Porous aromatic skeleton membrane electrode material and preparation method and application thereof

By performing click reaction and metal salt solution reduction on thiol-modified foam metal, a porous aromatic framework membrane electrode material was prepared, which solved the problems of poor electrocatalyst stability and large usage of precious metals, and achieved efficient electrocatalytic hydrogen evolution performance and long-term performance. stability.

CN118814221APending Publication Date: 2024-10-22NORTHEAST NORMAL UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410951858.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing porous membrane electrode materials have poor electrocatalyst stability under neutral or alkaline conditions, large amounts of catalytic metal are used, high preparation costs, and insufficient operating stability under high current densities.

Method used

Using the preparation method of porous aromatic framework membrane electrode materials, through click reaction on the surface of thiol-modified foam metal, combined with metal salt solution for reduction, a catalytically active porous aromatic framework membrane electrode material is formed, which reduces the use of precious metals and improves stability. .

Benefits of technology

It realizes the rapid and simple preparation of porous aromatic framework membrane electrode materials under mild conditions, reduces the amount of catalyst used and preparation costs, improves catalytic activity and stability, especially maintains excellent hydrogen evolution performance and long-term performance under high current density. stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118814221A_ABST
    Figure CN118814221A_ABST
Patent Text Reader

Abstract

The invention relates to the field of porous membrane electrode materials, in particular to a porous aromatic framework membrane electrode material and a preparation method and application thereof.Under the inert atmosphere condition, an organic monomer and a photoinitiator serve as raw materials, a click reaction is initiated in an organic solvent under the illumination condition, and the porous aromatic framework material is obtained, the organic monomer is an organic monomer containing sulfydryl and an organic monomer containing alkynyl or alkenyl; foam metal is placed in a synthesis system of the porous aromatic framework material, and a foam metal material modified by the porous aromatic framework is obtained; the porous aromatic skeleton modified foam metal material is immersed in a metal salt solution and reduced through a reducing reagent, the metal / porous aromatic skeleton membrane electrode material with catalytic activity is obtained, and the Pt-coated PAF-260-m / NF electrode material prepared through the method has low hydrogen evolution overpotential and excellent hydrogen evolution performance and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of porous membrane electrode materials, and in particular to a porous aromatic skeleton membrane electrode material and a preparation method and application thereof. Background Art

[0002] Hydrogen is an important clean energy source, which is widely used in the fields of new energy, industry (low-carbon metallurgy, high-purity materials) and biomedicine. Hydrogen mainly comes from two methods: industrial hydrogen production and water electrolysis. The use of renewable energy to produce hydrogen will have broad application prospects. At present, there are many metals that can be used as active components of electrocatalytic hydrogen evolution electrodes, such as transition metal elements such as platinum, palladium, rhodium, iridium, osmium, ruthenium, and their phosphorus, sulfides, etc. However, the catalyst often forms a primary cell with the metal substrate during the catalytic process, causing the active components to dissolve, or the hydrogen bubbles generated for a long time cause the catalyst to detach, which ultimately leads to a decrease in catalytic activity and stability, greatly increasing the production cost and energy loss in actual production.

[0003] At present, there are many methods to solve the above problems, such as using Nafion as a catalyst coating and carrier, using SiO x , Al2O3, TiO2 and hydrogel film encapsulation of electrode surface, use of porous materials for catalyst loading, which will bury some active sites to a certain extent. Secondly, these measures are effective at high current density (industrial current density: 300-1000mA / cm 2 , the laboratory current density is usually 10-100mA / cm 2 ) Poor stability during long-term operation. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a porous aromatic skeleton membrane electrode material and a preparation method and application thereof. The porous aromatic membrane electrode prepared by the preparation method provided by the present invention can solve the problem of poor stability of electrocatalysts under neutral or alkaline conditions, while also reducing the usage of catalytic metals and the preparation cost of the catalyst.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] A method for preparing a porous aromatic skeleton membrane electrode material comprises the following steps:

[0007] The thiol-modified foam metal, an organic monomer, a photoinitiator and an organic solvent are mixed, and under inert atmosphere conditions, the organic monomer and the photoinitiator are used as raw materials to initiate a click reaction on the surface of the thiol-modified foam metal in an organic solvent under light conditions, and the initiation is completed quickly under mild reaction conditions, and the foam metal is modified by the thiol group to promote a more stable combination of the membrane material and the substrate, so as to obtain a porous aromatic skeleton-modified foam metal material, wherein the organic monomer is an organic monomer containing a thiol group and an organic monomer containing an alkynyl group or an alkene group;

[0008] The porous aromatic skeleton modified foam metal material is immersed in a metal salt solution, and the metal salt solution is reduced by a reducing agent to obtain a porous aromatic skeleton membrane electrode material containing metal elements and having catalytic activity.

