High-strength fireproof polyolefin cable material and cable preparation method thereof
Through the combination of microwave cross-linking technology and modified materials, the problem of insufficient flame retardant performance of traditional polyolefin cable materials in fires has been solved, the improvement of high strength, heat resistance and flame retardancy has been achieved, and the thickness of traditional polyolefin cable materials has been overcome. Limitations and deficiencies in mechanical properties.
Patent Information
- Application Number
- CN202410792345.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-24
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-22
AI Technical Summary
Traditional polyolefin cable materials have no obvious carbon residue in case of fire and cannot melt and bond with ceramic powder to form a dense flame retardant layer, resulting in insufficient flame retardant performance. Moreover, traditional cross-linking methods cannot effectively improve mechanical properties and performance in the presence of high inorganic fillers. Drip resistance.
Microwave cross-linking technology is used to combine modified EVA resin and glass fiber modified PP, and zinc borate @Zn(OH)2 hybrid modified wollastonite powder and glass powder are used to form a chemical and physical interpenetrating network structure to promote MPP and PAPP catalyzes the carbonization of the resin matrix to enhance the flame retardancy and drip resistance of the cable material.
It significantly improves the heat resistance and flame retardancy of cable materials, avoids melt dripping and high temperature shrinkage, enhances the material's flame retardancy and drip resistance, and at the same time overcomes the thickness limitations of traditional cross-linking technology.
Smart Images

Figure CN118812949A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cable materials, and in particular relates to a high-strength fireproof polyolefin cable material and a cable preparation method thereof. Background Art
[0002] Polyolefin materials have excellent mechanical properties, insulation and processability, and are widely used in the preparation of cable materials. As people's requirements for power facilities become higher and higher, the application of flame-retardant cables in the power field is becoming more and more extensive, and the market demand is increasing.
[0003] Flame-retardant and fireproof cables are required to have good self-extinguishing performance, low smoke performance, good mechanical properties, and good electrical properties, so that they can play a key role in responding to emergencies such as fires, protecting personnel safety, and reducing property losses. Traditional flame-retardant cable materials are mainly halogen-containing flame retardants, which release a large amount of toxic gases such as halogen acids when burned. These gases are not only highly irritating to the human respiratory tract and eyes, but may also cause secondary pollution to the surrounding environment. At the scene of a fire, these toxic gases may cause poisoning or even death to personnel, increasing the difficulty of rescue.
[0004] Ceramic cable materials have been the focus of scientific and industrial attention in recent years. The preparation method is to add a certain amount of ceramic powder to the cable resin matrix and then melt blend it. The flame retardant and fireproof mechanism of this ceramic cable material is that the ceramic powder melts at high temperature and then bonds to the residual carbon after the decomposition of the resin matrix to form a dense carbon-containing ceramic layer, which plays a role in flame retardancy and fireproofing. However, this method has the following problems for cable materials with polyolefin resin matrix:
[0005] ① Due to the addition of a large amount of inorganic fire-retardant fillers, the mechanical properties of the cable material are reduced; ② Traditional ceramic polyolefin fire-retardant materials, due to the high-temperature melting fluidity of the ceramic filler, will aggravate the melting dripping of the material under high temperature or combustion; ③ Polyolefin materials (such as EVA, polypropylene, etc.) are almost completely decomposed into carbon oxides after pyrolysis, and evaporate rapidly under high heat release, without obvious carbon residue, and cannot melt and bond with ceramic powder during combustion to form a dense flame-retardant carbon-containing ceramic layer, and cannot play a good flame-retardant and fire-retardant role. ④ The traditional cross-linking method to improve the mechanical properties and anti-dripping of the material cannot wrap the wire in the presence of high inorganic fire-retardant fillers and the cross-linking thickness is limited. Summary of the invention
[0006] The problem in the prior art is that after the pyrolysis of the cable material based on polypropylene resin, there is no obvious residual carbon, and it cannot melt and bond with the ceramic powder during the combustion process to form a dense flame-retardant carbon-containing ceramic layer, and cannot play a good flame-retardant and fire-proof role. Based on the above technical problems, the present invention provides a high-strength fire-resistant polyolefin cable material, which includes the following components by weight:
[0007] PP 20-25 copies;
[0008] Glass fiber modified PP 20-25 parts;
[0009] Modified EVA 10-15 parts;
[0010] 15-20 parts of modified wollastonite powder;
[0011] PAPP 24-30 copies;
[0012] MPP 12-15 copies;
[0013] 20-25 parts of glass powder.
