Preparation process for improving moisture resistance of impregnated paper
Through the process of modified melamine glue impregnation and modified nano-silica emulsion coating, combined with physical moisture resistance and chemical moisture resistance, the problem of poor moisture resistance of impregnated paper is solved, and the moisture resistance and service life are significantly improved.
Patent Information
- Application Number
- CN202411258135.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-09-09
AI Technical Summary
The existing impregnated paper has poor moisture-proof performance and is easily damaged by moisture when stored for a long time, affecting its service life and practicality.
Using the process of modified melamine glue impregnation and modified nano-silica emulsion coating, physical moisture-proof and chemical moisture-proof are combined to form an inside-out moisture-proof system.
Significantly improves the moisture-proof performance of impregnated paper, extending its service life and improving practicality.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of impregnated paper production, in particular to a preparation process for improving the moisture-proof performance of impregnated paper. Background Art
[0002] Impregnated paper is mainly made of specially produced base paper, which is impregnated with synthetic resin and dried, and then covered on the artificial board substrate and hot-pressed to form decorative surface paper. With the improvement of living standards, consumers have higher and higher requirements for the performance of impregnated paper, especially moisture-proof performance.
[0003] For example, Chinese patent CN110042701B discloses a moisture-proof and flame-retardant impregnated paper and a preparation method thereof, comprising a base paper layer, a moisture-proof layer attached to the upper surface of the base paper layer, a flame-retardant adhesive film layer attached to the upper surface of the moisture-proof layer, and a wear-resistant layer attached to the upper surface of the flame-retardant adhesive film layer; the flame-retardant adhesive film layer is prepared by printing a layer of composite flame-retardant material on the upper surface of the moisture-proof layer; the composite flame-retardant material comprises the following raw materials in parts by weight: 20-30 parts of phosphorus-nitrogen composite flame retardant, 10-15 parts of melamine A, 5-10 parts of PVC resin, 20-30 parts of MF prepolymer, 5-15 parts of ZnSn(OH)6, 1-5 parts of nano-TiO2, 1-5 parts of urea A and 1-5 parts of PVP. The moisture-proof and flame-retardant impregnated paper has excellent moisture-proof and flame-retardant properties by arranging a moisture-proof layer on the base paper layer. However, the existing impregnated paper has poor moisture-proof performance and is easily damaged by moisture when stored for a long time, which greatly affects the service life of the impregnated paper and greatly reduces the practicality of the impregnated paper. Therefore, the present invention provides a preparation process for improving the moisture-proof performance of impregnated paper. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a preparation process for improving the moisture-proof performance of impregnated paper, which solves the problem that the existing impregnated paper has poor moisture-proof performance and is easily damaged by moisture during long-term storage, which greatly affects the service life and practicality of the impregnated paper.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: A preparation process for improving the moisture-proof performance of impregnated paper, specifically comprising the following steps: S1. Glue impregnation: immerse the base paper in modified melamine glue for 30-60 minutes, dry it, and obtain melamine impregnated paper; S2. Emulsion coating: 5-10 parts by weight of modified nano-silicon dioxide emulsion, 1-3 parts by weight of hexadecyltrimethoxysilane, and 30-50 parts by weight of polyurethane emulsion are stirred evenly, then double-sided coating is performed and drying is performed.
[0006] The specific steps of the glue impregnation in S1 are: S1.1. Adjust the pH value of 100 parts by weight of 37% formaldehyde aqueous solution to 8.0-8.5, heat to 40-50°C, add 25-35 parts by weight of melamine and 25-55 parts by weight of urea, continue to heat to 90-95°C, keep warm for 40-60 minutes, adjust the pH value to 5.0-5.5, keep warm for 20-40 minutes; S1.2, add 15-35 parts by weight of urea, adjust the pH value to 7.5-8.0, and continue to keep warm for 80-100 minutes; S1.3, cooling to 45-55°C, adding 5-10 parts by weight of diethylene glycol ether and 1-5 parts by weight of urea, stirring for 60-90 minutes, cooling to room temperature, adding 1-5 parts by weight of bentonite, 1-5 parts by weight of basalt fiber, 5-10 parts by weight of water, and 1-2 parts by weight of hexadecyltrimethoxysilane to obtain an impregnating glue; S1.4, soak the base paper in the impregnating glue for 10-20 minutes, and dry at 50-70°C to obtain melamine impregnated paper.