[0009] In a preferred embodiment of the present invention, the thiol-containing organic monomer is 1,4-benzenedithiol, and the alkynyl- or alkenyl-containing organic monomer is one of 1,3,5-triethynylbenzene, 1,3,5-trivinylbenzene, 1,3,5-triphenylethynylbenzene, and 1,3,5-tristyrylbenzene.

[0010] In a preferred embodiment of the present invention, the photoinitiator is one or more of benzoin dimethyl ether, benzil dimethyl ketal, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 4,6-trimethylbenzoylphosphine oxide, and 2-carboxy-2-methylpropiophenone.

[0011] In a preferred embodiment of the present invention, the mass fraction of the photoinitiator in the organic monomer is 2-5%, the molar ratio of the organic monomer containing a mercapto group to the organic monomer containing an alkynyl group or an alkenyl group is 3:2, and the reaction temperature is room temperature.

[0012] In a preferred embodiment of the present invention, the lighting condition is sunlight, natural light, xenon lamp or ultraviolet lamp.

[0013] In a preferred embodiment of the present invention, the inert gas includes nitrogen or argon.

[0014] In a preferred embodiment of the present invention, the organic solvent is one or more of dichloromethane, tetrahydrofuran, N,N-dimethylformamide, and acetonitrile, and the reducing agent is one of ethanol, methanol, ethylene glycol, and sodium borohydride.

[0015] In a preferred embodiment of the present invention, the foam metal is one of foam nickel, foam iron and foam copper.

[0016] In a preferred embodiment of the present invention, the metal salt solution is an aqueous solution containing potassium tetrachloroplatinate, and other transition metals with catalytic properties such as iron, cobalt, nickel, etc. can be used to replace metal platinum.

[0017] Another object of the present invention is to provide a porous aromatic skeleton membrane electrode material prepared by any of the preparation methods described above.

[0018] The third object of the present invention is to provide an application of the porous aromatic skeleton membrane electrode material described above in electrochemical hydrogen evolution under alkaline conditions.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. In the present invention, an organic monomer, a photoinitiator and an organic solvent are mixed under inert gas conditions, a click reaction is initiated under light conditions, and a thiol-modified foam metal is added to obtain a porous aromatic skeleton-modified foam metal material, and then the porous skeleton-modified foam metal is immersed in a metal salt solution with catalytic performance, and the metal salt solution is reduced by a reducing agent to obtain a porous aromatic skeleton membrane electrode material containing metal elements with catalytic activity; the synthesis method of the present invention is simple, can be carried out under mild conditions, is easy to operate, and can reduce the amount of precious metal catalyst used. The prepared platinum-containing porous aromatic skeleton-modified membrane electrode material uses less precious metal (Pt≤0.15mg cm -2 ) can be obtained with a platinum content of 0.5 mg cm -2 The hydrogen evolution performance is comparable to that of commercial Pt / C catalysts.

[0021] 2. The Pt@PAF-260-m / NF electrode material prepared by the present invention benefits from the high specific surface area of ​​the porous aromatic skeleton material and the uniform pore structure throughout, which can improve the mass transfer efficiency. The rich active metal anchoring sites (alkyne groups, thiol groups) can act on the foam metal and catalytically active metal to enhance its force on the metal. Therefore, it has a low hydrogen evolution overpotential, good stability and excellent hydrogen evolution performance.

[0022] 3. The present invention prepares porous aromatic skeleton materials through a quick and simple method, which does not require expensive catalysts or cumbersome and complicated processes. The prepared porous aromatic skeleton membrane electrode material can be directly loaded with platinum and other metals for electrolysis of water for hydrogen evolution.