[0014] Preferably, the mass percentage of glass fiber in the glass fiber modified PP is 10-15wt%, and the length of the glass fiber is 3-5mm.
[0015] Preferably, the preparation method of the modified EVA comprises the following steps:
[0016] The grafted graphite oxide and EVA resin are mixed at a mass ratio of 4:100-200, and then extruded and granulated through an extruder to obtain modified EVA material with the required particle size. During the extrusion process, the temperature from the hopper to the extrusion die is set at 80-115°C, and the die heating temperature is 105°C.
[0017] Preferably, the preparation method of modified wollastonite powder comprises the following steps:
[0018] (1) adding zinc sulfate to 100 mL of aqueous solution, stirring uniformly at a constant temperature of 45-50° C., to obtain an aqueous solution of zinc sulfate with a mass concentration of 40-45 mg / mL;
[0019] (2) adding wollastonite powder to the aqueous zinc sulfate solution obtained in step (1), wherein the mass ratio of the wollastonite powder to the zinc sulfate in step (1) is 50-55:4, and stirring at a constant temperature of 45-50° C. to obtain a mixed solution;
[0020] (3) adding borax and zinc oxide to the mixed solution obtained in step (2), and stirring at a constant temperature of 85-90° C. for 5-6 hours, then adjusting the pH of the reaction system to 8-9, and after the reaction is completed, filtering and drying to obtain modified wollastonite powder; the mass ratio of the borax to the zinc sulfate in step (1) is 2-3:1, and the mass ratio of the borax to the zinc oxide is 4-5:1.
[0021] Preferably, the average particle size of the borax is 1-2 μm.
[0022] Preferably, the average particle size of the zinc oxide is 1-2 μm.
[0023] Preferably, the pH adjuster is an aqueous sodium hydroxide solution.
[0024] Preferably, the average particle size of the glass powder is 1-6 μm.
[0025] Preferably, 3-6 parts of auxiliary agents are also included.
[0026] Preferably, the auxiliary agent includes one or more of a lubricant, a stabilizer, and an antioxidant.
[0027] Preferably, the preparation method of the high-strength fire-resistant polyolefin cable obtained by the high-strength fire-resistant polyolefin cable material comprises the following steps:
[0028] S1, mixing the components of the high-strength fire-resistant polyolefin cable material evenly according to the formula amount to obtain a premix;
[0029] S2, using an extruder to melt and extrude the premixed materials respectively, and after the extruded materials are cross-linked by microwaves, they are cooled and granulated to obtain high-strength fire-resistant polyolefin cable materials with a desired particle size;
[0030] S3, placing the obtained high-strength fire-resistant polyolefin cable materials in an extruder for melt extrusion to obtain an insulating layer, and making the insulating layer cover the outer surface of the metal conductor to obtain a coating material, and then placing the obtained coating materials in a microwave cross-linking furnace for microwave cross-linking to obtain a high-strength fire-resistant polyolefin cable.
[0031] 12. A high-strength fire-resistant polyolefin cable according to claim 11, characterized in that the temperature of the premix melt extrusion is 170-230°C, the time of microwave cross-linking is 6-10s, and the power of microwave cross-linking is 600-800W.
