Method for preparing earth pressure balance shield muck improved slurry by using waste silty clay
By using waste silty clay and additives to prepare earth pressure balance shield soil improvement mud, the problem of high bentonite cost and low resource utilization rate is solved, the economic and environmental benefits of soil improvement are realized, and the technical requirements of construction are met. .
Patent Information
- Application Number
- CN202410840716.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-22
AI Technical Summary
In earth pressure balance shield construction, the existing muck modifier bentonite has high cost and low resource utilization, which leads to environmental pollution and economic waste, and it is difficult to effectively utilize the shield muck.
Waste silty clay is mixed with water and additives (such as sodium carbonate or sodium pyrophosphate). After 24 hours of hydration, the excavated water ratio is 9:11 or 1:1 and the additive concentration is 1% to 5%. Muck soil improvement mud can replace bentonite as a muck soil conditioner. It can be used to improve muck after removing impurities and screening.
The resource utilization of waste is realized, the cost of soil improvement is reduced, the environmental and economic benefits are improved, and the improved mud is improved to meet engineering technical requirements and improve construction efficiency.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of earth pressure balance shield construction, and in particular relates to a method for preparing earth pressure balance shield slag improved slurry by utilizing waste silty clay. Background Art
[0002] As a major underground construction method, shield construction has the advantages of fast construction speed, low environmental impact and high safety, and has been widely used in underground rail transit construction. The earth pressure balance shield (EPBS) achieves support for the working face and reaction to the groundwater pressure by applying a propulsion force to the ballast cut by the shield machine, thereby completing the excavation of the shield machine. The excavation slag as a supporting medium needs to have low shear strength, appropriate fluidity, and low permeability to ensure the stability of the working face and avoid water ingress when excavating below the groundwater level. Therefore, it is necessary to improve the shield slag so that the shield slag has stable properties to form uniform plastic flow. Otherwise, it will cause the shield to form a "mud cake", the cutterhead will wear, and it will be difficult to discharge slag, which will seriously affect the construction efficiency. In the construction process of the earth pressure balance shield, bentonite is often used as a slag improver, and the preparation of bentonite slurry as engineering slurry is very costly.
[0003] At present, a large amount of shield slag is discharged during the excavation of EPBS. The use of open-air stacking or landfilling will lead to soil and groundwater pollution and damage to the surrounding landscape and ecological environment. The annual output of shield slag in my country exceeds 119 million tons, but the actual utilization rate is less than 1%. Shield slag has significant environmental and economic benefits in resource utilization. Waste silty clay is the main shield slag of EPBS, and it is of great significance to expand the reuse channels of waste silty clay. Summary of the invention
[0004] The present invention provides a method for preparing earth pressure balance shield slag improved slurry by utilizing waste silty clay. The method can utilize the waste silty clay instead of bentonite as a soil conditioner to prepare earth pressure balance shield slag improved slurry, thereby realizing waste utilization, reducing costs, and having higher economic and environmental benefits.
[0005] The technical solution of the present invention is as follows:
[0006] The invention discloses a method for preparing improved slurry for earth pressure balance shield slag using waste silty clay, comprising mixing the waste silty clay with water and an admixture, and placing the mixture for 24 hours for hydration to prepare improved slag slurry with an excavation water ratio of 9:11 to 1:1 and an admixture concentration of 1% to 5%.
[0007] Furthermore, in the method for preparing earth pressure balance shield slag improved slurry using waste silty clay, the admixture is sodium carbonate or sodium pyrophosphate.
[0008] Furthermore, in the method of preparing earth pressure balance shield slag improved mud using waste silty clay, when the admixture is sodium carbonate, the slag improved mud is prepared with a soil-water ratio of 1:1 and an admixture concentration of 1% to 3%.
[0009] Furthermore, in the method of preparing earth pressure balance shield slag improved mud using waste silty clay, when the admixture is sodium pyrophosphate, the slag improved mud is prepared with a soil-water ratio of 9:11 and an admixture concentration of 3% to 5%.