[0023] 4. The preparation method of the present invention avoids using expensive Nation as a binder, which can reduce the amount of catalyst used, improve the stability of the catalyst, better load the catalytic metal, and can operate stably under high current density. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the infrared spectrum of the porous aromatic framework PAF-260 powder prepared in Example 1 of the present invention;

[0025] Figure 2This is a graph showing the carbon dioxide adsorption at 195K of the platinum-containing porous aromatic framework PAF-260 prepared in Example 1 of the present invention;

[0026] Figure 3 This is a thermogravimetric spectrum of the porous aromatic framework PAF-260 prepared in Example 1 of the present invention;

[0027] Figure 4 The scanning electron microscope and element distribution diagram of the porous aromatic skeleton membrane electrode material (Pt@PAF-260-m / NF) prepared in Example 2 of the present invention;

[0028] Figure 5 This is a hydrogen evolution performance diagram of the porous aromatic skeleton membrane electrode material (Pt@PAF-260-m / NF) prepared in Example 2 of the present invention;

[0029] Figure 6 The porous aromatic skeleton membrane electrode material (Pt@PAF-260-m / NF) prepared in Example 2 of the present invention is 1Acm -2 (1000mA cm -2 ) for 1000h hydrogen evolution stability. DETAILED DESCRIPTION

[0030] The following is a detailed description of the technical solutions in the embodiments of the present invention in combination with the preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] It should be noted that all professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.

[0032] Example 1

[0033] A method for preparing a porous aromatic framework material (PAF-260) comprises the following steps:

[0034] Under a nitrogen atmosphere, 1,4-benzenedithiol (43 mg, 3 mmol), 1,3,5-triethynylbenzene (30 mg, 2 mmol), benzoin dimethyl ether (2 mg, 2-5 wt%) and 40 mL of dichloromethane were added to a 50 mL two-necked flask. After stirring for 20 minutes under xenon lamp irradiation, the brown-yellow solid was collected by filtration, and the monomer and photoinitiator were repeatedly washed with dichloromethane. Then, the porous aromatic framework material PAF-260 was obtained at 120 ° C. for 12 hours with a yield of 70%.

[0035] Example 2

[0036] A method for preparing a porous aromatic skeleton membrane electrode material containing platinum and based on nickel foam, comprising the following steps:

[0037] (1) The purchased nickel foam was cut into a size of 0.8 cm × 1 cm. Before use, the nickel foam was thoroughly ultrasonically cleaned with acetone (10 minutes), anhydrous ethanol (10 minutes), deionized water (10 minutes), 1% hydrochloric acid water (30 minutes), deionized water (10 minutes), and anhydrous ethanol (10 minutes), and then vacuum dried at 50°C to obtain clean nickel foam (NF). The cleaned nickel foam was immersed in 100 mL of ethanol solution containing 10 mM 1,4-benzenedithiol for 12 hours, and then rinsed with anhydrous ethanol to obtain thiol-modified nickel foam (NF-SH);

[0038] (2) The cleaned and modified nickel foam, 1,4-benzenedithiol (43 mg, 3 mmol), 1,3,5-triethynylbenzene (30 mg, 2 mmol), benzoin dimethyl ether (2 mg, 2.73 wt%) and 40 mL of dichloromethane were added to a 50 mL two-necked flask, and stirred for 20 minutes under xenon light irradiation. After the reaction was completed, the nickel foam was taken out and ultrasonic cleaning was used to remove the yellow particles on the surface, and the nickel foam was placed in a drying oven at 80° C. for 10 minutes and then taken out to obtain a porous aromatic skeleton membrane modified nickel foam material (PAF-260-m / NF);

[0039] (3) The porous aromatic skeleton membrane modified nickel foam material (PAF-260-m / NF) obtained in step (2) and 1 mL K2PtCl4 aqueous solution (1 mg mL -1 ), 1 mL of methanol was added to the centrifuge tube, and after ultrasonic mixing, it was placed for 12 hours, and then ultrasonic cleaning was used to remove the excess black particles on the surface. The tube was placed in a drying oven at 60°C and dried for 20 minutes, and then taken out to obtain a platinum-containing porous aromatic skeleton membrane electrode based on nickel foam (Pt@PAF-260-m / NF).