[0032] The present invention has the following beneficial effects:
[0033] (1) The present invention adopts microwave cross-linking technology in the production process of cable materials, which overcomes the limitation of radiation cross-linking technology on cable thickness. At the same time, in the cabling process, the preparation of cross-linked polyolefin cables is achieved by first coating the conductor with resin and then rapidly cross-linking with microwaves, thereby avoiding the problem that the resin cannot coat the conductor due to thermal cross-linking before extrusion, and also avoiding the problem of low efficiency of subsequent thermal cross-linking.
[0034] (2) The modified EVA resin and the glass fiber modified PP in the cable material formula of the present invention form a chemically and physically interpenetrating network structure during the cabling process, which significantly improves the heat resistance of the obtained cable material and is not easy to melt and drip at a temperature below 350° C., providing conditions for the crystalline ceramic reaction of wollastonite and glass powder after pyrolysis, further improving the flame retardancy of the cable material;
[0035] (3) The cable material formula of the present invention uses wollastonite powder modified by zinc borate@Zn(OH)2 hybridization. The essence of this material is that nano zinc borate and Zn(OH)2 are deposited on the surface of wollastonite by electrostatic adsorption, and the in-situ catalytic carbonization of the resin matrix by MPP and PAPP flame retardants is achieved under the catalytic action of transition metals. The principle is that the dehydration of the resin matrix by MPP and PAPP is promoted, and the increase of residual carbon provides a material basis for the later ceramicization reaction, which is the key to avoiding high-temperature shrinkage, ablation, cracking and burning through of the cable material;
[0036] (4) The glass fiber in the glass fiber modified PP has a certain fire resistance. At high temperature, it will exist in the residue system after ablation in the form of a skeleton, providing an attachment point for the deposition of residual carbon and the growth of ceramic structure, thereby significantly improving the flame retardancy and anti-dripping properties of the material. Under the cable material formula system of the present invention, the glass fiber can form a relatively dense residue with the residual carbon and the ceramic structure. When the glass fiber is more, it is easy to form a wick effect, and thus cannot play a significant flame retardant effect. When the glass fiber is less, on the one hand, it cannot provide an attachment point for the deposition of residual carbon and the growth of ceramic structure, and has no obvious effect on improving the strength of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 : is an infrared comparison spectrum of the modified EVA obtained in Example 1 of the present invention and pure EVA.
[0038] Figure 2 : is a comparative test result diagram of the gel content of modified EVA and pure EVA in Example 1 of the present invention.
[0039] Figure 3 : is a microstructure diagram of the cable material obtained in Example 1 of the present invention at 1000°C;
[0040] Figure 4 : is a ceramic phase structure diagram of the cable material obtained in Example 1 of the present invention at 1000°C;
[0041] Figure 5 : It is the self-supporting performance test result of the cable material obtained in Example 1 of the present invention at room temperature to 1000°C. DETAILED DESCRIPTION
[0042] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.
[0043] The PP used in the following examples of the present invention was purchased from Yaqing Plastic Products Factory, Dongfeng Town, Zhongshan City.
[0044] The modified EVA in the following embodiments of the present invention is prepared according to the following steps:
[0045] The grafted graphite oxide and EVA resin are mixed at a mass ratio of 4:100, and then extruded and granulated by an extruder to obtain modified EVA of the required particle size. During the extrusion process, the temperature from the hopper to the extrusion die is set at 80-115°C. During the extrusion process, the temperature of zone 1 is 80°C, the temperature of zone 2 is 105°C, the temperature of zone 3 is 105°C, the temperature of zone 4 is 110°C, the temperature of zone 5 is 115°C, the temperature of zone 6 is 110°C, the temperature of zone 7 is 105°C, and the head heating temperature is 105°C. The preparation method of the grafted graphite oxide is as follows:
[0046] (1) dissolving 100 parts of dichlorobenzene, 15 parts of paraformaldehyde, 3 parts of anhydrous tin tetrachloride and 55 parts of trimethylsilyl chloride in 800 parts of N,N-dimethylformamide, reacting at 70° C. for 7 hours to obtain a N,N-dimethylformamide solution containing dichlorobenzene;
[0047] (2) In 500 mL of a 1.5 wt% N,N-dimethylformamide solution containing dichlorodiphenylamine, 20 parts of graphene oxide and 5 parts of anhydrous sodium carbonate were added, and the mixture was ultrasonicated at 1100 W for 35 min, and then reacted at 70 ° C for 7 h to obtain a dichlorodiphenylamine-loaded graphene oxide solution. The solution was filtered and washed with deionized water, and the solid powder was dried at 100 ° C to obtain dichlorodiphenylamine-grafted graphite oxide.
