Preparation method of electromagnetic shielding optical cable
By using modified graphite aerogel and a multi-layer shielding layer in optical cables, the problem of insufficient shielding performance of optical cables in high temperature and electromagnetic environments is solved, high heat resistance and electromagnetic shielding performance are improved, and it is suitable for high-temperature applications. technology field.
Patent Information
- Application Number
- CN202410684215.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-08
- Publication Date
- 2024-10-22
AI Technical Summary
Existing optical cables lack effective shielding performance in high temperature and electromagnetic environments, making it difficult to meet the special application requirements in high-tech fields.
Modified graphite aerogel is used as the sheath layer, and pyrrolidone microspheres are introduced between the graphene layers, combined with the melamine foam layer, foam metal layer and carbon fiber to form a porous structure and tightly connected shielding layer to enhance the heat resistance of the optical cable. and electromagnetic shielding performance.
It achieves high heat resistance, mechanical strength and electromagnetic shielding performance of the optical cable, significantly improves the overall performance of the optical cable, and is suitable for high temperature and electromagnetic environments.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of communication optical cables, and in particular to a method for preparing an electromagnetic shielding optical cable. Background Art
[0002] Optical cables are manufactured to meet optical, mechanical or environmental performance specifications. They are communication cable components that use one or more optical fibers placed in a sheath as transmission media and can be used individually or in groups. Optical cables are mainly composed of optical fibers and plastic protective sleeves and plastic sheaths. They are not only widely used in conventional communications, but also in other high-tech fields such as sensing, measurement, control, data acquisition, such as mining industry, aerospace industry, military, oil and gas, and high-temperature medical applications. These fields involve some special application environments, such as high temperature environment, electromagnetic environment, etc.
[0003] However, most of the current research on optical cables is focused on heat resistance and flame retardancy, and little attention is paid to optical cables used in the field of electromagnetic shielding. Therefore, this application studies and prepares an optical cable with good heat resistance, high strength and high electromagnetic shielding properties. Summary of the invention
[0004] The object of the present invention is to provide an electromagnetic shielding optical cable and a preparation method thereof to solve the problems raised in the above background technology.
[0005] An electromagnetic shielding optical cable comprises a sheath layer, a shielding layer and a cable core from the outside to the inside, characterized in that the sheath layer is modified graphite aerogel; and the cable core is an optical fiber.
[0006] Preferably, the modified graphite aerogel is prepared by introducing pyrrolidone microspheres between graphene layers; the pyrrolidone microspheres are prepared by reacting maleic anhydride, N-vinyl pyrrolidone and vinyl cyclohexyl ether.
[0007] Preferably, the shielding layer comprises a melamine foam layer, a foam metal layer and carbon fiber.
[0008] Preferably, the carbon fiber is prepared by pre-oxidation and carbonization after wet spinning of polyacrylonitrile; the foam metal layer is prepared by in-situ reduction of nickel sulfate, hydrazine hydrate and hexadecyltrimethylammonium bromide on the carbon fiber; the melamine foam layer is prepared by coating the foam metal layer with melamine formaldehyde resin etherified with hexafluorobutanol and foaming it.