[0040] Example 3

[0041] A method for preparing a platinum-containing porous aromatic skeleton membrane electrode material based on foamed iron comprises the following steps:

[0042] (1) The purchased foam iron was cut into a size of 0.8 cm × 1 cm. Before use, the foam iron was thoroughly ultrasonically cleaned with acetone (10 minutes), anhydrous ethanol (10 minutes), deionized water (10 minutes), 1% hydrochloric acid water (30 minutes), deionized water (10 minutes), and anhydrous ethanol (10 minutes) solutions, and then vacuum dried at 50°C to obtain clean foam iron (IF). The cleaned foam iron was soaked in 100 mL of ethanol solution containing 10 mM 1,4-benzenedithiol for 12 hours, and then rinsed with anhydrous ethanol to obtain modified foam iron (IF-SH);

[0043] (2) The cleaned and modified foam iron, 1,4-benzenedithiol (43 mg, 3 mmol), 1,3,5-triethynylbenzene (30 mg, 2 mmol), benzoin dimethyl ether (2 mg, 2.73 wt%) and 40 mL of dichloromethane were added to a 50 mL two-necked flask, stirred for 20 minutes under xenon light irradiation. After the reaction was completed, the foam iron was taken out and ultrasonic cleaning was used to remove the yellow particles on the surface. The foam iron was placed in a drying oven at 80° C. and dried for 10 minutes, and then taken out to obtain a porous aromatic skeleton membrane modified foam iron material (PAF-260-m / IF);

[0044] (3) The porous aromatic skeleton membrane modified iron foam material (PAF-260-m / IF) obtained in step (2) and 1 mL K2PtCl4 aqueous solution (1 mg mL -1 ), 1 mL of methanol was added into the centrifuge tube, and after ultrasonic mixing, it was placed for 12 hours, and then the excess black particles on the surface were removed by ultrasonic cleaning. The electrode was placed in a drying oven at 60°C and dried for 20 minutes, and then taken out to obtain a porous aromatic skeleton membrane electrode based on nickel foam containing platinum (Pt@PAF-260-m / IF).

[0045] Example 4

[0046] A method for preparing a platinum-containing porous aromatic skeleton membrane electrode material based on copper foam, comprising the following steps:

[0047] (1) The purchased copper foam was cut into a size of 0.8 cm × 1 cm. Before use, the copper foam was thoroughly ultrasonically cleaned with acetone (10 minutes), anhydrous ethanol (10 minutes), deionized water (10 minutes), 1% hydrochloric acid water (30 minutes), deionized water (10 minutes), and anhydrous ethanol (10 minutes), and then vacuum dried at 50°C to obtain clean copper foam (CuF). The cleaned copper foam was immersed in 100 mL of ethanol solution containing 10 mM 1,4-benzenedithiol for 12 hours, and then rinsed with anhydrous ethanol to obtain thiol-modified copper foam (CuF-SH);

[0048] (2) The cleaned and modified copper foam, 1,4-benzenedithiol (43 mg, 3 mmol), 1,3,5-triethynylbenzene (30 mg, 2 mmol), benzoin dimethyl ether (1.46 mg, 2 wt%) and 40 mL of dichloromethane were added to a 50 mL two-necked flask, stirred for 20 minutes under xenon light irradiation. After the reaction was completed, the copper foam was taken out and ultrasonic cleaning was used to remove the yellow particles on the surface. The copper foam was placed in a drying oven at 80° C. and dried for 10 minutes, and then taken out to obtain a porous aromatic skeleton membrane modified copper foam material (PAF-260-m / CuF);

[0049] (3) The porous aromatic skeleton membrane modified copper foam material (PAF-260-m / CuF) obtained in step (2) and 1 mL K2PtCl4 aqueous solution (1 mg mL -1 ), 1 mL of methanol was added into the centrifuge tube, and after ultrasonic mixing, it was placed for 12 hours, and then the excess black particles on the surface were removed by ultrasonic cleaning. The tube was placed in a drying oven at 60°C and dried for 20 minutes, and then taken out to obtain a platinum-containing porous aromatic skeleton membrane electrode based on copper foam (Pt@PAF-260-m / CuF).

