Laminating plurality of thin lithium bars onto current collector layer to form wider lithium metal anode
By arranging a current collector layer on the rolling surface and using rollers to press lithium metal, combined with a polymer coating and an adhesion promotion coating, the problem of insufficient width of the lithium metal anode electrode is solved, and the width of the lithium metal anode layer is expanded and The lamination quality is improved to meet the needs of large battery cells.
Patent Information
- Application Number
- CN202311422868.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2023-10-30
- Publication Date
- 2024-10-22
AI Technical Summary
Existing technology is difficult to manufacture lithium metal anode electrodes with a width exceeding 150mm, which cannot meet the needs of large bag-type battery cells, and there are limitations in the processing and handling of lithium foil.
By setting the current collector layer on the rolling surface, N strips of lithium metal are arranged in parallel and pressed using rollers to form a laminated lithium metal anode layer, and a polymer coating and an adhesion promoting coating are used to control the pressing process The width of the lamination and bonding, the roller ends are equipped with cylindrical sections or cylindrical knives to limit the expansion of the lithium metal layer.
The width of the lithium metal anode layer has been expanded to 550-600mm to meet the needs of large battery cells, and the lamination quality and lithium metal utilization have been improved through optimized processes.
Smart Images

Figure CN118825199A_ABST
Abstract
Description
[0001] The information provided in this section is for the purpose of generally presenting the background of the present disclosure. The work of the presently named inventors, to the extent it is described in this section and in aspects that may not otherwise qualify as prior art at the time of filing, is neither explicitly nor implicitly admitted to be prior art against the present disclosure. Technical Field
[0002] The present disclosure relates to battery cells, and more particularly to lithium metal anodes for battery cells. Background Art
[0003] Electric vehicles such as hybrid vehicles and battery electric vehicles include a battery pack including one or more battery modules including a plurality of battery cells. The battery cells include electrodes such as an anode electrode and a cathode electrode and a separator. Summary of the invention
[0004] The method for manufacturing an anode electrode includes: providing a current collector layer on a rolling surface; arranging N lithium metal strips parallel to each other on the current collector layer, where N is an integer greater than one; and pressing the N lithium metal strips against the rolling surface to form a laminated lithium metal anode layer on the current collector layer.
[0005] In other features, the method includes pressing N strips of lithium metal by rollers. Pressing the N strips of lithium metal is performed by N rollers. A first strip of the N strips of lithium metal is laminated by a first roller of the N rollers, a second strip of the N strips of lithium metal is laminated by a second roller of the N rollers, and an Nth strip of the N strips of lithium metal is laminated by an Nth roller of the N rollers.
[0006] In other features, the method includes applying a first coating on the current collector layer and applying a second coating on the current collector layer parallel to and spaced apart from the first coating, wherein N strips of lithium metal are laminated to the current collector layer between the first coating and the second coating. The first coating and the second coating include polymer coatings.
[0007] In other features, the roller includes a first cylindrical portion and a second cylindrical portion disposed at opposite axial ends of the roller; and the first cylindrical portion and the second cylindrical portion have a diameter greater than the diameter of the cylindrical body of the roller. The first cylindrical portion and the second cylindrical portion are made of a softer material than the material used for the cylindrical body of the roller.
[0008] In other features, the roller includes a first cylindrical knife and a second cylindrical knife arranged at opposite axial ends of the roller. The first cylindrical knife and the second cylindrical knife have a diameter in the range of from 80% to 120% of the diameter of the cylindrical body of the roller. The diameter of the first cylindrical knife and the second cylindrical knife is larger than the diameter of the cylindrical body of the roller, and the larger amount is 80% to 120% of the thickness of the laminated lithium metal anode layer. The first cylindrical knife and the second cylindrical knife cut the opposite sides of the laminated lithium metal anode layer without cutting the current collector layer.
[0009] In other features, the roller includes (N-1) cylindrical portions aligned with (N-1) interfacial portions of the N strips of lithium metal. The (N-1) cylindrical portions are made of a softer material than the material used for the cylindrical body of the roller. The method includes applying a lithium adhesion promoting coating on a current collector layer in predetermined areas where adhesion of the N strips of lithium metal is desired. The lithium adhesion promoting coating includes a carbon coating. The current collector layer includes copper foil.
[0010] The method for manufacturing an anode electrode includes: providing a current collector layer on a rolling surface; arranging N strips of lithium metal in parallel with each other on the current collector layer, wherein N is an integer greater than one; and pressing the N strips of lithium metal against the rolling surface using a roller to form a laminated lithium metal anode layer on the current collector layer. The roller includes a first cylindrical portion and a second cylindrical portion arranged at opposite axial ends of the roller. The first cylindrical portion and the second cylindrical portion have a diameter greater than a diameter of a cylindrical body of the roller.
[0011] In other features, the first cylindrical portion and the second cylindrical portion are made of a softer material than the material used for the cylindrical body of the roller.