[0009] Preferably, the method for preparing the electromagnetic shielding optical cable comprises the following specific steps: (1) Dispersing graphene oxide in deionized water with a mass of 30 to 50 times that of graphene oxide, ultrasonically dispersing it at 100 to 150 kHz for 20 to 30 minutes, adding pyrrolidone microspheres with a mass of 0.25 to 0.35 times that of graphene oxide, and continuing ultrasonically dispersing it for 20 to 30 minutes, transferring it to a hydrothermal reactor, reacting it at 180 to 200°C for 12 to 16 hours, and freeze-drying it in a freeze dryer at -50 to -60°C, and finally heat treating it at 800 to 900°C for 2 to 3 hours to obtain a modified graphite aerogel; (2) Disperse nickel acetate in deionized water with a mass fraction of 30 to 40 times the mass of nickel acetate, stir evenly, add hydrazine hydrate with a mass fraction of 80 to 85% with a mass fraction of 3 to 5 times the mass of nickel acetate, and stir at 30 to 50 rpm for 0.5 to 1 hour to prepare a nickel acetate solution; soak the carbon fiber precursor in a nitric acid solution with a mass fraction of 60 to 70%, heat it to 80 to 90°C, react for 1 to 2 hours, remove it, rinse it with deionized water for 3 to 5 minutes, wipe it dry and stretch it to a diameter of 0.06 to 0.08 mm, Transfer to a hydrothermal reactor, add 3-5% glutamic acid solution with a mass fraction of 5-10 times the mass of carbon fiber precursor, heat to 160-180°C for reaction for 0.5-1h, then add nickel acetate solution with a mass fraction of 20-25 times the mass of carbon fiber precursor and hexadecyltrimethylammonium bromide with a mass fraction of 0.15-0.25 times the mass of carbon fiber precursor, continue to react for 6-8h, transfer to a carbonization furnace, carbonize at 500-1000°C for 3-5h under a nitrogen atmosphere to obtain a carbon fiber with a foam metal layer; (3) Soak the carbon fiber with the foam metal layer in etherified melamine, add sodium dodecylbenzene sulfonate at a mass of 0.01 to 0.04 times the mass of the etherified melamine, stir at 2000 to 2500 rpm for 2 to 5 minutes, then add n-pentane at a mass of 0.02 to 0.04 times the mass of the etherified melamine as a foaming agent and oxalic acid at a mass of 0.08 to 0.1 times the mass of the etherified melamine as a catalyst, continue stirring for 5 to 8 seconds, fish out the carbon fiber with the foam metal layer, wrap the cable core, and place it in a mold preheated at 90 to 100 ° C for 3 to 5 minutes, seal it and place it in a carbon fiber oven with a foam metal layer for foaming and curing, take it out after 2 to 3 hours, and finally dry it in a drying oven for 24 to 48 hours to obtain a cable core with a shielding layer; (4) The modified graphite aerogel, polyamide and epoxy resin are mixed in a mass ratio of 2:0.5:6~3:0.8:8 and placed in a screw extruder. The mixture is melt-extruded on the surface of the cable core with a shielding layer. The melt temperature is 315~355°C and the thickness of the sheath layer is 0.05~0.15mm. The mixture is transferred to a drying oven and dried at 60~80°C for 5~6h to obtain an electromagnetic shielding optical cable.
[0010] Preferably, in the above step (1): the preparation method of pyrrolidone microspheres is: maleic anhydride, azobisisobutyronitrile and Freon 225 are mixed in a mass ratio of 2:0.15:10-4:0.2:15, and N-vinyl pyrrolidone with a mass ratio of 0.8-1.2 times of maleic anhydride, vinyl cyclohexyl ether with a mass ratio of 0.5-0.8 times of maleic anhydride and cross-linking agent divinylbenzene with a mass ratio of 0.02-0.05 times of maleic anhydride are added in sequence, stirring until the solution is clear, replacing the air with nitrogen, heating to 60-62°C under a nitrogen atmosphere, reacting for 6-8h, ultrasonically dispersing at 100-200kHz for 2-3min and Soxhlet purification with acetone for 36-48h, and finally drying in a vacuum drying oven at 45-55°C to constant weight to obtain pyrrolidone microspheres.
[0011] Preferably, in the above step (2): the preparation method of carbon fiber precursor is: polyacrylonitrile and dimethyl diamide are mixed in a mass ratio of 1:10~3:10, heated to 85~100°C, and mixed for 0.5~1h under the assistance of 200~300W microwave, and then 0.1~0.2 times the mass of polyacrylonitrile propylene glycol and 0.05~0.15 times the mass of polyacrylonitrile thiourea are added, mixed evenly, to obtain a spinning solution, and wet electrospinning is performed at 70~90°C, and the coagulation temperature is 5~15°C to obtain carbon fiber precursor.
[0012] Preferably, in the above step (3): the preparation method of etherified melamine is: melamine, paraformaldehyde and triethylamine are mixed in a mass ratio of 1:6:20 to 1:8:40, the temperature is raised to 90 to 95°C, and after complete dissolution, the temperature is kept warm for 1 to 2 hours, hexafluorobutanol in an amount of 0.15 to 0.3 times the mass of melamine is added, and the pH is adjusted to 5.2 to 5.5 with nitric acid, the temperature is maintained at 90 to 95°C, the reaction is carried out for 12 to 24 hours, and the pH is adjusted to 8 to 9 with triethylamine to obtain etherified melamine.
[0013] Preferably, in the above step (3): the cable core is an optical fiber with a diameter of 0.2-0.5 mm.
[0014] Preferably, in the above step (4), the thickness of the shielding layer is 0.1 to 0.2 mm.