[0007] In S1.3, after cooling to room temperature, grind 1-5 parts by weight of basalt fiber with a diameter of 3-5 μm and 5-10 parts by weight of water for 30-60 minutes, add 1-2 parts by weight of hexadecyltrimethoxysilane and stir for 20-40 minutes, then add 1-5 parts by weight of bentonite and continue stirring for 10-20 minutes to obtain a modified product, which is added to the system as a whole.
[0008] The diameter of the basalt fiber is 3-5 microns.
[0009] The preparation method of the modified nano-silica emulsion in S2 is as follows: 40-50 parts by weight of isopropanol, adjust the pH value to 4-5 with acetic acid, stir evenly with 10-20 parts by weight of water, then dropwise add 10-20 parts by weight of aminopropyltriethoxysilane while stirring, and then add 2-4 parts by weight of nano-silica and stir evenly to obtain the modified nano-silica emulsion.
[0010] The drying temperature of the glue dipping in S1 is 130-140°C.
[0011] The drying temperature of the coating emulsion in S2 is 120-130°C. Beneficial Effects
[0012] The present invention provides a preparation process for improving the moisture-proof performance of impregnated paper, S1, glue impregnation: immersing base paper in short-fiber-modified melamine glue for 30-60 minutes, drying, and obtaining melamine impregnated paper; S2, coating emulsion: 5-10 parts by weight of modified nano-silicon dioxide emulsion, 1-3 parts by weight of hexadecyltrimethoxysilane, and 30-50 parts by weight of polyurethane emulsion are stirred evenly, and then double-sided coating is performed, and then drying is performed. The present invention immerses base paper in short-fiber-modified melamine glue in the glue impregnation step, and in the emulsion coating step, modified nano-silicon dioxide emulsion and polyurethane emulsion are stirred evenly, and then double-sided coating is performed, physical moisture-proof and chemical moisture-proof are combined with each other, and the upper layer moisture-proof system is formed from the inside to the outside, thereby effectively improving the moisture-proof performance of the impregnated paper of the present invention. DETAILED DESCRIPTION
[0013] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0014] A preparation process for improving the moisture-proof performance of impregnated paper, specifically comprising the following steps: S1. Glue impregnation: immerse the base paper in modified melamine glue for 35 minutes, dry it, and obtain melamine impregnated paper; S2. Emulsion coating: 5 parts by weight of modified nano-silicon dioxide emulsion, 1 part by weight of hexadecyltrimethoxysilane and 30 parts by weight of polyurethane emulsion are stirred evenly, then coated on both sides and dried.
[0015] The specific steps of the glue impregnation in S1 are: S1.1, add 100 parts by weight of 37% formaldehyde aqueous solution and adjust the pH value to 8.0, heat to 40°C, add 25 parts by weight of melamine and 25 parts by weight of urea, continue to heat to 90°C, keep warm for 40 minutes, adjust the pH value to 5.0, and keep warm for 20 minutes; S1.2, add 15 parts by weight of urea, adjust the pH value to 7.5, and continue to keep warm and react for 80 minutes; S1.3, cooling to 45 ° C, 5 parts by weight of diethylene glycol ether and 1 part by weight of urea, stirring for 60 minutes, cooling to room temperature, adding 1 part by weight of bentonite, 1 part by weight of basalt fiber, 5 parts by weight of water, 1 part by weight of hexadecyltrimethoxysilane, to obtain impregnation glue; S1.4, soak the base paper in the impregnating glue for 10 minutes, and dry it at 50°C to obtain melamine impregnated paper.
[0016] In S1.3, after cooling to room temperature, grind 1 part by weight of basalt fiber with a diameter of 3 μm with 5 parts by weight of water for 30 minutes, add 1 part by weight of hexadecyltrimethoxysilane and stir for 20 minutes, then add 1 part by weight of bentonite and continue stirring for 10 minutes to obtain a modified product, which is added to the system as a whole.
[0017] The diameter of the basalt fiber is 3 microns.