[0010] Furthermore, the method for preparing earth pressure balance shield slag improved mud using waste silty clay, the preparation process of the waste silty clay is as follows: take EPBS tunnel silty clay slag, remove impurities therein, and dry it in a constant temperature oven at 105-110°C for 24 hours; after drying, cool the soil sample to room temperature and sieve it using a sieving instrument, and collect particles with a particle size less than 0.1 mm as raw materials.
[0011] Furthermore, in the method of preparing improved slurry for earth pressure balance shield slag using waste silty clay, during stirring and mixing: the speed of the mixer is 600 rpm, and the stirring time is 20 to 30 minutes.
[0012] Furthermore, the method for preparing earth pressure balance shield slag improved mud using waste silty clay, the slag improved mud is subjected to funnel viscosity, colloid rate, filtration loss, specific gravity physical property tests and rheological tests, and the test results are as follows: filtration loss <15ml, funnel viscosity is 40-90s, colloid rate>96, specific gravity is 1.1-1.5g / cm 3 , the rheological properties are in line with the use indicators of engineering mud and meet the engineering technical requirements.
[0013] Furthermore, in the method for preparing improved slurry for earth pressure balance shield slag using waste silty clay, the rheological properties of engineering slurry use indexes use the rheological properties of bentonite slurry with concentrations of 10% and 14% as upper and lower limits.
[0014] Furthermore, in the method for preparing earth pressure balance shield slag improved slurry using waste silty clay, the injection ratio of the slag improved slurry is 26% to 30% to meet the requirement of 180 to 210 mm slump of improved slag on site. The injection ratio of the slag improved slurry is the ratio of the slurry volume to the slag volume.
[0015] The beneficial effects of the present invention are as follows: the present invention can use waste silty clay to replace bentonite as a soil conditioner to prepare earth pressure balance shield slag improved mud, realizing waste utilization, reducing costs, and having high economic and environmental benefits. The present invention performs hydration for 24 hours when adding admixtures, and it is necessary to allow sufficient chemical reaction time between the admixtures and the waste silty clay mud particles. The large number of active groups and permanent negative charges on the surface of the waste silty clay particles will adsorb the Na in the admixtures. + , the metal cations on the particle surface and the Na + An ion replacement reaction occurs, forming a special electrostatic connection between the particle crystal layer and the metal ions, causing the structure of the mud particles to change and become more dispersed. DETAILED DESCRIPTION
[0016] Example 1
[0017] Prepare the slag improved mud with a soil-water ratio of 1:1 and an admixture concentration of 3%, and the admixture is sodium carbonate; after stirring and mixing, leave it for 24 hours to hydrate; the slag improved mud is subjected to funnel viscosity, colloid rate, filtration loss, specific gravity physical property tests and rheological tests. The test results are as follows: filtration loss <15ml, funnel viscosity 40~90s, colloid rate>96, specific gravity 1.1~1.5g / cm 3 , and its rheological properties are in line with the usage indicators of engineering mud. The physical and rheological properties of the slag improved mud under this ratio can meet the requirements of on-site construction.
[0018] The physical property tests and rheological tests are as follows:
[0019] Filtration loss: Use ZNS-2A medium-pressure dehydration meter to measure. Start timing when the first drop of filtrate flows out. After 30 minutes, the filtrate in the measuring cylinder is the filtration loss.
[0020] Funnel viscosity: Funnel viscosity is measured using a Russian funnel (Russian funnel time for 20°C water is 15±0.5s).
[0021] Colloid rate: Pour the slurry into a 100ml measuring cylinder, let it stand for 24 hours and read the sedimentation value. The ratio of the sedimentation to 100ml is the colloid rate.
[0022] Specific gravity: NB-1 slurry hydrometer is used to measure density (specific gravity is the ratio of the density of mud to the density of pure water at 3.98℃ under standard atmospheric pressure).
[0023] Rheological properties: measured by ZNN-D12D digital viscometer. Bentonite slurries with concentrations of 10% and 14% were selected as standards.
