Method for adding iron and burdening in center of silicon iron heat furnace
By adding iron ingredients to the center of the ferrosilicon submersible furnace, using iron oxide scale and blue carbon to adjust the proportion of ingredients, destroying the SiC generated during the SiO2 reduction process, solving the problem of the dead zone caused by the carbon deficiency of the furnace material, and restoring the activity of the submerged furnace. , improve productivity and silicon recovery rate, reduce power consumption, and ensure long-term stable production.
Patent Information
- Application Number
- CN202410936018.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-22
AI Technical Summary
During the ferrosilicon smelting process, the carbon content of the furnace charge causes the reaction to lose balance and form a 'dead material zone', which makes the submerged arc furnace inactive, leading to reduced productivity, reduced silicon recovery rate, increased power consumption, fluctuations in product composition, and even The dead furnace phenomenon seriously affects economic benefits.
By adding iron ingredients to the center of the ferrosilicon submersible furnace, using ingredients such as iron oxide scale and blue charcoal, scientifically adjusting the proportion of ingredients, destroying SiC generated during the SiO2 reduction process, restoring the reaction conditions in the furnace, and gradually restoring the activity and normality of the submersible furnace. Production.
It effectively shortens the furnace condition adjustment time, achieves long-term stable production, reduces power consumption, improves the recovery rate and productivity of ferrosilicon alloy, and avoids the occurrence of dead furnace phenomena.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ferrosilicon alloy smelting, in particular to a method for adding iron ingredients in the center of a ferrosilicon ore furnace. Background Art
[0002] Ferrosilicon is the main deoxidizer and alloying agent in steelmaking. Except for some boiling steel, almost all steel grades use ferrosilicon as a deoxidizer. At the same time, adding a certain amount of silicon can significantly improve the strength, hardness and elasticity of steel. Therefore, structural steel, tool steel, spring steel, etc. contain a certain amount of silicon. Ferrosilicon is also a reducing agent in the production of alloys such as ferromolybdenum and ferrotitanium.
[0003] Ferrosilicon smelting mainly uses the submerged arc ore-fired furnace method. Most of the submerged arc ore-fired furnaces of ferrosilicon adopt a semi-enclosed form with a low smoke hood. At present, the newly built ore-fired furnaces in China have reached more than 25.5MVA. In the production practice of ferrosilicon smelting, it is found that during the ferrosilicon smelting process, there is a SiC formation and SiC decomposition zone in the ferrosilicon furnace. This limited area is very important to ensure the smooth operation of the furnace. That is, it is hoped that the newly generated SiC must be completely decomposed when it is still in the high reactivity stage shortly after its appearance to avoid the formation of stable large pieces of SiC. When the generated SiO and CO rise through the charge, as much SiO as possible should react with carbon, and at the same time, the decomposition reaction of SiO can be fully developed. These reactions have a significant impact on the productivity of the ore-fired furnace, the recovery rate of silicon and the power consumption. When the charge in the furnace is deficient in carbon, the carbon balance of the charge reaction in the furnace is broken, and the carbon in the electrode will participate in the charge reaction, causing abnormal consumption of the electrode. The working end of the electrode shrinks sharply, which in turn causes the crucible around the working end of the electrode to shrink. Further, the molten pool formed by the three-phase electrode crucible is connected and shrinks, and then loses connectivity. The charge in the center of the submerged arc furnace loses its reaction conditions, resulting in a "dead material zone", which causes the submerged arc furnace to lose its activity and even a dead furnace. The furnace has to be dug, disrupting the normal production order of the enterprise and seriously affecting the enterprise's economic benefits.
[0004] After research, it was found that during the ferrosilicon smelting process, iron can destroy the intermediate product SiC generated during the reduction of SiO2, thereby causing the reaction to proceed in the direction of silicon production. The reaction formula is Fe + nSiC = FeSin + nC. This reaction starts at 1400K and proceeds violently at 1500-1600K. In the temperature range of 1400-2300K, silicon carbide exhibits unstable characteristics when iron is present.