[0018] The preparation method of the modified nano-silica emulsion in S2 is as follows: 40 parts by weight of isopropanol is adjusted to pH 4 with acetic acid, and the mixture is stirred evenly with 10 parts by weight of water, and then 10 parts by weight of aminopropyltriethoxysilane is added dropwise while stirring, and then 2 parts by weight of nano-silica is added and stirred evenly to obtain the modified nano-silica emulsion.
[0019] The drying temperature of the glue impregnation in S1 is 130°C.
[0020] The drying temperature of the coating emulsion in S2 is 120°C. Example 2
[0021] A preparation process for improving the moisture-proof performance of impregnated paper, specifically comprising the following steps: S1. Glue impregnation: immerse the base paper in modified melamine glue for 40 minutes, dry it, and obtain melamine impregnated paper; S2. Emulsion coating: 8 parts by weight of modified nano-silicon dioxide emulsion, 2 parts by weight of hexadecyltrimethoxysilane and 40 parts by weight of polyurethane emulsion are stirred evenly, then coated on both sides and dried.
[0022] The specific steps of the glue impregnation in S1 are: S1.1, add 100 parts by weight of 37% formaldehyde aqueous solution and adjust the pH value to 8.5, heat to 45°C, add 30 parts by weight of melamine and 40 parts by weight of urea, continue to heat to 92°C, keep warm for 50 minutes, adjust the pH value to 5.5, and keep warm for 30 minutes; S1.2, add 25 parts by weight of urea, adjust the pH value to 7.8, and continue to keep warm for 90 minutes; S1.3, cooling to 50 ° C, 8 parts by weight of diethylene glycol ether and 3 parts by weight of urea, stirring for 70 minutes, cooling to room temperature, adding 3 parts by weight of bentonite, 3 parts by weight of basalt fiber, 8 parts by weight of water, 1 part by weight of hexadecyltrimethoxysilane, to obtain impregnation glue; S1.4, soak the base paper in the impregnating glue for 15 minutes, and dry it at 60°C to obtain melamine impregnated paper.
[0023] In S1.3, after cooling to room temperature, grind 3 parts by weight of basalt fiber and 8 parts by weight of water for 50 minutes, add 1 part by weight of hexadecyltrimethoxysilane and stir for 30 minutes, then add 3 parts by weight of bentonite and continue stirring for 15 minutes to obtain a modified product, which is added to the system as a whole.
[0024] The diameter of the basalt fiber is 4 microns.
[0025] The preparation method of the modified nano-silica emulsion in S2 is as follows: 45 parts by weight of isopropanol, the pH value is adjusted to 5 with acetic acid, and the mixture is stirred evenly with 15 parts by weight of water, and then 15 parts by weight of aminopropyltriethoxysilane is added dropwise while stirring, and then 3 parts by weight of nano-silica is added and stirred evenly to obtain the modified nano-silica emulsion.
[0026] The drying temperature of the glue dipping in S1 is 135°C.
[0027] The drying temperature of the coating emulsion in S2 is 125°C. Example 3
[0028] A preparation process for improving the moisture-proof performance of impregnated paper, specifically comprising the following steps: S1, glue impregnation: immerse the base paper in modified melamine glue for 60 minutes, dry it, and obtain melamine impregnated paper; S2. Emulsion coating: 10 parts by weight of modified nano-silicon dioxide emulsion, 3 parts by weight of hexadecyltrimethoxysilane and 50 parts by weight of polyurethane emulsion are stirred evenly, then coated on both sides and dried.
[0029] The specific steps of the glue impregnation in S1 are: S1.1, add 35 parts by weight of melamine-55 parts by weight of urea to 100 parts by weight of a 37% formaldehyde aqueous solution and adjust the pH value to 8.5, heat to 50°C, continue to heat to 95°C, keep warm for 60 minutes, adjust the pH value to 5.5, and keep warm for 40 minutes; S1.2, add 35 parts by weight of urea, adjust the pH value to 8.0, and continue to keep warm for 100 minutes; S1.3, cooling to 55 ° C, 10 parts by weight of diethylene glycol ether and 5 parts by weight of urea, stirring for 90 minutes, cooling to room temperature, adding 5 parts by weight of bentonite, 5 parts by weight of basalt fiber, 10 parts by weight of water, 2 parts by weight of hexadecyltrimethoxysilane, to obtain impregnation glue; S1.4, soak the base paper in the impregnating glue for 20 minutes, and dry it at 70°C to obtain melamine impregnated paper.