[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: The electromagnetic shielding optical cable prepared by the present invention comprises a sheath layer, a shielding layer and a cable core from outside to inside; the sheath layer is an epoxy resin added with modified graphite aerogel; the shielding layer comprises a melamine foam layer, a foam metal layer and carbon fiber; Modified graphite aerogel is prepared by introducing pyrrolidone microspheres between graphene layers; pyrrolidone microspheres are prepared by the reaction of maleic anhydride, N-vinyl pyrrolidone and vinyl cyclohexyl ether, and contain anhydride and lactam groups on the surface, and have a cross-linked structure inside. The addition of epoxy resin enhances the heat resistance of the sheath layer; pyrrolidone microspheres are attached to graphene, so that the modified graphite aerogel has a porous structure and an interconnected three-dimensional network structure, which can not only disperse the external force, but also improve the mechanical strength of the sheath layer, and also have electromagnetic shielding performance; the modified graphite aerogel between the sheath layer and the shielding layer can also react with the melamine foam layer to tightly connect the sheath layer and the shielding layer, thereby enhancing the strength of the optical cable; The shielding layer is prepared by depositing foamed metal on the surface of carbon fiber and then coating it with foamed etherified melamine resin; a molecular film containing oxygen and nitrogen groups is coated on the surface of carbon fiber precursor obtained by wet spinning of polyacrylonitrile, and pre-oxidation is carried out in a hydrothermal reactor, and nickel sulfate, hydrazine hydrate and hexadecyltrimethylammonium bromide are added to in-situ reduce the carbon fiber surface to generate foamed metal nickel, and then the surface is coated with melamine formaldehyde resin etherified by hexafluorobutanol, and foaming forms a melamine foam layer; Glutamic acid introduces carboxyl groups on the surface of carbon fiber and forms a molecular film containing oxygen and nitrogen groups, and during pre-oxidation, the carbon fiber can absorb nickel ions and in-situ reduce the metal nickel with a foamed cubic crystal structure on the surface to tightly adsorb the foamed metal nickel on the surface of the molecular film containing oxygen and nitrogen groups, and the added hexadecyltrimethylammonium bromide not only forms an ion layer on the surface of nickel particles, but also prevents the agglomeration of metal nickel particles, reduces the average diameter of the chain, increases the porosity of the foamed metal nickel, enables electromagnetic waves to be reflected in the holes inside the shielding layer, and enhances the electromagnetic shielding property of the optical cable. DETAILED DESCRIPTION
[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the electromagnetic shielding optical cables prepared in the examples and comparative examples as follows: Heat resistance: The examples and comparative examples were subjected to limiting oxygen index test according to GB / T2406; Mechanical properties: The examples and comparative examples were tested for elongation at break and tensile strength according to GB / T 2951.42.
[0018] Electromagnetic shielding property: The electromagnetic shielding effectiveness of the embodiments and comparative examples was tested according to GB / T30142.
[0019] Example 1 (1) Maleic anhydride, azobisisobutyronitrile and Freon 225 were mixed at a mass ratio of 2:0.15:10, and N-vinyl pyrrolidone (0.8 times the mass of maleic anhydride), vinyl cyclohexyl ether (0.5 times the mass of maleic anhydride) and cross-linking agent divinylbenzene (0.02 times the mass of maleic anhydride) were added in sequence. After stirring until the solution was clear, nitrogen was passed to replace the air. The temperature was raised to 60°C under a nitrogen atmosphere. After reacting for 6 hours, ultrasonic dispersion was performed at 100 kHz for 2 minutes and Soxhlet purification was performed with acetone for 36 hours. The mixture was placed in a vacuum drying oven at 45°C and dried to a constant weight to obtain pyrrolidone microspheres; the graphene oxide was dispersed in deionized water 30 times the mass of the graphene oxide, and ultrasonically dispersed at 100kHz for 20 minutes, and pyrrolidone microspheres 0.25 times the mass of the graphene oxide were added, and ultrasonic dispersion was continued for 20 minutes, and the mixture was transferred to a hydrothermal reactor, reacted at 180°C for 12 hours, and freeze-dried in a freeze dryer at -50°C, and finally heat-treated at 800°C for 2 hours to obtain a modified graphite aerogel; (2) Polyacrylonitrile and dimethyl diamide were mixed in a mass ratio of 1:10, heated to 85°C, and mixed for 0.5 h under the assistance of a 200 W microwave. Then, 0.1 times the mass of polyacrylonitrile of propylene glycol and 0.05 times the mass of polyacrylonitrile of thiourea were added and mixed evenly to obtain a spinning solution. Wet electrospinning was performed at 70°C with a coagulation temperature of 5°C to obtain carbon fiber precursor. Nickel acetate was dispersed in deionized water with a mass of 30 times the mass of nickel acetate. After stirring evenly, 80% hydrazine hydrate with a mass fraction of 3 times the mass of nickel acetate was added and stirred at 30 rpm for 0.5 h to obtain a nickel acetate solution. The fibers were immersed in a nitric acid solution with a mass fraction of 60%, heated to 80°C for reaction for 1 hour, taken out and rinsed with deionized water for 3 minutes, wiped dry and stretched to a diameter of 0.06 mm, transferred to a hydrothermal