[0005] Through experiments, it was found that iron can be used to destroy the intermediate product SiC generated during the reduction process of SiO2 and the unstable characteristics of silicon carbide in the presence of iron. When the charge at the center of the furnace loses the reaction conditions and a dead zone is produced, iron oxide scale, lignite and other ingredients are added to the center of the furnace, and the proportion of ingredients is adjusted scientifically in stages to gradually restore the activity of the dead zone in the center of the furnace, thereby restoring the normal production of the furnace, thereby eliminating the effects of carbon deficiency in the charge on the furnace's productivity, reduced silicon recovery rate, increased power consumption, fluctuations in product composition and deterioration of furnace conditions. Summary of the invention
[0006] The invention provides a method for adding iron to the center of a ferrosilicon ore furnace, which is simple in process and easy to operate, adopts a scientific proportioning and adding method, and can restore the ore furnace to a normal production state when a serious carbon deficiency of electrode charge occurs in the center of a ferrosilicon ore furnace, thereby ensuring the normal ferrosilicon alloy smelting process.
[0007] The present invention provides a method for adding iron to a ferrosilicon ore furnace, comprising the following steps: S1. Determination of carbon deficiency in electrode charge When the output of 25MVA ferrosilicon submerged arc furnace dropped from 75 tons / day to 72 tons / day, the electrode pressure increased from 450mm / day to 520mm / day, the current of submerged arc furnace jumped, the electrode displacement was adjusted between 100mm-600mm, the arc sound could be heard, and the furnace eye was difficult to open, which was judged to be carbon deficiency of electrode charge; S2. Adjust fuel ratio Adjust the fuel ratio of ferrosilicon alloy into the furnace. The fuel is based on silica: 1000kg, semi-coke: 580kg±10kg, iron oxide: 185kg±5kg; S3. Furnace center charging 1) There are three electrodes in the submerged arc furnace, named A phase, B phase and C phase in sequence. The three electrodes are arranged in a regular triangle with the furnace core as the center, and are vertically inserted into the furnace charge. The depth of burial in the charge is ≥ 2.2 meters; 2) Adjust the batches of materials to the central material pipe of the submerged arc furnace. The specific batching method is to use 1000kg of silica as the batching base for each batch of materials, increase the iron oxide to 210kg / batch, and increase the semi-coke to 190kg / batch; 3) After batching, start unloading the material into the central material pipe of the ore-fired furnace according to the above batching method. After the material circulation, the central material pipe will circulate 4-5 more batches of material per day, and the current will gradually stabilize. When the daily output is continuously stable at 75 tons / day and the electrode pressure is stable at 450mnm / day, the furnace condition will return to normal, the normal material batch will be restored, and the furnace condition adjustment time will be shortened.
[0008] In step S3 3), the material is continuously discharged into the central material pipe of the ore-fired furnace according to the adjusted batching method, and the electrode insertion depth, the material surface settling speed and the iron output are observed, counted and analyzed as controlled quantitative values. When the material surface settling speed slows down and the iron output does not increase, the raw material batches are gradually increased by 3kg / batch of iron oxide scale and 1kg / batch of semi-coke. After each increase, the batching of the material batches is not less than 10 batches, the increase of iron oxide scale is controlled within a range of 30kg-50kg, and the increase of semi-coke is controlled within a range of 10kg-20kg.
[0009] In step S1, a temperature measuring gun is used to detect the temperature of the molten iron at the tapping port of the ferrosilicon ore furnace. The normal molten iron temperature is in the range of 1600-1750°C. If the molten iron temperature at the tapping port of the ferrosilicon ore furnace is less than 1550°C, it can be determined that the charge is carbon deficient.
[0010] In step S3 2), when adding iron oxide scale and lignite to the electrode, before adding iron oxide scale and lignite around phase A, phase B and phase C, when the iron tapping time exceeds 40 minutes, the single furnace output still does not reach 7.5 tons / furnace, and this situation occurs for more than 3 consecutive furnaces, the two-phase electrode material pipe close to the iron tapping furnace eye should be adjusted to the material structure, and 30kg / batch of iron oxide scale and 10kg / batch of lignite should be added to the original material. When it is observed that the iron tapping flow rate gradually stabilizes, and the output can reach 7.5 tons / furnace after 40 minutes, and after 3 consecutive furnaces, it is adjusted to the normal material batch structure for material batching.