[0048] The EVA resin used in the following examples of the present invention has a VA content of 28 wt% (mass fraction) and a melt index of 6 g / 10 min. It is purchased from BASF-Yangtze and has a product number or brand name of 6110M.
[0049] PAPP used in the following examples of the present invention has CAS number: 66034-17-1.
[0050] The MPP used in the following examples of the present invention was purchased from Ningbo Zhiwei New Material Technology Co., Ltd., product number: 1616039701.
[0051] The glass powder used in the following examples of the present invention was purchased from Shanggao Mingzheng Plastic Chemical Co., Ltd., with the product number GS-3000.
[0052] The high-strength fire-resistant polyolefin cable material in the following embodiments of the present invention is prepared as follows:
[0053] S1, mixing the components of the high-strength fire-resistant polyolefin cable material evenly according to the formula amount to obtain a premix;
[0054] S2, using an extruder to melt and extrude the premixes respectively, the temperature of the premixes being melted and extruded is 230° C. After the extruded materials are cross-linked by microwaves, they are cooled and granulated to obtain a high-strength fire-resistant polyolefin cable material with an average particle size of 5 mm;
[0055] S3, placing the obtained high-strength fireproof polyolefin cable material in an extruder for melt extrusion to obtain an insulating layer, and making the insulating layer cover the outer surface of the copper metal conductor to obtain a coating material, and then placing the obtained coating material in a microwave cross-linking furnace for microwave cross-linking, the microwave cross-linking time is 6s, the microwave cross-linking power is 800W, and after the microwave cross-linking is completed, a high-strength fireproof polyolefin cable is obtained. The microwave cross-linking furnace is an intelligent experimental microwave oven|laboratory microwave oven, model nai-sys-wbl.
[0056] Example 1
[0057] A high-strength fire-resistant polyolefin cable material, the components of which are as follows in parts by weight:
[0058] PP 20 copies;
[0059] Glass fiber modified PP 20 parts;
[0060] Modified EVA 10 parts;
[0061] 15 parts of modified wollastonite powder;
[0062] PAPP 24;
[0063] MPP 12 copies;
[0064] 20 parts of glass powder.
[0065] The modified wollastonite powder is prepared in the following steps:
[0066] (1) adding zinc sulfate to 100 mL of aqueous solution, stirring at a constant temperature of 45° C. to obtain an aqueous solution of zinc sulfate with a mass concentration of 40 mg / mL;
[0067] (2) adding wollastonite powder to the aqueous zinc sulfate solution obtained in step (1), wherein the mass ratio of the wollastonite powder to the zinc sulfate in step (1) is 50:4, and stirring at a constant temperature of 45° C. to obtain a mixed solution;
[0068] (3) adding borax and zinc oxide to the mixed solution obtained in step (2), and stirring at a constant temperature of 90° C. for 5 h, then adjusting the pH of the reaction system to 8, and after the reaction is completed, filtering and drying to obtain modified wollastonite powder; the mass ratio of the borax to the zinc sulfate in step (1) is 2:1, and the mass ratio of the borax to the zinc oxide is 4:1.
[0069] The average particle size of the wollastonite powder is 8 μm.
[0070] The average particle size of the borax is 2 μm.
[0071] The average particle size of the zinc oxide is 2 μm.
[0072] The pH regulator used in the preparation method of modified wollastonite powder is 0.5M sodium hydroxide aqueous solution.