[0024] The on-site slag is improved by injecting slag improvement slurry at an injection ratio of 28% to 30%. The slump is in the range of 180mm to 220mm. The slag has good fluidity, plasticity and viscosity, and the improvement effect obviously meets the on-site construction requirements.
[0025] The slump test process is as follows: Stir the improved slag slurry and add a certain volume of slag into the slump cone in layers, with each layer height of about 50mm-100mm. After each layer of sample is placed, gently tap the outer wall of the slump cone to remove air and achieve uniform distribution. Open the jump valve to allow the improved slag to flow freely, and then close the valve. Slowly lift the slump cone to separate it from the slag sample and allow the slag to collapse freely. Record the height reached by the slump cone when it is separated, which is the slump.
[0026] Example 2
[0027] Prepare slag improved mud with a soil-water ratio of 9:11 and an admixture concentration of 3%, with the admixture being sodium pyrophosphate; after stirring and mixing, leave it for 24 hours to hydrate; the physical and rheological properties of the slag improved mud with this ratio can meet the requirements of on-site construction.
[0028] The on-site slag is improved by injecting slag improvement slurry at an injection ratio of 26% to 28%. The slump is in the range of 180mm to 220mm. The slag has good fluidity, plasticity and viscosity, and the improvement effect obviously meets the on-site construction requirements.
Claims
1. A method for preparing improved slurry for earth pressure balance shield using waste silty clay. It is characterized in that The waste silty clay is mixed with water and admixtures and left to hydrate for 24 hours to prepare the slag-improved mud with a soil-water ratio of 9:11 to 1:1 and an admixture concentration of 1% to 5%.
2. The method for preparing improved slurry for earth pressure balance shield using waste silty clay according to claim 1, It is characterized in that The additive is sodium carbonate or sodium pyrophosphate.
3. The method for preparing improved slurry for earth pressure balance shield using waste silty clay according to claim 2, It is characterized in that When the admixture is sodium carbonate, the slag improved mud is prepared with a soil-water ratio of 1:1 and an admixture concentration of 1% to 3%.
4. The method for preparing improved slurry for earth pressure balance shield using waste silty clay according to claim 2, It is characterized in that When the admixture is sodium pyrophosphate, the slag improved mud is prepared with a soil-water ratio of 9:11 and an admixture concentration of 3% to 5%.
5. The method for preparing improved slurry for earth pressure balance shield using waste silty clay according to claim 1, It is characterized in that The preparation process of waste silty clay is as follows: take the silty clay residue of the EPBS tunnel, remove impurities therein, and dry it in a constant temperature oven at 105-110°C for 24 hours; after drying, cool the soil sample to room temperature and sieve it using a sieving instrument, and collect particles with a particle size less than 0.1 mm as raw materials.
6. The method for preparing improved slurry for earth pressure balance shield using waste silty clay according to claim 1, It is characterized in that When stirring and mixing: the stirring speed is 600 rpm and the stirring time is 20 to 30 minutes.
7. The method for preparing improved slurry for earth pressure balance shield using waste silty clay according to claim 1, It is characterized in that The improved slag slurry was subjected to funnel viscosity, colloid rate, filtration loss, specific gravity physical property tests and rheological tests. The test results are as follows: filtration loss <15ml, funnel viscosity 40-90s, colloid rate >96, specific gravity 1.1-1.5g / cm 3 , the rheological properties are in line with the use indicators of engineering mud and meet the engineering technical requirements.
8. The method for preparing improved slurry for earth pressure balance shield using waste silty clay according to claim 7, It is characterized in that The engineering mud usage index of rheological properties uses the rheological properties of bentonite mud with concentrations of 10% and 14% as the upper and lower limits.
9. The method for preparing improved slurry for earth pressure balance shield using waste silty clay according to claim 1, It is characterized in that The injection ratio of the slag improvement slurry is 26% to 30% to meet the on-site improved slag slump requirement of 180 to 210 mm.