reactor, and a glutamic acid solution with a mass fraction of 3% 5 times the mass of the carbon fiber precursor was added. The temperature was raised to 160°C for reaction for 0.5 hours, and then a nickel acetate solution with a mass fraction of 20 times the mass of the carbon fiber precursor and a hexadecyltrimethylammonium bromide with a mass fraction of 0.15 times the mass of the carbon fiber precursor were added. The reaction continued for 6 hours, and the fibers were transferred to a carbonization furnace and carbonized at 500°C for 3 hours under a nitrogen atmosphere to obtain a carbon fiber with a foam metal layer. (3) Melamine, paraformaldehyde and triethylamine were mixed in a mass ratio of 1:6:20, heated to 90°C, and kept warm for 1 hour after they were completely dissolved. Hexafluorobutanol (0.15 times the mass of melamine) was added, and the pH was adjusted to 5.2 with nitric acid. The temperature was kept at 90°C and reacted for 12 hours. The pH was then adjusted to 8 with triethylamine to obtain etherified melamine. The carbon fiber with the foam metal layer was immersed in the etherified melamine, and sodium dodecylbenzene sulfonate (0.01 times the mass of etherified melamine) was added. The mixture was stirred at 2000 rpm. Stir for 2 minutes, then add 0.02 times the mass of etherified melamine as a foaming agent, n-pentane, and 0.08 times the mass of etherified melamine as a catalyst, oxalic acid, and continue stirring for 5 seconds. Then, fish out the carbon fiber with the foam metal layer, coat an optical fiber with a diameter of 0.2 mm, and place it in a mold preheated at 90°C for 3 minutes, seal it and place it in a carbon fiber oven with a foam metal layer for foaming and curing, take it out after 2 hours, and finally dry it in a drying oven for 24 hours to obtain a cable core with a shielding layer, and the thickness of the shielding layer is 0.1 mm; (4) The modified graphite aerogel, polyamide and epoxy resin were mixed in a mass ratio of 2:0.5:6 and placed in a screw extruder. The mixture was melt-extruded on the surface of the cable core with a shielding layer. The melt temperature was 315°C and the thickness of the sheath layer was 0.05 mm. The mixture was transferred to a drying oven and dried at 60°C for 5 h to obtain an electromagnetic shielding optical cable.
[0020] Example 2 (1) Maleic anhydride, azobisisobutyronitrile and Freon 225 were mixed in a ratio of 3:0.18:13 by weight, and N-vinyl pyrrolidone (1.1 times the weight of maleic anhydride), vinyl cyclohexyl ether (0.6 times the weight of maleic anhydride) and crosslinking agent divinylbenzene (0.04 times the weight of maleic anhydride) were added in sequence. The solution was stirred until it became clear, and then nitrogen was introduced to replace the air. The temperature was raised to 61°C under a nitrogen atmosphere, and the reaction was continued for 7 hours. The solution was then ultrasonically dispersed at 150 kHz for 4 minutes and purified by Soxhlet with acetone for 42 hours. The mixture was then placed in a vacuum drying oven at 50°C and dried to a constant weight to obtain pyrrolidone microspheres; graphene oxide was dispersed in deionized water 40 times the mass of graphene oxide, ultrasonically dispersed at 130kHz for 25 minutes, pyrrolidone microspheres 0.3 times the mass of graphene oxide were added, and ultrasonic dispersion was continued for 25 minutes, and the mixture was transferred to a hydrothermal reactor, reacted at 190°C for 14 hours, and freeze-dried in a freeze dryer at -55°C, and finally heat treated at 850°C for 2 hours to obtain modified graphite aerogel; (2) Polyacrylonitrile and dimethyl diamide were mixed in a mass ratio of 2:10, heated to 90°C, and mixed for 0.5h under the assistance of a 250W microwave. Then, 0.15 times the mass of polyacrylonitrile of propylene glycol and 0.01 times the mass of polyacrylonitrile of thiourea were added and mixed evenly to obtain a spinning solution. Wet electrospinning was performed at 80°C with a coagulation temperature of 10°C to obtain carbon fiber precursor. Nickel acetate was dispersed in deionized water with a mass of 35 times the mass of nickel acetate. After stirring evenly, hydrazine hydrate with a mass fraction of 83% and a mass fraction of 4 times the mass of nickel acetate was added and stirred at 40rpm for 0.5h to obtain a nickel acetate solution. The carbon fiber precursor was immersed in a nitric acid solution with a mass fraction of 65%, heated to 85°C for reaction for 1 hour, taken out and rinsed with deionized water for 4 minutes, wiped dry and stretched to a diameter of 0.07 mm, transferred to a hydrothermal reactor, and a 4% glutamic acid solution with a mass fraction of 7 times the mass of the carbon fiber precursor was added. After heating to 170°C for reaction for 0.5 hours, a nickel acetate solution with a mass fraction of 23 times the mass of the carbon fiber precursor and hexadecyltrimethylammonium bromide with a mass fraction of 0.2 times the mass of the carbon fiber precursor were added, and the reaction was continued for 7 hours. The carbon fiber was transferred to a carbonization furnace and carbonized at 700°C for 4 hours under a nitrogen atmosphere to obtain a carbon fiber with a foam metal layer. (3) Melamine, paraformaldehyde and triethylamine were mixed in a mass ratio of 1:7:30, heated to 94°C, and kept warm for 1 hour after they were completely dissolved. Hexafluorobutanol (0.22 times the mass of melamine) was added, and the pH was adjusted to 5.4 with nitric acid. The temperature was kept at 93°C and reacted for 18 hours. The pH was then adjusted to 8.5 with triethylamine to obtain etherified melamine. The carbon fiber with the foam metal layer was immersed in the