[0011] In the step S1, when the electrode charge is seriously deficient in carbon, the charge with crust on the core of the ferrosilicon ore furnace is dug out from the furnace of the ferrosilicon ore furnace by using a tamping rod of a furnace tamping machine and pushed out of the furnace.
[0012] Beneficial effects of the present invention: 1) Add silica, blue charcoal and iron oxide to the ferrosilicon blast furnace. Blue charcoal is used as a reducing agent to reduce the oxygen in silica and iron oxide to form carbon monoxide. The silicon in silica combines with the iron in iron oxide to form ferrosilicon.
[0013] 2) By adjusting the amount of ingredients in the central feed pipe of the ore-fired furnace and increasing the amount of iron oxide scale within a certain range, the time for adjusting the furnace condition can be shortened from the original three days to one day. In addition, through the personalized adjustment of the iron addition method in the center of the ferrosilicon ore-fired furnace, the long-term stability of the furnace condition can be achieved. The stabilization time can be stabilized to more than 90 days without changing the origin of the raw materials and fuels.
[0014] 3) When adding iron oxide scale and semi-coke to the electrode, before adding iron oxide scale and semi-coke around phases A, B and C, when the tapping time exceeds 40 minutes, the output of a single furnace still does not reach 7.5 tons / furnace, and this situation occurs for more than 3 consecutive furnaces, the two-phase electrode material pipe close to the tapping furnace eye should be adjusted to adjust the batching structure, and add 30kg / batch of iron oxide scale and 10kg / batch of semi-coke on the basis of the original batching. When the tapping flow is observed to be gradually stable, and the output can reach 7.5 tons / furnace after 40 minutes and after 3 consecutive furnaces, it is adjusted to the normal batch structure for batching. The purpose is that after the channel from the tapping flow to the furnace eye is blocked by the material melted in the dead material area, it can be adjusted in time by adding iron materials in a personalized way to reduce the impact on the normal production rhythm and achieve the purpose of rapid adjustment.
[0015] 4) This method can solve the problem that when the charge at the carbon-deficient center in the ferrosilicon blast furnace loses the reaction conditions and produces a dead zone, iron can be used to destroy the intermediate product SiC generated in the reduction process of SiO2 and the unstable characteristics of SiC in the presence of iron. Iron oxide scale and lignite are added to the center of the blast furnace, and the proportion of ingredients is scientifically adjusted in stages to gradually restore the activity of the dead zone in the center of the blast furnace, thereby restoring the blast furnace to normal production state, thereby solving the problems of reduced productivity of the blast furnace, reduced silicon recovery rate, increased power consumption, fluctuation of product composition and deterioration of furnace condition caused by carbon deficiency in the charge. DETAILED DESCRIPTION
[0016] Example 1. The present invention will be further described below in conjunction with specific embodiments. A method for adding iron to a ferrosilicon ore furnace center according to the present invention comprises the following steps: S1. Determination of carbon deficiency in electrode charge When the output of 25MVA ferrosilicon submerged arc furnace dropped from 75 tons / day to 72 tons / day, the electrode pressure increased from 450mm / day to 520mm / day, the current of submerged arc furnace jumped, the electrode displacement was adjusted between 100mm-600mm, the arc sound could be heard, and the furnace eye was difficult to open, which was judged to be carbon deficiency of electrode charge; S2. Adjust fuel ratio Adjust the fuel ratio of ferrosilicon alloy into the furnace. The fuel is based on silica: 1000kg, semi-coke: 580kg±10kg, iron oxide: 185kg±5kg; S3. Furnace center charging 1) There are three electrodes in the submerged arc furnace, named A phase, B phase and C phase in sequence. The three electrodes are arranged in a regular triangle with the furnace core as the center, and are vertically inserted into the furnace charge. The depth of burial in the charge is ≥ 2.2 meters; 2) Adjust the batches of materials to the central material pipe of the submerged arc furnace. The specific batching method is to use 1000kg of silica as the batching base for each batch of materials, increase the iron oxide to 210kg / batch, and increase the semi-coke to 190kg / batch; 3) After batching, start unloading the material into the central material pipe of the ore-fired furnace according to the above batching method. After the material circulation, the central material pipe will circulate 4-5 more batches of material per day, and the current will gradually stabilize. When the daily output is continuously stable at 75 tons / day and the electrode pressure is stable at 450mnm / day, the furnace condition will return to normal, the normal material batch will be restored, and the furnace condition adjustment time will be shortened.