[0073] The average particle size of the glass powder is 6 μm.
[0074] The glass fiber modified PP used was purchased from Suqian Nanjing University of Technology New Materials Research Institute Co., Ltd. The average length of the customized material glass fiber was 3 mm, and the mass percentage of glass fiber was 10%.
[0075] The infrared contrast spectra of the modified EVA obtained in Example 1 of the present invention and the pure EVA are shown in the attached specification. Figure 1 shown.
[0076] The gel content comparison test results of the modified EVA and pure EVA obtained in Example 1 of the present invention are shown in the attached manual. Figure 2 shown.
[0077] The microstructure of the cable material obtained in Example 1 of the present invention at 1000°C is shown in the attached specification. Figure 3 shown.
[0078] The ceramic phase structure diagram of the cable material obtained in Example 1 of the present invention at 1000°C is shown in the attached manual. Figure 4 shown.
[0079] The self-supporting performance test results of the cable material obtained in Example 1 of the present invention at room temperature to 1000°C are shown in the attached manual. Figure 5 shown.
[0080] Example 2
[0081] A high-strength fire-resistant polyolefin cable material, the components of which are as follows in parts by weight:
[0082] PP 22 copies;
[0083] Glass fiber modified PP 21 parts;
[0084] Modified EVA 12 parts;
[0085] 15 parts of modified wollastonite powder;
[0086] PAPP 25 copies;
[0087] MPP 12 copies;
[0088] 20 parts of glass powder.
[0089] The modified wollastonite powder is prepared in the following steps:
[0090] (1) adding zinc sulfate to 100 mL of aqueous solution, stirring at a constant temperature of 47° C. to obtain an aqueous solution of zinc sulfate with a mass concentration of 42 mg / mL;
[0091] (2) adding wollastonite powder to the aqueous zinc sulfate solution obtained in step (1), wherein the mass ratio of the wollastonite powder to the zinc sulfate in step (1) is 52:4, and stirring at a constant temperature of 50° C. to obtain a mixed solution;
[0092] (3) adding borax and zinc oxide to the mixed solution obtained in step (2), and stirring at a constant temperature of 85° C. for 6 h, then adjusting the pH of the reaction system to 8.5, and completing the reaction. After filtering and drying, modified wollastonite powder is obtained; the mass ratio of the borax to the zinc sulfate in step (1) is 2.2:1, and the mass ratio of the borax to the zinc oxide is 4.2:1.
[0093] The average particle size of the wollastonite powder is 8 μm.
[0094] The average particle size of the borax is 2 μm.
[0095] The average particle size of the zinc oxide is 2 μm.
[0096] The pH regulator used in the preparation method of modified wollastonite powder is 0.5 mol / L sodium hydroxide aqueous solution.
[0097] The average particle size of the glass powder is 6 μm.
[0098] The glass fiber modified PP used was purchased from Suqian Nanjing University of Technology New Materials Research Institute Co., Ltd. The average length of the customized material glass fiber was 4 mm, and the mass percentage of the glass fiber was 12%.
[0099] Example 3
[0100] A high-strength fire-resistant polyolefin cable material, the components of which are as follows in parts by weight:
[0101] PP 23 copies;
[0102] Glass fiber modified PP 22 parts;
[0103] Modified EVA 12 parts;
[0104] 16 parts of modified wollastonite powder;
[0105] PAPP 26 copies;
[0106] MPP 13 copies;
[0107] 22 parts of glass powder.
[0108] The modified wollastonite powder is prepared in the following steps:
[0109] (1) adding zinc sulfate to 100 mL of aqueous solution, stirring at a constant temperature of 50° C. to obtain an aqueous solution of zinc sulfate with a mass concentration of 43 mg / mL;
[0110] (2) adding wollastonite powder to the aqueous zinc sulfate solution obtained in step (1), wherein the mass ratio of the wollastonite powder to the zinc sulfate in step (1) is 53:4, and stirring at a constant temperature of 50° C. to obtain a mixed solution;
[0111] (3) adding borax and zinc oxide to the mixed solution obtained in step (2), and stirring at a constant temperature of 90° C. for 5 h, then adjusting the pH of the reaction system to 9, and after the reaction is completed, filtering and drying to obtain modified wollastonite powder; the mass ratio of the borax to the zinc sulfate in step (1) is 2.5:1, and the mass ratio of the borax to the zinc oxide is 4.3:1.