etherified melamine, and sodium dodecylbenzene sulfonate (0.03 times the mass of etherified melamine) was added. The mixture was stirred at 2200 rpm. Stir for 4 minutes, then add 0.03 times the mass of etherified melamine as a foaming agent, n-pentane, and 0.09 times the mass of etherified melamine as a catalyst, oxalic acid, and continue stirring for 6 seconds, then fish out the carbon fiber with the foam metal layer, coat an optical fiber with a diameter of 0.3 mm, and place it in a mold preheated at 95°C for 4 minutes, seal it and place it in a carbon fiber oven with a foam metal layer for foaming and curing, take it out after 2.5 hours, and finally dry it in a drying oven for 36 hours to obtain a cable core with a shielding layer, and the thickness of the shielding layer is 0.5 mm; (4) The modified graphite aerogel, polyamide and epoxy resin were mixed in a mass ratio of 2:0.6:7 and placed in a screw extruder. The mixture was melt-extruded on the surface of the cable core with a shielding layer. The melt temperature was 335°C and the thickness of the sheath layer was 0.1 mm. The mixture was transferred to a drying oven and dried at 70°C for 5 h to obtain an electromagnetic shielding optical cable.
[0021] Example 3 (1) Maleic anhydride, azobisisobutyronitrile and Freon 225 were mixed in a ratio of 4:0.2:15 by weight, and N-vinyl pyrrolidone (1.2 times the weight of maleic anhydride), vinyl cyclohexyl ether (0.8 times the weight of maleic anhydride) and crosslinking agent divinylbenzene (0.05 times the weight of maleic anhydride) were added in sequence. After stirring until the solution was clear, nitrogen was passed to replace the air. The temperature was raised to 62°C under a nitrogen atmosphere. After reacting for 8 hours, ultrasonic dispersion was performed at 200 kHz for 3 minutes and Soxhlet purification was performed with acetone for 48 hours. The mixture was placed in a vacuum drying oven at 55°C and dried to a constant weight to obtain pyrrolidone microspheres; graphene oxide was dispersed in deionized water 50 times the mass of graphene oxide, ultrasonically dispersed at 150kHz for 30 minutes, pyrrolidone microspheres 0.35 times the mass of graphene oxide were added, and ultrasonic dispersion was continued for 30 minutes, and the mixture was transferred to a hydrothermal reactor, reacted at 200°C for 16 hours, and freeze-dried in a freeze dryer at -60°C, and finally heat-treated at 900°C for 3 hours to obtain modified graphite aerogel; (2) Polyacrylonitrile and dimethyl diamide were mixed in a mass ratio of 3:10, heated to 100°C, and mixed for 1 hour under the assistance of a 300 W microwave. Then, 0.2 times the mass of polyacrylonitrile of propylene glycol and 0.15 times the mass of polyacrylonitrile of thiourea were added and mixed evenly to obtain a spinning solution. Wet electrospinning was carried out at 90°C and the coagulation temperature was 15°C to obtain carbon fiber precursor. Nickel acetate was dispersed in deionized water with a mass of 40 times the mass of nickel acetate. After stirring evenly, hydrazine hydrate with a mass fraction of 85% was added with a mass fraction of 5 times the mass of nickel acetate, and stirred at 50 rpm for 1 hour to obtain a nickel acetate solution. The carbon fiber precursor was prepared. Soak in a 70% nitric acid solution, heat to 90°C and react for 2 hours, take out and rinse with deionized water for 5 minutes, wipe dry and stretch to a diameter of 0.08 mm, transfer to a hydrothermal reactor, add a 5% glutamic acid solution with a mass fraction of 10 times the mass of the carbon fiber precursor, heat to 180°C and react for 1 hour, then add a nickel acetate solution with a mass fraction of 25 times the mass of the carbon fiber precursor and hexadecyltrimethylammonium bromide with a mass fraction of 0.25 times the mass of the carbon fiber precursor, continue to react for 8 hours, transfer to a carbonization furnace, and carbonize at 1000°C for 35 hours under a nitrogen atmosphere to obtain a carbon fiber with a foam metal layer; (3) Melamine, paraformaldehyde and triethylamine were mixed in a mass ratio of 1:8:40, heated to 95°C, and kept warm for 2 hours after they were completely dissolved. Hexafluorobutanol (0.3 times the mass of melamine) was added, and the pH was adjusted to 5.5 with nitric acid. The temperature was kept at 95°C and reacted for 24 hours. The pH was then adjusted to 9 with triethylamine to obtain etherified melamine. The carbon fiber with the foam metal layer was immersed in the etherified melamine, and sodium dodecylbenzene sulfonate (0.04 times the mass of etherified melamine) was added. The mixture was stirred at 2500 rpm. Stir for 5 minutes, then add 0.04 times the mass of etherified melamine as a foaming agent, n-pentane, and 0.1 times the mass of etherified melamine as a catalyst, oxalic acid, and continue stirring for 8 seconds. Then, fish out the carbon fiber with the foam metal layer, coat an optical fiber with a diameter of 0.5 mm, and place it in a mold preheated at 100°C for 5 minutes, seal it and place it in a carbon fiber oven with a foam metal layer for foaming and curing, take it out after 3 hours, and finally dry it in a drying oven for 48 hours to obtain a cable core with a shielding layer, and the thickness of the shielding layer is 0.2 mm; (4) The modified graphite aerogel, polyamide and epoxy resin were mixed in a mass ratio of 3:0.8:8 and placed in a screw extruder. The mixture was melt-extruded on the surface of the cable core with a shielding layer. The melt temperature was 355°C and the thickness of the sheath layer was 0.15 mm. The mixture was transferred to a drying oven and dried at 80°C for 6 h to obtain an electromagnetic shielding optical cable.