[0017] In step S3 3), the material is continuously discharged into the central material pipe of the ore-fired furnace according to the adjusted batching method, and the electrode insertion depth, the material surface settling speed and the iron output are observed, counted and analyzed as controlled quantitative values. When the material surface settling speed slows down and the iron output does not increase, the method of increasing the amount of iron oxide scale by 3kg / batch and the amount of semi-coke by 1kg / batch in the raw material batch is gradually increased. The batching of the material batch after each increase is not less than 10 batches, the increase of the iron oxide scale is controlled within a range of 30kg-50kg, and the increase of the semi-coke is controlled within a range of 10kg-20kg. When the iron output, power consumption and electrode consumption return to normal values, the addition of iron oxide scale and semi-coke is completed.
[0018] In step S1, a temperature measuring gun is used to detect the temperature of the molten iron at the tapping port of the ferrosilicon ore furnace. The normal molten iron temperature is in the range of 1600-1750°C. If the molten iron temperature at the tapping port of the ferrosilicon ore furnace is less than 1550°C, it can be determined that the charge is carbon deficient.
[0019] In step S3 2), when adding iron oxide scale and lignite to the electrode, before adding iron oxide scale and lignite around phase A, phase B and phase C, when the iron tapping time exceeds 40 minutes, the single furnace output still does not reach 7.5 tons / furnace, and this situation occurs for more than 3 consecutive furnaces, the two-phase electrode material pipe close to the iron tapping furnace eye should be adjusted to the material structure, and 30kg / batch of iron oxide scale and 10kg / batch of lignite should be added to the original material. When it is observed that the iron tapping flow rate gradually stabilizes, and the output can reach 7.5 tons / furnace after 40 minutes, and after 3 consecutive furnaces, it is adjusted to the normal material batch structure for material batching.
[0020] In the step S1, when the electrode charge is seriously deficient in carbon, the charge with crust on the core of the ferrosilicon ore furnace is dug out from the furnace of the ferrosilicon ore furnace by using a tamping rod of a furnace tamping machine and pushed out of the furnace.
[0021] Ferrosilicon furnace No. 4 is used: capacity is 25.5MW, diameter of three electrodes are 1.3m, arranged in a regular triangle around the furnace core, inner diameter of the furnace is 8.1m, depth of the furnace is 3.15m, 10 furnaces of iron are produced per day (5 furnaces in the day shift and 5 furnaces in the night shift), average iron output per furnace is 7.1 tons, average smelting power consumption is 8800KW.h / t.
[0022] In early March 2021, abnormal furnace conditions occurred in 15 furnaces for 1.5 consecutive days. The smelting power consumption continued to rise from 8790KW.h / t to 9430KW.h / t. The iron output of each furnace dropped from 7.15 tons to 4.89 tons. The electrodes were difficult to insert and the arc sound could be clearly heard. The electrode consumption per ton of iron increased from 55kg to 72kg. The measured temperature of the molten iron at the tapping mouth dropped from 1610℃ to 1490℃, and it was determined that the charge was carbon deficient.
[0023] First, adjust the raw material and fuel ratio of ferrosilicon alloy into the furnace. Each batch of materials uses 1000kg of silica as the basic unit of ingredients, the basic amount of blue coke is kept at 580kg + 3kg, and the iron oxide is adjusted at 185kg + 1kg. At the same time, on the 6.8-meter platform, iron oxide scale and lignite are manually added around the A, B and C electrodes. Each batch of materials uses 1000kg of silica as the basic unit, 36kg of iron oxide scale and 12kg of lignite as the base unit. The materials are added in a ladder from the direction of the electrode to the direction of the furnace core at a scale of 300mm, and the adjustment control is based on 5 furnaces.