[0050] Example 5

[0051] A method for preparing a porous aromatic skeleton membrane electrode material containing platinum and based on nickel foam, comprising the following steps:

[0052] (1) The purchased nickel foam was cut into a size of 0.8 cm × 1 cm. Before use, the nickel foam was thoroughly ultrasonically cleaned with acetone (10 minutes), anhydrous ethanol (10 minutes), deionized water (10 minutes), 1% hydrochloric acid water (30 minutes), deionized water (10 minutes), and anhydrous ethanol (10 minutes), and then vacuum dried at 50°C to obtain clean nickel foam (NF). The cleaned NF was immersed in 100 mL of ethanol solution containing 10 mM 1,4-benzenedithiol for 12 hours, and then rinsed with anhydrous ethanol to obtain thiol-modified nickel foam (NF-SH);

[0053] (2) The cleaned and modified nickel foam, 1,4-benzenedithiol (43 mg, 3 mmol), 1,3,5-triethynylbenzene (30 mg, 2 mmol), benzoin dimethyl ether (3.65 mg, 5 wt%) and 40 mL of dichloromethane were added to a 50 mL two-necked flask, and stirred for 20 minutes under xenon light irradiation. After the reaction was completed, the nickel foam was taken out and ultrasonic cleaning was used to remove the yellow particles on the surface. The nickel foam was placed in a drying oven at 80° C. and dried for 10 minutes, and then taken out to obtain a porous aromatic skeleton membrane modified nickel foam material (PAF-260-m / NF);

[0054] (3) The porous aromatic skeleton membrane modified nickel foam material (PAF-260-m / NF) obtained in step (2) and 1 mL K2PtCl4 aqueous solution (1 mg mL -1 ), 1 mL of methanol was added to the centrifuge tube, and after ultrasonic mixing, it was placed for 12 h, and then ultrasonic cleaning was used to remove excess black particles on the surface. The tube was placed in a drying oven and dried at 60 ° C for 20 minutes, and then taken out to obtain a platinum-containing porous aromatic framework electrode based on nickel foam (Pt@PAF-260-m / NF).

[0055] Results Analysis

[0056] The prepared platinum-containing porous aromatic skeleton membrane electrode material was tested on a CHI760E electrochemical workstation using a three-electrode system. The reference electrode was a saturated silver chloride electrode, the working electrode was a porous aromatic skeleton membrane electrode, the counter electrode was a graphite rod, and 1 mol / L KOH solution was used as the electrolyte. The hydrogen evolution performance and stability of the PAF membrane electrode were tested at 25°C.

[0057] Figure 1 This is the infrared spectrum of the porous aromatic skeleton PAF-260 powder prepared in Example 1 of the present invention. Figure 1 As shown, by comparing the infrared spectra of the porous aromatic skeleton material prepared in Example 1, 1,4-benzenedithiol and 1,3,5-triethynylbenzene used in Example 1, it can be seen that at 2565cm -1 The -SH absorption peak at 3282 cm -1 The ≡CH absorption peak at 2111cm -1 The -C≡C- absorption peak at 1679cm -1 The appearance of the absorption peak of -C=C- proves that the synthesis is successful.

[0058] Figure 2 The carbon dioxide adsorption curve of the porous aromatic framework PAF-260 prepared in Example 1 at 195K is as follows: Figure 2As shown, through pore analysis of carbon dioxide adsorption-desorption isotherms, it was found that the prepared porous aromatic framework PAF-260 has a uniform microporous and mesoporous pore structure with pore sizes distributed at 1.48nm and 3.87nm. The micro-mesoporous pores can ensure the effective transmission of various media during the catalytic process.

[0059] Figure 3 Thermogravimetric spectrum of the porous aromatic framework PAF-260 prepared in Example 1 is shown in FIG. Figure 3 As shown, through thermogravimetric research, the material is stable to 300°C and begins to lose weight, indicating that the prepared porous aromatic framework PAF-260 has high thermal stability.

[0060] Figure 4 The scanning electron microscope and element distribution diagram of the platinum-containing porous aromatic skeleton membrane electrode material (Pt@PAF-260-m / NF) prepared in Example 2 are as follows: Figure 4 As shown, it can be seen that the elements in the membrane electrode material are evenly distributed, and the average size of the metal platinum nanoparticles is about 50nm.

[0061] Figure 5 This is a hydrogen evolution performance diagram of the platinum-containing porous aromatic skeleton membrane electrode material (Pt@PAF-260-m / NF) prepared in Example 2, as shown in Figure 5 As shown in Figure 2, the PAF-260-m / NF electrode before loading with platinum has poor electrocatalytic hydrogen evolution performance. After loading with platinum, the hydrogen evolution performance of the Pt@PAF-260-m / NF electrode is greatly improved. -2 The overpotential is 34 mV, which is about twice the performance of commercial Pt / C (20wt%).