[0022] Comparative Example 1 The formulation composition of Comparative Example 1 is the same as that of Example 2. The difference between the preparation method of the electromagnetic shielding optical cable and Example 2 is only the difference in step (1), and step (1) is modified as follows: dispersing graphene oxide in deionized water with a mass 40 times that of graphene oxide, ultrasonically dispersing at 130 kHz for 50 min, transferring to a hydrothermal reactor, reacting at 190° C. for 14 h, freeze-drying in a freeze dryer at -55° C., and finally heat-treating at 850° C. for 2 h to obtain a modified graphite aerogel.
[0023] Comparative Example 2 The formulation composition of Comparative Example 2 is the same as that of Example 2. The preparation method of the electromagnetic shielding optical cable differs from that of Example 2 only in steps (1) (4). Steps (1) (4) are modified as follows: (1) maleic anhydride, azobisisobutyronitrile and Freon 225 are mixed at a mass ratio of 3:0.18:13, and N-vinyl pyrrolidone with a mass ratio of 1.1 times that of maleic anhydride, vinyl cyclohexyl ether with a mass ratio of 0.6 times that of maleic anhydride and cross-linking agent divinylbenzene with a mass ratio of 0.04 times that of maleic anhydride are added in sequence, and the solution is stirred until it becomes clear, and then nitrogen is passed to replace the air, and the temperature is raised to 61°C under a nitrogen atmosphere, and after reacting for 7 hours, ultrasonic dispersion is performed at 150kHz for 4 minutes and Soxhlet purification is performed with acetone for 42 hours, and finally the solution is dried in a vacuum drying oven at 50°C to constant weight to prepare a product. Pyrrolidone microspheres were obtained; graphene oxide was dispersed in deionized water with a mass 40 times that of graphene oxide, ultrasonically dispersed at 130 kHz for 50 minutes, transferred to a hydrothermal reactor, reacted at 190°C for 14 hours, freeze-dried in a freeze dryer at -55°C, and finally heat treated at 850°C for 2 hours to obtain modified graphite aerogel; (4) pyrrolidone microspheres, modified graphite aerogel, polyamide and epoxy resin were mixed in a mass ratio of 0.5:1.5:0.6:7 and placed in a screw extruder, melt-extruded on the surface of a cable core with a shielding layer, the melt temperature was 335°C, the sheath layer thickness was 0.1 mm, transferred to a drying oven, and dried at 70°C for 5 hours to obtain an electromagnetic shielding optical cable.
[0024] Comparative Example 3 The formulation composition of Comparative Example 3 is the same as that of Example 2. The preparation method of the electromagnetic shielding optical cable is different from that of Example 2 only in that the treatment of step (1) is not performed, and step (4) is modified as follows: polyamide and epoxy resin are mixed in a mass ratio of 0.6:7 and placed in a screw extruder, melt-extruded on the surface of the cable core with a shielding layer, the melt temperature is 335°C, the thickness of the sheath layer is 0.1mm, transferred to a drying box, and dried at 70°C for 5h to obtain an electromagnetic shielding optical cable.
[0025] Comparative Example 4 The prescription composition of comparative example 4 is the same as that of example 2. The preparation method of the electromagnetic shielding optical cable is different from that of example 2 only in step (3), which is modified as follows: an optical fiber with a diameter of 0.5 mm is coated with a carbon fiber with a foam metal layer to obtain a cable core with a shielding layer, and the thickness of the shielding layer is 0.2 mm.