[0024] The iron output and smelting power consumption were tracked and counted, and the taphole temperature was tracked and measured. After 15 furnaces of continuous adjustment, the iron output of each furnace gradually recovered to 7.16 tons, the smelting power consumption per ton of iron dropped from 9430KW.h / t to 8795KW.h / t, the measured temperature of the molten iron at the taphole dropped from 1490℃ to 1615℃, the electrode was easy to insert, and the electrode consumption dropped from 72kg to 55kg. It was determined that the production had returned to normal and the addition of material batches was stopped.
[0025] Example 2. The present invention will be further described below in conjunction with specific embodiments. A method for adding iron to a ferrosilicon ore furnace center according to the present invention comprises the following steps: S1. Determination of carbon deficiency in electrode charge When the output of 25MVA ferrosilicon submerged arc furnace dropped from 75 tons / day to 72 tons / day, the electrode pressure increased from 450mm / day to 520mm / day, the current of submerged arc furnace jumped, the electrode displacement was adjusted between 100mm-600mm, the arc sound could be heard, and the furnace eye was difficult to open, which was judged to be carbon deficiency of electrode charge; S2. Adjust fuel ratio Adjust the fuel ratio of ferrosilicon alloy into the furnace. The fuel is based on silica: 1000kg, semi-coke: 580kg±10kg, iron oxide: 185kg±5kg; S3. Furnace center charging 1) There are three electrodes in the submerged arc furnace, named A phase, B phase and C phase in sequence. The three electrodes are arranged in a regular triangle with the furnace core as the center, and are vertically inserted into the furnace charge. The depth of burial in the charge is ≥ 2.2 meters; 2) Adjust the batches of materials to the central material pipe of the submerged arc furnace. The specific batching method is to use 1000kg of silica as the batching base for each batch of materials, increase the iron oxide to 210kg / batch, and increase the semi-coke to 190kg / batch; 3) After batching, start unloading the material into the central material pipe of the ore-fired furnace according to the above batching method. After the material circulation, the central material pipe will circulate 4-5 more batches of material per day, and the current will gradually stabilize. When the daily output is continuously stable at 75 tons / day and the electrode pressure is stable at 450mnm / day, the furnace condition will return to normal, the normal material batch will be restored, and the furnace condition adjustment time will be shortened.
[0026] In step S3 3), the material is continuously discharged from the central material pipe of the ore-fired furnace according to the adjusted batching method, and the electrode insertion depth, the material surface sinking speed and the iron output are observed, counted and analyzed as the control quantitative values. When the material surface sinking speed slows down and the iron output does not increase, the method of increasing the iron scale by 3kg / batch and the blue coke by 1kg / batch in the raw material batch is gradually increased, and the batching of each batch after each increase is not less than 10 batches. The increase of the iron scale is controlled within the range of 30kg-50kg, and the increase of the blue coke is controlled within the range of 10kg-20kg. When the iron output, power consumption and electrode consumption return to normal values, the addition of the iron scale and blue coke ends.
[0027] In step S1, a temperature measuring gun is used to detect the temperature of the molten iron at the tapping port of the ferrosilicon ore furnace. The normal molten iron temperature is in the range of 1600-1750°C. If the molten iron temperature at the tapping port of the ferrosilicon ore furnace is less than 1550°C, it can be determined that the charge is carbon deficient.
[0028] In step S3 2), when adding iron oxide scale and lignite to the electrode, before adding iron oxide scale and lignite around phase A, phase B and phase C, when the iron tapping time exceeds 40 minutes, the single furnace output still does not reach 7.5 tons / furnace, and this situation occurs for more than 3 consecutive furnaces, the two-phase electrode material pipe close to the iron tapping furnace eye should be adjusted to the material structure, and 30kg / batch of iron oxide scale and 10kg / batch of lignite should be added to the original material. When it is observed that the iron tapping flow rate gradually stabilizes, and the output can reach 7.5 tons / furnace after 40 minutes, and after 3 consecutive furnaces, it is adjusted to the normal material batch structure for material batching.
[0029] In the step S1, when the electrode charge is seriously deficient in carbon, the charge with crust on the core of the ferrosilicon ore furnace is dug out from the furnace of the ferrosilicon ore furnace by using a tamping rod of a furnace tamping machine and pushed out of the furnace.