[0112] The average particle size of the wollastonite powder is 8 μm.
[0113] The average particle size of the borax is 2 μm.
[0114] The average particle size of the zinc oxide is 2 μm.
[0115] The pH regulator used in the preparation method of modified wollastonite powder is 0.5M sodium hydroxide aqueous solution.
[0116] The average particle size of the glass powder is 6 μm.
[0117] The glass fiber modified PP used was purchased from Suqian Nanjing University of Technology New Materials Research Institute Co., Ltd. The average length of the customized material glass fiber was 5 mm, and the mass percentage of glass fiber was 15%.
[0118] Example 4
[0119] A high-strength fire-resistant polyolefin cable material, the components of which are as follows in parts by weight:
[0120] PP 23 copies;
[0121] Glass fiber modified PP 22 parts;
[0122] Modified EVA 13 parts;
[0123] 18 parts of modified wollastonite powder;
[0124] PAPP 27 copies;
[0125] MPP 13 copies;
[0126] 24 parts of glass powder.
[0127] The modified wollastonite powder is prepared in the following steps:
[0128] (1) adding zinc sulfate to 100 mL of aqueous solution, stirring at a constant temperature of 50° C. to obtain an aqueous solution of zinc sulfate with a mass concentration of 43 mg / mL;
[0129] (2) adding wollastonite powder to the aqueous zinc sulfate solution obtained in step (1), wherein the mass ratio of the wollastonite powder to the zinc sulfate in step (1) is 52:4, and stirring at a constant temperature of 50° C. to obtain a mixed solution;
[0130] (3) adding borax and zinc oxide to the mixed solution obtained in step (2), and stirring at a constant temperature of 88° C. for 6 h, then adjusting the pH of the reaction system to 8, and after the reaction is completed, filtering and drying to obtain modified wollastonite powder; the mass ratio of the borax to the zinc sulfate in step (1) is 2.8:1, and the mass ratio of the borax to the zinc oxide is 4.7:1.
[0131] The average particle size of the wollastonite powder is 8 μm.
[0132] The average particle size of the borax is 2 μm.
[0133] The average particle size of the zinc oxide is 2 μm.
[0134] The pH regulator used in the preparation method of modified wollastonite powder is 0.5M sodium hydroxide aqueous solution.
[0135] The average particle size of the glass powder is 6 μm.
[0136] The glass fiber modified PP used was customized by Suqian Nanjing University of Technology New Materials Research Institute Co., Ltd. The average length of the customized material glass fiber is 3mm, and the mass percentage of glass fiber is 10%.
[0137] Example 5
[0138] A high-strength fire-resistant polyolefin cable material, the components of which are as follows in parts by weight:
[0139] PP 25 copies;
[0140] Glass fiber modified PP 25 parts;
[0141] Modified EVA 15 parts;
[0142] 20 parts of modified wollastonite powder;
[0143] PAPP 30 copies;
[0144] MPP 15 copies;
[0145] 25 parts of glass powder.
[0146] The modified wollastonite powder is prepared in the following steps:
[0147] (1) adding zinc sulfate to 100 mL of aqueous solution, stirring uniformly at a constant temperature of 45° C., to obtain an aqueous solution of zinc sulfate with a mass concentration of 45 mg / mL;
[0148] (2) adding wollastonite powder to the aqueous zinc sulfate solution obtained in step (1), wherein the mass ratio of the wollastonite powder to the zinc sulfate in step (1) is 55:4, and stirring at a constant temperature of 50° C. to obtain a mixed solution;
[0149] (3) adding borax and zinc oxide to the mixed solution obtained in step (2), and stirring at a constant temperature of 90° C. for 5 h, then adjusting the pH of the reaction system to 8, and after the reaction is completed, filtering and drying to obtain modified wollastonite powder; the mass ratio of the borax to the zinc sulfate in step (1) is 3:1, and the mass ratio of the borax to the zinc oxide is 5:1.