[0026] Comparative Example 5 The formulation composition of comparative example 5 is the same as that of example 2. The preparation method of the electromagnetic shielding optical cable is different from that of example 2 only in step (2), which is modified as follows: polyacrylonitrile and dimethyl diamide are mixed in a mass ratio of 2:10, heated to 90°C, and mixed for 0.5h under the assistance of a 250W microwave, and then 0.15 times the mass of polyacrylonitrile of propylene glycol and 0.01 times the mass of polyacrylonitrile of thiourea are added, mixed evenly, and a spinning solution is obtained, and wet electrospinning is performed at 80°C, and the coagulation temperature is 10°C to obtain a spinning solution. Carbon fiber precursor: The carbon fiber precursor was immersed in a nitric acid solution with a mass fraction of 65%, heated to 85°C for reaction for 1 hour, taken out and rinsed with deionized water for 4 minutes, wiped dry and stretched to a diameter of 0.07 mm, transferred to a hydrothermal reactor, and a 4% glutamic acid solution with a mass fraction of 7 times the mass of the carbon fiber precursor was added, heated to 170°C for reaction for 0.5 hours, and then transferred to a carbonization furnace, and carbonized at 700°C for 4 hours under a nitrogen atmosphere to obtain a carbon fiber with a foam metal layer.
[0027] Comparative Example 6 (1) Maleic anhydride, azobisisobutyronitrile and Freon 225 were mixed in a ratio of 3:0.18:13 by weight, and N-vinyl pyrrolidone (1.1 times the weight of maleic anhydride), vinyl cyclohexyl ether (0.6 times the weight of maleic anhydride) and crosslinking agent divinylbenzene (0.04 times the weight of maleic anhydride) were added in sequence. The solution was stirred until it became clear, and then nitrogen was introduced to replace the air. The temperature was raised to 61°C under a nitrogen atmosphere, and the reaction was continued for 7 hours. The solution was then ultrasonically dispersed at 150 kHz for 4 minutes and purified by Soxhlet with acetone for 42 hours. The mixture was then placed in a vacuum drying oven at 50°C and dried to a constant weight to obtain pyrrolidone microspheres; graphene oxide was dispersed in deionized water 40 times the mass of graphene oxide, ultrasonically dispersed at 130kHz for 25 minutes, pyrrolidone microspheres 0.3 times the mass of graphene oxide were added, and ultrasonic dispersion was continued for 25 minutes, and the mixture was transferred to a hydrothermal reactor, reacted at 190°C for 14 hours, and freeze-dried in a freeze dryer at -55°C, and finally heat treated at 850°C for 2 hours to obtain modified graphite aerogel; (2) The modified graphite aerogel, polyamide and epoxy resin were mixed in a mass ratio of 2:0.6:7 and placed in a screw extruder. The mixture was melt-extruded on the surface of an optical fiber with a diameter of 0.5 mm. The melt temperature was 335°C and the sheath layer thickness was 0.1 mm. The mixture was transferred to a drying oven and dried at 70°C for 5 h to obtain an electromagnetic shielding optical cable.
[0028] Effect example Table 1 below shows the performance analysis results of the electromagnetic shielding optical cables using Examples 1, 2, 3 of the present invention and Comparative Examples 1, 2, 3, 4, 5, 6.
[0029] Table 1 Oxygen index (%) Tensile strength (MPa) Elongation at break (%) Electromagnetic shielding (dB) Example 1 42 158 11.3 69 Example 2 43 160 10.7 65 Example 3 41 155 10.9 68 Comparative Example 1 35 141 8.5 55 Comparative Example 2 40 152 8.9 57 Comparative Example 3 31 135 8.1 55 Comparative Example 4 33 136 7.7 58 Comparative Example 5 36 136 7.4 53 Comparative Example 6 28 125 6.8 51 By comparing the experimental data of the embodiments and the comparative examples in Table 1, it can be clearly found that the electromagnetic shielding optical cables prepared in Examples 1, 2, and 3 have better heat resistance, mechanical properties, and electromagnetic shielding properties; From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Examples 1, 2, 3, it can be found that the modified graphite aerogel obtained by introducing pyrrolidone microspheres between graphene layers has a cross-linked structure inside, and the addition of epoxy resin enhances the heat resistance of the sheath layer, so that the modified graphite aerogel has a porous structure and an interconnected three-dimensional network structure, which improves the mechanical strength of the sheath layer and also has electromagnetic shielding performance, and the sheath layer and the shielding layer are tightly connected to enhance the strength of the optical cable; from the comparison of the experimental data of Examples 1, 2, 3 and Comparative Examples 4, 5, 6, it can be found that by depositing foamed metal on the surface of the carbon fiber and then coating the shielding layer made of foamed etherified melamine resin, electromagnetic waves can be reflected in the holes inside the shielding layer, thereby enhancing the electromagnetic shielding property of the optical cable.