[0030] Ferrosilicon No. 3 furnace is used: capacity is 25.5MW, the diameter of three electrodes is 1.3m, arranged in a regular triangle around the furnace core, the inner diameter of the furnace is 8.2m, the depth of the furnace is 3.2m, and 10 furnaces of iron are produced per day (5 furnaces in the day shift and 5 furnaces in the night shift). The average iron output of each furnace is 7.2 tons, and the average smelting power consumption is 8750KW.h / t.
[0031] In mid-February 2022, abnormal furnace conditions occurred in 20 furnaces for two consecutive days. The smelting power consumption continued to rise from 8720KW.h / t to 9300KW.h / t, the iron output of each furnace dropped from 7.3 tons to 4.3 tons, the electrodes were difficult to insert, and the arc sound could be clearly heard. The electrode consumption per ton of iron increased from 55kg to 67kg, and the measured temperature of molten iron at the tapping mouth dropped from 1620℃ to 1530℃, which was judged to be carbon deficient in the charge.
[0032] First, adjust the raw material and fuel ratio of ferrosilicon alloy entering the furnace. Each batch of materials uses 1000kg of silica as the basic unit of ingredients, the basic amount of lignite is adjusted from 580kg+6kg, and the iron oxide scale is adjusted from 185kg+2kg.
[0033] At the same time, iron oxide scale and semi-coke are added around the electrodes of phases A, B and C on the 6.8m platform. The silica quantity of each batch is 1000kg as the batching unit, 30kg of iron oxide scale and 10kg of semi-coke are added. The materials are added from the electrode direction to the furnace core direction at a scale of 300mm, and the adjustment section is controlled with 5 heats.
[0034] The iron output and smelting power consumption were tracked and counted, and the taphole temperature was tracked and measured. After 9 furnaces of continuous adjustment, the iron output of each furnace gradually recovered to 7.25 tons, the smelting power consumption per ton of iron dropped from 9300KW.h / t to 8710KW.h / t, the measured temperature of the molten iron at the taphole dropped from 1530℃ to 1630℃, the electrode was easy to insert, and the electrode consumption dropped from 67kg to 53kg. It was determined that the production had returned to normal and the addition of material batches was stopped.
[0035] Example 3. The present invention will be further described below in conjunction with specific embodiments. A method for adding iron to a ferrosilicon ore furnace center according to the present invention comprises the following steps: S1. Determination of carbon deficiency in electrode charge When the output of 25MVA ferrosilicon submerged arc furnace dropped from 75 tons / day to 72 tons / day, the electrode pressure increased from 450mm / day to 520mm / day, the current of submerged arc furnace jumped, the electrode displacement was adjusted between 100mm-600mm, the arc sound could be heard, and the furnace eye was difficult to open, which was judged to be carbon deficiency of electrode charge; S2. Adjust fuel ratio Adjust the fuel ratio of ferrosilicon alloy into the furnace. The fuel is based on silica: 1000kg, semi-coke: 580kg±10kg, iron oxide: 185kg±5kg; S3. Furnace center charging 1) There are three electrodes in the submerged arc furnace, named A phase, B phase and C phase in sequence. The three electrodes are arranged in a regular triangle with the furnace core as the center, and are vertically inserted into the furnace charge. The depth of burial in the charge is ≥ 2.2 meters; 2) Adjust the batches of materials to the central material pipe of the submerged arc furnace. The specific batching method is to use 1000kg of silica as the batching base for each batch of materials, increase the iron oxide to 210kg / batch, and increase the semi-coke to 190kg / batch; 3) After batching, start unloading the material into the central material pipe of the ore-fired furnace according to the above batching method. After the material circulation, the central material pipe will circulate 4-5 more batches of material per day, and the current will gradually stabilize. When the daily output is continuously stable at 75 tons / day and the electrode pressure is stable at 450mnm / day, the furnace condition will return to normal, the normal material batch will be restored, and the furnace condition adjustment time will be shortened.