[0150] The average particle size of the wollastonite powder is 8 μm.
[0151] The average particle size of the borax is 2 μm.
[0152] The average particle size of the zinc oxide is 2 μm.
[0153] The pH regulator used in the preparation method of modified wollastonite powder is 0.5M sodium hydroxide aqueous solution.
[0154] The average particle size of the glass powder is 6 μm.
[0155] The glass fiber modified PP used is provided by Suqian Nanjing University of Technology New Materials Research Institute Co., Ltd. The average length of the customized material glass fiber is 3mm and the mass percentage of glass fiber is 15%.
[0156] Comparative Example 1 is the same as Example 1, except that the modified wollastonite powder in Example 1 is replaced by pure wollastonite powder in equal parts by weight.
[0157] Comparative Example 2 is the same as Example 1, except that the modified EVA in Example 1 is replaced by pure EVA resin in equal parts by weight.
[0158] Comparative Example 3 is the same as Example 1, except that, during the preparation of the modified EVA in Comparative Example 3, the mass ratio of the grafted graphite oxide to the EVA resin is 2:100.
[0159] Comparative Example 4 is the same as Example 1, except that modified glass fiber modified PP is not added in Comparative Example 4.
[0160] Comparative Example 5 is the same as Example 1, except that, in the glass fiber-modified PP used in Comparative Example 5, the mass percentage of glass fiber is 20 wt %, and the average length of the glass fiber is 3 mm.
[0161] Comparative Example 6 is the same as Example 1, except that, in the glass fiber-modified PP used in Comparative Example 6, the mass percentage of glass fiber is 5 wt %, and the average length of the glass fiber is 3 mm.
[0162] Comparative Example 7 is the same as Example 1, except that, in the preparation process of the modified wollastonite powder in Comparative Example 7, the mass ratio of the wollastonite powder to the zinc sulfate in step (1) is 50:2.
[0163] Comparative Example 8 is the same as Example 1, except that in the preparation process of the modified wollastonite powder in Comparative Example 8, the mass ratio of the wollastonite powder to the zinc sulfate in step (1) is 50:8.
[0164] Comparative Example 9 is the same as Example 1, except that the mass ratio of borax to zinc sulfate in step (1) during the preparation of the modified wollastonite powder in Comparative Example 9 is 1:1.
[0165] Comparative Example 10 is the same as Example 1, except that the mass ratio of borax to zinc sulfate in step (1) during the preparation of the modified wollastonite powder in Comparative Example 10 is 1:2.
[0166] Performance Testing
[0167] The cable materials obtained in Examples 1-5 of the present invention and Comparative Examples 1-10 were respectively subjected to relevant performance tests, and the specific test results are shown in Table 1 and Table 1.
[0168] The test methods involved are as follows:
[0169] Tensile strength and elongation at break of cable materials: tested in accordance with ASTM D638 standard test standard, with a tensile rate of 50mm / min.
[0170] Impact strength of cable materials: tested in accordance with ASTMD256 test standard.
[0171] Fire resistance of cable materials: Use a butane spray gun (1300°C flame) to ablate a 4mm thick sample sheet and observe whether the sample sheet is burned through or carbonized.
[0172] Flame retardant properties of cable materials: tested in accordance with UL94 horizontal and vertical burning test.
[0173] Self-supporting performance of cable material from room temperature to 1000℃: suspend a 50mm*5mm*2mm spline on parallel refractory bricks, with the suspended part length of 12mm, and the length of the spline on each refractory brick is equal. Place the placed spline in a muffle furnace at room temperature, raise the temperature to 1000 degrees at a rate of 10 degrees per minute, and observe the bending degree of the suspended spline. Burning means no self-support, and the larger the bending angle, the worse the self-support.
