows:

[0136] (1) Relative viscosity η r

[0137] Ubbelohde viscometer concentrated sulfuric acid method: Accurately weigh 0.5±0.0002g of the dried polyamide resin sample, add 50mL of concentrated sulfuric acid (96%) to dissolve to obtain a polyamide solution, and measure and record the concentrated sulfuric acid flow time t0 and the polyamide solution flow time t in a 25±0.02℃ constant temperature water bath. Relative viscosity calculation formula: Relative viscosity η r =t / t0.

[0138] (2) Melting point, crystallization point, crystallization half-peak width and crystallization enthalpy

[0139] The test method is based on ISO 11357-3, with a heating rate of 20°C / min.

[0140] (3) Yellowness Index

[0141] The test method refers to HG / T3862-2006.

[0142] (4) Amino terminal content

[0143] Accurately weigh 1g of sample and dissolve it in 40ml of hexafluoroisopropanol. Record the mass m of the sample. After it is completely dissolved, titrate it with 0.1mol / L HCL standard solution. Record the molar concentration c of the standard solution and the volume V of the hydrochloric acid consumed. Calculate the amino content:

[0144] (5) Moisture content

[0145] The moisture content of the samples was tested by Karl Fischer potentiometric titration at a temperature of 230 °C.

[0146] (6) Molecular weight distribution

[0147] Testing instrument: Gel permeation chromatography

[0148] Test method: The test was carried out by gel permeation chromatography (GPC). The standard substance was PMMA and the solvent was hexafluoroisopropanol. After complete dissolution, it was filtered through a PTFE membrane and analyzed at 40°C to obtain the molecular weight and distribution relative to PMMA.

[0149] The results are shown in Table 1.

[0150] Table 1

[0151]

[0152] It can be seen from the data in Table 1 that the high temperature resistant polyamide resin chips obtained by the continuous polymerization process of the present invention have a lower yellow index, better crystallization ability, narrower molecular weight distribution, and more uniform product distribution.

[0153] Those skilled in the art know that PDI (Polymer dispersity index) is a polymer dispersity index used to describe the molecular weight distribution of a polymer, and its value is also = M(w) / M(n), and its value is greater than 1. The larger the PDI, the wider the molecular weight distribution, and the smaller the PDI, the more uniform the molecular weight distribution.

Claims

1. A continuous production method of high temperature resistant polyamide, characterized in that: The steps include: S1, mixing the polymerization monomer of the high temperature resistant polyamide with water to prepare a salt solution; S2, prepolymerizing the salt solution under low pressure to obtain a first polyamide melt; S3, subjecting the first polyamide melt to high pressure prepolymerization to obtain a second polyamide melt; S4, flashing and final polymerizing the second polyamide melt to obtain a high temperature resistant polyamide; The polymer monomers of the high temperature resistant polyamide include diamines and dibasic acids, wherein the diamines are selected from one or more terminal diamines having carbon atoms of 1 to 15; the dibasic acids include dibasic acid A1 and dibasic acid A2, wherein the dibasic acid A1 is selected from aromatic dicarboxylic acids and their derivatives, and the dibasic acid A2 is selected from one or more aliphatic dicarboxylic acids having carbon atoms of 4 to 18.

2. The continuous production method of high temperature resistant polyamide according to claim 1, characterized in that: The molar ratio of the diamine to the dibasic acid is (0.9-1.2):1, further (1-1.08):1; and / or, The molar ratio of the dibasic acid A1 to the dibasic acid A2 is (0.5-4):1; and / or, The diamine includes one or more of 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine and 1,14-tetradecanediamine; and / or, The dibasic acid A1 includes terephthalic acid and its derivatives and / or isophthalic acid and its derivatives, preferably terephthalic acid; and / or, The dibasic acid A2 includes one or more of adipic acid, 1,8-octanedioic acid, 1,10-decanedioic acid, 1,11-undecanedioic acid, 1,12-dodecanedioic acid, 1,13-tridecanedioic acid, 1,14-tetradecanedioic acid and 1,16-hexadecanedioic acid.

3. The continuous production method of high temperature resistant polyamide according to claim 1, characterized in that: In step S1, the temperature at which the polymerized monomer of the high temperature resistant polyamide is mixed with water is 70-170° C., more preferably 90-165° C.; and / or, In step S1, the concentration of the salt solution is 40-80wt%, preferably 45-75wt%; and / or, In step S1, the pH value of the salt solution is 7.2-9.8, preferably 7.35-9.