[0030] In S1.3, after cooling to room temperature, 5 parts by weight of basalt fiber with a diameter of 5 μm and 10 parts by weight of water are ground for 60 minutes, 2 parts by weight of hexadecyltrimethoxysilane are added and stirred for 40 minutes, and then 5 parts by weight of bentonite are added and stirred for 20 minutes to obtain a modified product, which is added to the system as a whole.
[0031] The diameter of the basalt fiber is 5 microns.
[0032] The preparation method of the modified nano-silica emulsion in S2 is as follows: 50 parts by weight of isopropanol, adjust the pH value to 5 with acetic acid, stir evenly with 20 parts by weight of water, then dropwise add 20 parts by weight of aminopropyltriethoxysilane while stirring, and then add 4 parts by weight of nano-silica and stir evenly to obtain the modified nano-silica emulsion.
[0033] The drying temperature of the glue impregnation in S1 is 140° C., and the glue application amount of the glue impregnation is 75 g / m2.
[0034] The drying temperature of the coated emulsion in S2 is 130° C., and the coating amount of the emulsion is 10 g / m2.
[0035] In Examples 1-3 of the present invention, the alkaline regulator in the glue impregnation is a sodium hydroxide solution with a mass fraction of 15%, and the acid regulator is a formic acid solution with a mass fraction of 3%.
[0036] The preparation method of the polyurethane emulsion in Examples 1-3 of the present invention is: (1) 200 parts by weight of polyether polyol (PTMG 2000), 40 parts by weight of polybutylene adipate (PBA) and 5 parts by weight of 1,4-butanediol were mixed and uniformly stirred, and then 100 parts by weight of TDI-80 were added, and a prepolymerization reaction was carried out in the presence of 0.1 parts by weight of bismuth isooctanoate at a temperature of 75°C for 3 hours; (2) Cool the prepolymer to 45°C, add 170 parts by weight of butyl acrylate monomer to the prepolymer, stir for 60 minutes, add 15 parts by weight of triethylamine, stir for 15 minutes to react and form salt; then cool the reactor to 20°C, add 460 parts by weight of water, stir and emulsify, add 5 parts by weight of an aqueous solution of ethylenediamine (mass fraction 20%), continue stirring and reacting for 30 minutes, (3) Raise the temperature to 75°C, and add 0.05 parts by weight of an aqueous solution of initiator ammonium persulfate (mass fraction 0.25%) dropwise at a uniform rate over 3 h. Then raise the temperature to 80°C and keep it at that temperature for 2 h. Then cool it to room temperature to obtain a polyurethane emulsion.
[0037] Comparative Example 1
[0038] The difference between this comparative example and Example 2 is that this comparative example does not use modified glue, but uses the glue impregnation described in S1. The specific steps are: S1.1, add 100 parts by weight of 37% formaldehyde aqueous solution and adjust the pH value to 8.5, heat to 45°C, add 30 parts by weight of melamine and 40 parts by weight of urea, continue to heat to 92°C, keep warm for 50 minutes, adjust the pH value to 5.5, and keep warm for 30 minutes; S1.2, add 25 parts by weight of urea, adjust the pH value to 7.8, and continue to keep warm for 90 minutes; S1.3, cooling to 50 ° C, 8 parts by weight of diethylene glycol ether and 3 parts by weight of urea, stirring for 70 minutes, and then cooling to room temperature to obtain impregnation glue; S1.4, soak the base paper in the impregnating glue for 15 minutes, and dry it at 60°C to obtain melamine impregnated paper.
[0039] Comparative Example 2
[0040] The difference between this comparative example and Example 2 is that this comparative example does not adopt the step of coating the emulsion.
[0041] Experimental data
[0042] The water absorption tester model used in the embodiment of the present invention is ST-5684. The specific formula of water absorption of paper is: C=(G2-G1)×100, where C is the water absorption value; G2 is the weight of the paper sample after water absorption; G1 is the weight of the paper sample before water absorption.
[0043] The water absorption tester was used to test the embodiments 1-3 and the comparative examples 1-2 respectively, and the water absorption values of the three samples were calculated by the formula.