[0036] In step S3 3), the material is continuously discharged from the central material pipe of the ore-fired furnace according to the adjusted batching method, and the electrode insertion depth, the material surface sinking speed and the iron output are observed, counted and analyzed as the control quantitative values. When the material surface sinking speed slows down and the iron output does not increase, the method of increasing the iron scale by 3kg / batch and the blue coke by 1kg / batch in the raw material batch is gradually increased, and the batching of each batch after each increase is not less than 10 batches. The increase of the iron scale is controlled within the range of 30kg-50kg, and the increase of the blue coke is controlled within the range of 10kg-20kg. When the iron output, power consumption and electrode consumption return to normal values, the addition of the iron scale and blue coke ends.
[0037] In step S1, a temperature measuring gun is used to detect the temperature of the molten iron at the tapping port of the ferrosilicon ore furnace. The normal molten iron temperature is in the range of 1600-1750°C. If the molten iron temperature at the tapping port of the ferrosilicon ore furnace is less than 1550°C, it can be determined that the charge is carbon deficient.
[0038] In step S3 2), when adding iron oxide scale and lignite to the electrode, before adding iron oxide scale and lignite around phase A, phase B and phase C, when the iron tapping time exceeds 40 minutes, the single furnace output still does not reach 7.5 tons / furnace, and this situation occurs for more than 3 consecutive furnaces, the two-phase electrode material pipe close to the iron tapping furnace eye should be adjusted to the material structure, and 30kg / batch of iron oxide scale and 10kg / batch of lignite should be added to the original material. When it is observed that the iron tapping flow rate gradually stabilizes, and the output can reach 7.5 tons / furnace after 40 minutes, and after 3 consecutive furnaces, it is adjusted to the normal material batch structure for material batching.
[0039] In the step S1, when the electrode charge is seriously deficient in carbon, the charge with crust on the core of the ferrosilicon ore furnace is dug out from the furnace of the ferrosilicon ore furnace by using a tamping rod of a furnace tamping machine and pushed out of the furnace.
[0040] Ferrosilicon furnace No. 4: capacity 25.5MW, three electrodes with a diameter of 1.3m each, arranged in a regular triangle around the furnace core, furnace inner diameter 8.1m, furnace depth 3.1m, 10 furnaces of iron are produced per day (5 furnaces in the day shift and 5 furnaces in the night shift), the average iron output of each furnace is 7.1 tons, and the average smelting power consumption is 8800KW.h / t.
[0041] In early May 2022, abnormal furnace conditions occurred in 25 furnaces for 2.5 consecutive days. The smelting power consumption continued to rise from 8720KW.h / t to 9450KW.h / t, the iron output of each furnace dropped from 7.3 tons to 4.2 tons, the electrodes were difficult to insert, and the arc sound could be clearly heard. The electrode consumption per ton of iron increased from 55kg to 72kg, the measured temperature of the molten iron at the tapping mouth dropped from 1620℃ to 1490℃, the temperature of the furnace core surface was 280℃, and a "dead material zone" appeared, which was determined to be carbon deficient in the charge.
[0042] First, adjust the raw material and fuel ratio of ferrosilicon alloy entering the furnace. Each batch of materials uses 1000kg of silica as the basic unit of ingredients. The basic amount of lignite is adjusted from 580kg+9kg, and that of iron oxide is adjusted from 185kg+3kg. Use a furnace tamping machine to dig out the dead material in the furnace core and push it out of the furnace, weighing 2500kg. Then add 470kg of iron oxide and 157kg of lignite in a ratio of 3:1, mix well, and refill the furnace core. Then, add iron oxide and lignite around the A, B, and C electrodes manually on a 6.8-meter platform. Each batch of materials uses 1000kg of silica as the basic unit of ingredients. 45kg of iron oxide and 15kg of lignite are added. The materials are added in a ladder from the electrode direction to the furnace core direction at a scale of 300mm, and 5 furnaces are used as the adjustment section control.
[0043] The iron output and smelting power consumption were tracked and counted, and the taphole temperature was tracked and measured. After 20 furnaces of continuous adjustment, the iron output of each furnace gradually recovered to 7.31 tons, the smelting power consumption per ton of iron dropped from 9450KW.h / t to 8715KW.h / t, the measured temperature of the molten iron at the taphole dropped from 1490℃ to 1620℃, the electrode was easy to insert, and the electrode consumption dropped from 72kg to 54kg. It was determined that the production had returned to normal and the addition of material batches was stopped.