65.

4. The continuous production method of high temperature resistant polyamide according to claim 1, characterized in that: In step S2, the low-pressure prepolymerization includes low-pressure prepolymerization 1 and low-pressure prepolymerization 2; Preferably, the temperature of the low-pressure prepolymerization 1 is below 180-215° C.; and / or, the pressure of the low-pressure prepolymerization 1 is 0.5-1.1 MPa, more preferably 0.8-1.1 MPa; and / or, the time of the low-pressure prepolymerization 1 is 30-120 min; Preferably, the temperature of the low-pressure prepolymerization 2 is below 215-235° C.; and / or, the pressure of the low-pressure prepolymerization 2 is 1.1-1.5 MPa; and / or, the time of the low-pressure prepolymerization 2 is 40-90 min.

5. The continuous production method of high temperature resistant polyamide according to claim 1, characterized in that: In step S3, the pressure of the high pressure prepolymerization is below 3.2 MPa, preferably 1.7-2.5 MPa; and / or, In step S3, the temperature of the high pressure prepolymerization is 240-310° C.; and / or, In step S3, the high pressure prepolymerization time is 60-420 min, preferably 100-400 min; and / or, In step S3, the mass percentage content of the obtained second polyamide melt is 85-95%.

6. The continuous production method of high temperature resistant polyamide according to claim 5, characterized in that: The temperature of the high pressure prepolymerization is controlled in stages, preferably in 2-6 stages; Preferably, the temperature of the latter stage is greater than or equal to the temperature of the former stage; Preferably, the temperature difference between the latter stage and the former stage is 0-50°C, more preferably 2-20°C; Preferably, the temperature of the first stage is 240-255°C; Preferably, the temperature of the last stage is 280-310°C.

7. The continuous production method of high temperature resistant polyamide according to claim 1, characterized in that: In step S4, the flash evaporation temperature is 290-340° C.; and / or, In step S4, the pressure of the material after flash evaporation is 0-50 KPa, and / or the temperature of the material after flash evaporation is 290-320° C.; and / or, In step S4, the final polymerization temperature is 290-340°C, preferably 295-330°C; and / or, In step S4, the final polymerization is carried out under normal pressure or vacuum conditions; Preferably, an inert gas is used for protection during final polymerization at normal pressure; Preferably, the final polymerization pressure under vacuum conditions is -0.095 to 0 MPa, more preferably -0.09 to 0 MPa; And / or, the method further comprises step S5, that is, performing underwater pelletizing on the high temperature resistant polyamide obtained in step S4 to obtain high temperature resistant polyamide resin slices; further, controlling the temperature of pelletizing water to be 55-80°C.

8. A continuous production device for high temperature resistant polyamide, comprising a salt-forming reaction device, a low pressure prepolymerization reaction device, a high pressure prepolymerization reaction device, a flash evaporation device and a final polymerization reaction device connected in sequence; The salt-forming reaction device comprises a salt-forming reaction kettle, which is used to mix the polymerized monomer of the high-temperature resistant polyamide with water to perform a salt-forming reaction to obtain a salt solution; The low-pressure prepolymerization reaction device comprises a first low-pressure prepolymerization reactor and a second low-pressure prepolymerization reactor; the first low-pressure prepolymerization reactor is used to carry out a first low-pressure prepolymerization reaction on the salt solution, and the second low-pressure prepolymerization reactor is used to carry out a second low-pressure prepolymerization reaction on the reaction product of the first low-pressure prepolymerization reaction to obtain a first polyamide melt; The high-pressure prepolymerization reaction device comprises at least two high-pressure prepolymerization reactors connected in series, preferably 2-6 high-pressure prepolymerization reactors connected in series, and the high-pressure prepolymerization reactor is used to perform a high-pressure prepolymerization reaction on the first polyamide melt to obtain a second polyamide melt; The flash evaporation device comprises a flash evaporator for flash evaporating and dehydrating the second polyamide melt; The final polymerization reaction device comprises a post-polymerization reactor, which is used for further polymerizing the reaction product after the flash evaporation.

9. The continuous production equipment of high temperature resistant polyamide according to claim 8, characterized in that: The continuous production equipment also includes a pelletizing device connected to the final polymerization reaction device, which is used to perform underwater pelletizing on the further polymerized product to obtain high temperature resistant polyamide resin chips.

10. A method for continuous production of high temperature resistant polyamide, which is carried out in the continuous production equipment as claimed in claim 8 or 9.