[0044]
[0045] By comparison, the water absorption value of the impregnated paper obtained by Comparative Example 1 without using modified glue and Comparative Example 2 without using coating emulsion is far lower than that of Examples 1-3. The moisture-proof performance of Comparative Examples 1 and 2 is poor, and the moisture-proof performance of the embodiment of the present invention is good.
[0046] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0047] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A preparation process for improving the moisture-proof performance of impregnated paper, characterized in that: The specific steps include: S1. Glue impregnation: immerse the base paper in short fiber modified melamine glue for 30-60 minutes, dry it, and obtain melamine impregnated paper; S2. Emulsion coating: 5-10 parts by weight of modified nano-silicon dioxide emulsion, 1-3 parts by weight of hexadecyltrimethoxysilane, and 30-50 parts by weight of polyurethane emulsion are stirred evenly, then double-sided coating is performed and drying is performed.
2. A preparation process for improving the moisture-proof performance of impregnated paper according to claim 1, characterized in that: The specific steps of the glue impregnation in S1 are: S1.
1. Adjust the pH value of 100 parts by weight of 37% formaldehyde aqueous solution to 8.0-8.5, heat to 40-50°C, add 25-35 parts by weight of melamine and 25-55 parts by weight of urea, continue to heat to 90-95°C, keep warm for 40-60 minutes, adjust the pH value to 5.0-5.5, keep warm for 20-40 minutes; S1.2, add 15-35 parts by weight of urea, adjust the pH value to 7.5-8.0, and continue to keep warm for 80-100 minutes; S1.3, cooling to 45-55°C, adding 5-10 parts by weight of diethylene glycol ether and 1-5 parts by weight of urea, stirring for 60-90 minutes, cooling to room temperature, adding 1-5 parts by weight of bentonite, 1-5 parts by weight of basalt fiber, 5-10 parts by weight of water, and 1-2 parts by weight of hexadecyltrimethoxysilane to obtain an impregnating glue; S1.4, soak the base paper in the impregnating glue for 10-20 minutes, and dry at 50-70°C to obtain melamine impregnated paper.
3. A preparation process for improving moisture-proof performance of impregnated paper according to claim 2, characterized in that: In S1.3, after cooling to room temperature, grind 1-5 parts by weight of basalt fiber and 5-10 parts by weight of water for 30-60 minutes, add 1-2 parts by weight of hexadecyltrimethoxysilane and stir for 20-40 minutes, then add 1-5 parts by weight of bentonite and continue stirring for 10-20 minutes to obtain a modified product, which is added to the system as a whole.
4. A preparation process for improving moisture-proof performance of impregnated paper according to claim 3, characterized in that: The diameter of the basalt fiber is 3-5 microns.
5. A preparation process for improving moisture-proof performance of impregnated paper according to claim 3, characterized in that: The preparation method of the modified nano-silica emulsion in S2 is as follows: 40-50 parts by weight of isopropanol, adjust the pH value to 4-5 with acetic acid, stir evenly with 10-20 parts by weight of water, then dropwise add 10-20 parts by weight of aminopropyltriethoxysilane while stirring, and then add 2-4 parts by weight of nano-silica and stir evenly to obtain the modified nano-silica emulsion.
6. A preparation process for improving moisture-proof performance of impregnated paper according to claim 1, characterized in that: The drying temperature of the glue dipping in S1 is 130-140°C.
7. A preparation process for improving moisture-proof performance of impregnated paper according to claim 1, characterized in that: The drying temperature of the coating emulsion in S2 is 120-130°C.
Citation Information
Patent Citations
Preparation method of multiple modified polyurethane emulsion
CN108976353A
Hydrophobic melamine resin and hydrophobic melamine resin coating comprising same
CN114891170A
Preparation process for improving brittleness of melamine impregnated paper
CN116065419A
OSB (oriented strand board) laminate flooring with biological function based on molecular nest technology and production process of OSB laminate flooring
CN117817781A
Moisture-proof impregnated paper and production process thereof
CN117926633A
Cited By
Preparation method of thermoplastic melamine glue impregnated decorative paper
CN120401272A
A method for preparing decorative paper impregnated with thermoplastic melamine adhesive