Claims
1. A method for adding iron to a ferrosilicon ore furnace, characterized in that: The following steps are involved: S1. Determination of carbon deficiency in electrode charge When the output of 25MVA ferrosilicon submerged arc furnace dropped from 75 tons / day to 72 tons / day, the electrode pressure increased from 450mm / day to 520mm / day, the current of submerged arc furnace jumped, the electrode displacement was adjusted between 100mm-600mm, the arc sound could be heard, and the furnace eye was difficult to open, which was judged to be carbon deficiency of electrode charge; S2. Adjust fuel ratio Adjust the fuel ratio of ferrosilicon alloy into the furnace. The fuel is based on silica: 1000kg, semi-coke: 580kg±10kg, iron oxide: 185kg±5kg; S3. Furnace center charging 1) There are three electrodes in the submerged arc furnace, named A phase, B phase and C phase in sequence. The three electrodes are arranged in a regular triangle with the furnace core as the center, and are vertically inserted into the furnace charge. The depth of burial in the charge is ≥ 2.2 meters; 2) Adjust the batches of materials to the central material pipe of the submerged arc furnace. The specific batching method is to use 1000kg of silica as the batching base for each batch of materials, increase the iron oxide to 210kg / batch, and increase the semi-coke to 190kg / batch; 3) After batching, start unloading the material into the central material pipe of the ore-fired furnace according to the above batching method. After the material circulation, the central material pipe will circulate 4-5 more batches of material per day, and the current will gradually stabilize. When the daily output is continuously stable at 75 tons / day and the electrode pressure is stable at 450mnm / day, the furnace condition will return to normal, the normal material batch will be restored, and the furnace condition adjustment time will be shortened.
2. The method for adding iron to a ferrosilicon ore furnace as claimed in claim 1, characterized in that: In step S3 3), the material is continuously discharged into the central material pipe of the ore-fired furnace according to the adjusted batching method, and the electrode insertion depth, the material surface settling speed and the iron output are observed, counted and analyzed as controlled quantitative values. When the material surface settling speed slows down and the iron output does not increase, the raw material batches are gradually increased by 3kg / batch of iron oxide scale and 1kg / batch of semi-coke. After each increase, the batching of the material batches is not less than 10 batches, the increase of iron oxide scale is controlled within a range of 30kg-50kg, and the increase of semi-coke is controlled within a range of 10kg-20kg.
3. The method for adding iron to a ferrosilicon ore furnace as claimed in claim 1, characterized in that: In step S1, a temperature measuring gun is used to detect the temperature of the molten iron at the tapping point of the ferrosilicon ore furnace. The normal molten iron temperature is in the range of 1600-1750°C. When the molten iron temperature at the tapping point of the ferrosilicon ore furnace is less than 1550°C, it can be determined that the charge is carbon deficient.
4. The method for adding iron to a ferrosilicon ore furnace as claimed in claim 1, characterized in that: In step S3 2), when adding iron oxide scale and lignite to the electrode, before adding iron oxide scale and lignite around phase A, phase B and phase C, when the iron tapping time exceeds 40 minutes, the single furnace output still does not reach 7.5 tons / furnace, and this situation occurs for more than 3 consecutive furnaces, the two-phase electrode material pipe close to the iron tapping furnace eye should be adjusted to the material structure, and 30kg / batch of iron oxide scale and 10kg / batch of lignite should be added to the original material. When it is observed that the iron tapping flow rate gradually stabilizes, and the output can reach 7.5 tons / furnace after 40 minutes, and after 3 consecutive furnaces, it is adjusted to the normal material batch structure for material batching.
5. The method for adding iron to a ferrosilicon ore furnace as claimed in claim 1, characterized in that: In the step S1, when the electrode charge is seriously deficient in carbon, the charge with crust on the core of the ferrosilicon ore furnace is dug out from the furnace of the ferrosilicon ore furnace by using a tamping rod of a furnace tamping machine and pushed out of the furnace.