[0062] Figure 6 The platinum-containing porous aromatic skeleton membrane electrode material (Pt@PAF-260-m / NF) prepared in Example 2 is 1Acm -2 (1000mA cm -2 ) for 1000 hours of electrocatalytic hydrogen evolution stability, such as Figure 6 As shown, thanks to the coordination ability of the thiol groups in the porous aromatic skeleton with the metal, the PAF-260 membrane can adhere firmly to the NF and fix the platinum nanoparticles, so that the electrode material maintains excellent long-term stability in the hydrogen evolution process under the action of large current.

[0063] In summary, the membrane electrode material modified with a porous aromatic skeleton containing platinum prepared by the present invention uses less precious metal (Pt≤0.15mg cm -2 ) can be obtained with a platinum content of 0.5 mg cm -2The electrocatalytic hydrogen evolution performance is comparable to that of commercial Pt / C catalysts. When measured in 1 mol / L KOH alkaline solution, only a small overpotential of 34 mV is required to reach a current density of 10 mA cm -2 , with a smaller Tafel slope of 28mv dec -1 At the same time, at 1A cm -2 (1000mA cm -2 ) can continuously and stably precipitate hydrogen for more than 1000 hours at a high current density of . In summary, the Pt@PAF-260-m / NF electrode material prepared in the present invention has a low hydrogen evolution overpotential in water electrolysis and excellent stability at high current density.

[0064] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0065] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a porous aromatic skeleton membrane electrode material, characterized in that: The following steps are involved: Mixing a thiol-modified foam metal, an organic monomer, a photoinitiator and an organic solvent, and in an inert gas atmosphere, using the organic monomer and the photoinitiator as raw materials, initiating a click reaction on the surface of the thiol-modified foam metal in an organic solvent under light conditions to obtain a porous aromatic skeleton membrane-modified foam metal material, wherein the organic monomer is an organic monomer containing a thiol group and an organic monomer containing an alkynyl group or an alkene group; The porous aromatic skeleton modified foam metal material is immersed in a metal salt solution, and the metal salt solution is reduced by a reducing agent to obtain a porous aromatic skeleton membrane electrode material with catalytic activity.

2. The method for preparing a porous aromatic skeleton membrane electrode material according to claim 1, characterized in that: The organic monomer containing a mercapto group is 1,4-benzenedithiol, and the organic monomer containing an alkynyl group or an alkenyl group is one of 1,3,5-triethynylbenzene, 1,3,5-trivinylbenzene, 1,3,5-triphenylethynylbenzene, and 1,3,5-triphenylethynylbenzene.

3. The method for preparing a porous aromatic skeleton membrane electrode material according to claim 1, characterized in that: The photoinitiator is one or more of benzoin dimethyl ether, benzil dimethyl ketal, phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide, 4,6-trimethylbenzoyl phosphine oxide, and 2-carboxy-2-methylpropiophenone.

4. The method for preparing a porous aromatic skeleton membrane electrode material according to claim 1, characterized in that: The mass fraction of the photoinitiator in the organic monomer is 2-5%, the molar ratio of the organic monomer containing a mercapto group to the organic monomer containing an alkynyl group or an alkenyl group is 3:2, and the reaction temperature is room temperature.

5. The method for preparing a porous aromatic skeleton membrane electrode material according to claim 1, characterized in that: The metal salt solution is a transition metal salt solution with catalytic performance, and the transition metal salt solution is a metal salt solution containing platinum, iron, cobalt and nickel.

6. The method for preparing a porous aromatic skeleton membrane electrode material according to claim 1, characterized in that: The lighting conditions are sunlight, natural light, xenon lamp or ultraviolet lamp.

7. The method for preparing a porous aromatic skeleton membrane electrode material according to claim 1, characterized in that: The organic solvent is one or more of dichloromethane, tetrahydrofuran, N,N-dimethylformamide, and acetonitrile, and the reducing agent is one of ethanol, methanol, ethylene glycol, and sodium borohydride.

8. The method for preparing a porous aromatic skeleton membrane electrode material according to claim 1, characterized in that: The foam metal is one of foam nickel, foam iron and foam copper.

9. A porous aromatic skeleton membrane electrode material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the porous aromatic skeleton membrane electrode material according to claim 9 in hydrogen evolution by water electrolysis.

Citation Information

Cited By

  • Porous aromatic skeleton photocatalyst, synthesis method and application thereof

    CN122806550A