[0030] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing an electromagnetic shielding optical cable, characterized in that: The method for preparing the electromagnetic shielding optical cable comprises the following specific steps: (1) Maleic anhydride, azobisisobutyronitrile and Freon 225 were mixed in a ratio of 3:0.18:13 by weight, and N-vinyl pyrrolidone (1.1 times the weight of maleic anhydride), vinyl cyclohexyl ether (0.6 times the weight of maleic anhydride) and crosslinking agent divinylbenzene (0.04 times the weight of maleic anhydride) were added in sequence. The solution was stirred until it became clear, and then nitrogen was introduced to replace the air. The temperature was raised to 61°C under a nitrogen atmosphere, and the reaction was continued for 7 hours. The solution was then ultrasonically dispersed at 150 kHz for 4 minutes and purified by Soxhlet with acetone for 42 hours. The mixture was then placed in a vacuum drying oven at 50°C and dried to a constant weight to obtain pyrrolidone microspheres; graphene oxide was dispersed in deionized water 40 times the mass of graphene oxide, ultrasonically dispersed at 130kHz for 25 minutes, pyrrolidone microspheres 0.3 times the mass of graphene oxide were added, and ultrasonic dispersion was continued for 25 minutes, and the mixture was transferred to a hydrothermal reactor, reacted at 190°C for 14 hours, and freeze-dried in a freeze dryer at -55°C, and finally heat treated at 850°C for 2 hours to obtain modified graphite aerogel; (2) Polyacrylonitrile and dimethyl diamide were mixed in a mass ratio of 2:10, heated to 90°C, and mixed for 0.5h under the assistance of a 250W microwave. Then, 0.15 times the mass of polyacrylonitrile of propylene glycol and 0.01 times the mass of polyacrylonitrile of thiourea were added and mixed evenly to obtain a spinning solution. Wet electrospinning was performed at 80°C with a coagulation temperature of 10°C to obtain carbon fiber precursor. Nickel acetate was dispersed in deionized water with a mass of 35 times the mass of nickel acetate. After stirring evenly, hydrazine hydrate with a mass fraction of 83% and a mass fraction of 4 times the mass of nickel acetate was added and stirred at 40rpm for 0.5h to obtain a nickel acetate solution. The carbon fiber precursor was immersed in a nitric acid solution with a mass fraction of 65%, heated to 85°C for reaction for 1 hour, taken out and rinsed with deionized water for 4 minutes, wiped dry and stretched to a diameter of 0.07 mm, transferred to a hydrothermal reactor, and a 4% glutamic acid solution with a mass fraction of 7 times the mass of the carbon fiber precursor was added. After heating to 170°C for reaction for 0.5 hours, a nickel acetate solution with a mass fraction of 23 times the mass of the carbon fiber precursor and hexadecyltrimethylammonium bromide with a mass fraction of 0.2 times the mass of the carbon fiber precursor were added, and the reaction was continued for 7 hours. The carbon fiber was transferred to a carbonization furnace and carbonized at 700°C for 4 hours under a nitrogen atmosphere to obtain a carbon fiber with a foam metal layer. (3) Melamine, paraformaldehyde and triethylamine were mixed in a mass ratio of 1:7:30, heated to 94°C, and kept warm for 1 hour after they were completely dissolved. Hexafluorobutanol (0.22 times the mass of melamine) was added, and the pH was adjusted to 5.4 with nitric acid. The temperature was kept at 93°C and reacted for 18 hours. The pH was then adjusted to 8.5 with triethylamine to obtain etherified melamine. The carbon fiber with the foam metal layer was immersed in the etherified melamine, and sodium dodecylbenzene sulfonate (0.03 times the mass of etherified melamine) was added. The mixture was stirred at 2200 rpm. Stir for 4 minutes, then add 0.03 times the mass of etherified melamine as a foaming agent, n-pentane, and 0.09 times the mass of etherified melamine as a catalyst, oxalic acid, and continue stirring for 6 seconds, then fish out the carbon fiber with the foam metal layer, coat an optical fiber with a diameter of 0.3 mm, and place it in a mold preheated at 95°C for 4 minutes, seal it and place it in a carbon fiber oven with a foam metal layer for foaming and curing, take it out after 2.5 hours, and finally dry it in a drying oven for 36 hours to obtain a cable core with a shielding layer, and the thickness of the shielding layer is 0.5 mm; (4) The modified graphite aerogel, polyamide and epoxy resin were mixed in a mass ratio of 2:0.6:7 and placed in a screw extruder. The mixture was melt-extruded on the surface of the cable core with a shielding layer. The melt temperature was 335°C and the thickness of the sheath layer was 0.1 mm. The mixture was transferred to a drying oven and dried at 70°C for 5 h to obtain an electromagnetic shielding optical cable.