[0174] Table 1
[0175]
[0176] Table 1
[0177]
[0178] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A high-strength fire-resistant polyolefin cable material, characterized in that: The composition includes the following components by weight: PP 20-25 copies; Glass fiber modified PP 20-25 parts; Modified EVA 10-15 parts; 15-20 parts of modified wollastonite powder; PAPP 24-30 copies; MPP 12-15 copies; 20-25 parts of glass powder.
2. The high-strength fire-resistant polyolefin cable material according to claim 1, characterized in that: The mass percentage of glass fiber in the glass fiber modified PP is 10-15wt%, and the length of the glass fiber is 3-5mm.
3. The high-strength fire-resistant polyolefin cable material according to claim 1, characterized in that: The preparation method of the modified EVA comprises the following steps: The grafted graphite oxide and EVA resin are mixed at a mass ratio of 4:100-200, and then extruded and granulated through an extruder to obtain modified EVA material with the required particle size. During the extrusion process, the temperature from the hopper to the extrusion die is set at 80-115°C, and the die heating temperature is 105°C.
4. The high-strength fire-resistant polyolefin cable material according to claim 1, characterized in that: The preparation method of modified wollastonite powder comprises the following steps: (1) adding zinc sulfate to 100 mL of aqueous solution, stirring uniformly at a constant temperature of 45-50° C., to obtain an aqueous solution of zinc sulfate with a mass concentration of 40-45 mg / mL; (2) adding wollastonite powder to the aqueous zinc sulfate solution obtained in step (1), wherein the mass ratio of the wollastonite powder to the zinc sulfate in step (1) is 50-55:4, and stirring at a constant temperature of 45-50° C. to obtain a mixed solution; (3) adding borax and zinc oxide to the mixed solution obtained in step (2), and stirring at a constant temperature of 85-90° C. for 5-6 hours, then adjusting the pH of the reaction system to 8-9, and after the reaction is completed, filtering and drying to obtain modified wollastonite powder; the mass ratio of the borax to the zinc sulfate in step (1) is 2-3:1, and the mass ratio of the borax to the zinc oxide is 4-5:
1.
5. The high-strength fire-resistant polyolefin cable material according to claim 4, characterized in that: The average particle size of the borax is 1-2 μm.
6. The high-strength fire-resistant polyolefin cable material according to claim 4, characterized in that: The average particle size of the zinc oxide is 1-2 μm.
7. The high-strength fire-resistant polyolefin cable material according to claim 4, characterized in that: The pH adjuster is a sodium hydroxide aqueous solution.
8. A high-strength fire-resistant polyolefin cable prepared using the high-strength fire-resistant polyolefin cable material as described in any one of claims 1 to 7.
9. The high-strength fire-resistant polyolefin cable according to claim 8, characterized in that: The preparation method comprises the following steps: S1, mixing the components of the high-strength fire-resistant polyolefin cable material evenly according to the formula amount to obtain a premix; S2, using an extruder to melt and extrude the premixed materials respectively, and after the extruded materials are cross-linked by microwaves, they are cooled and granulated to obtain high-strength fire-resistant polyolefin cable materials with a desired particle size; S3, placing the obtained high-strength fire-resistant polyolefin cable materials in an extruder for melt extrusion to obtain an insulating layer, and making the insulating layer cover the outer surface of the metal conductor to obtain a coating material, and then placing the obtained coating materials in a microwave cross-linking furnace for microwave cross-linking to obtain a high-strength fire-resistant polyolefin cable.
10. A high-strength fire-resistant polyolefin cable according to claim 9, characterized in that: The temperature of premix melt extrusion is 170-230° C., the time of microwave cross-linking is 6-10s, and the power of microwave cross-linking is 600-800W.