[0012] The method for manufacturing an anode electrode includes: providing a current collector layer on a rolling surface; arranging N strips of lithium metal on the current collector layer in parallel with each other, wherein N is an integer greater than one; and pressing the N strips of lithium metal against the rolling surface using a roller to form a laminated lithium metal anode layer having an increasing width on the current collector layer. The roller includes (N-1) cylindrical portions aligned with (N-1) interface portions of the N strips of lithium metal.
[0013] In other features, the (N-1) cylindrical portions are made of a softer material than the material used for the cylindrical body of the roller.
[0014] The present invention includes the following technical solutions:
[0015] 1. A method for manufacturing an anode electrode, comprising:
[0016] Disposing a current collector layer on the rolling surface;
[0017] Arranging N lithium metal strips parallel to each other on the current collector layer, wherein N is an integer greater than one; and
[0018] The N strips of lithium metal are pressed against the rolling surface to form a laminated lithium metal anode layer on the current collector layer.
[0019] 2. The method according to Scheme 1, wherein pressing the N lithium metal strips is performed by a roller.
[0020] 3. The method according to Scheme 1, wherein pressing the N strips of lithium metal is performed by N rollers.
[0021] 4. The method according to claim 3, wherein:
[0022] A first one of the N strips of lithium metal is laminated by a first one of the N rollers,
[0023] A second one of the N strips of lithium metal is laminated by a second one of the N rollers, and
[0024] The Nth of the N lithium metal strips is laminated by the Nth of the N rollers.
[0025] 5. The method according to Option 1 further includes applying a first coating on the current collector layer and applying a second coating on the current collector layer that is parallel to and spaced apart from the first coating, wherein the N lithium metal strips are laminated to the current collector layer between the first coating and the second coating.
[0026] 6. The method according to Option 5, wherein the first coating and the second coating comprise polymer coatings.
[0027] 7. The method according to claim 2, wherein:
[0028] The roller includes a first cylindrical portion and a second cylindrical portion disposed at opposite axial ends of the roller; and
[0029] The first cylindrical portion and the second cylindrical portion have a diameter greater than a diameter of the cylindrical body of the roller.
[0030] 8. A method according to Option 7, wherein the first cylindrical portion and the second cylindrical portion are made of a material softer than the material used for the cylindrical body of the roller.
[0031] 9. The method according to claim 2, wherein:
[0032] The roller comprises a first cylindrical cutter and a second cylindrical cutter arranged at opposite axial ends of the roller; and
[0033] The first cylindrical cutter and the second cylindrical cutter have a diameter in the range from 80% to 120% of the diameter of the cylindrical body of the roller.
[0034] 10. The method according to claim 9, wherein the diameters of the first cylindrical knife and the second cylindrical knife are larger than the diameter of the cylindrical body of the roller by 80% to 120% of the thickness of the laminated lithium metal anode layer.
[0035] 11. The method according to Option 9, wherein the first cylindrical knife and the second cylindrical knife cut opposite sides of the laminated lithium metal anode layer without cutting the current collector layer.
[0036] 12. The method according to Option 2, wherein the roller includes (N-1) cylindrical portions aligned with (N-1) interface portions of the N lithium metal strips.
[0037] 13. The method according to claim 12, wherein the (N-1) cylindrical portions are made of a material softer than the material used for the cylindrical body of the roller.
[0038] 14. The method according to claim 1, further comprising applying a lithium adhesion promoting coating on the current collector layer in predetermined areas where adhesion of the N strips of lithium metal is desired.
[0039] 15. The method of claim 14, wherein the lithium adhesion promoting coating comprises a carbon coating.
[0040] 16. The method according to claim 1, wherein the current collector layer comprises copper foil.
[0041] 17. A method for manufacturing an anode electrode, comprising:
[0042] Disposing a current collector layer on the rolling surface;
[0043] Arranging N lithium metal strips parallel to each other on the current collector layer, wherein N is an integer greater than one; and
[0044] Using a roller, pressing the N strips of lithium metal against the rolling surface to form a laminated lithium metal anode layer on the current collector layer,
[0045] wherein the roller comprises a first cylindrical portion and a second cylindrical portion arranged at opposite axial ends of the roller, and
[0046] Wherein, the diameters of the first cylindrical portion and the second cylindrical portion are greater than the diameter of the cylindrical body of the roller.
[0047] 18. The method according to claim 17, wherein the first cylindrical portion and the second cylindrical portion are made of a material softer than the material used for the cylindrical body of the roller.
[0048] 19. A method for manufacturing an anode electrode, comprising:
[0049] Disposing a current collector layer on the rolling surface;
[0050] Arranging N lithium metal strips parallel to each other on the current collector layer, wherein N is an integer greater than one; and
[0051] using a roller, pressing the N strips of lithium metal against the rolling surface to form a laminated lithium metal anode layer having an increased width on the current collector layer,
[0052] Wherein, the roller includes (N-1) cylindrical portions aligned with (N-1) interface portions of the N lithium metal strips.
[0053] 20. The method according to claim 19, wherein the (N-1) cylindrical portions are made of a material softer than the material used for the cylindrical body of the roller.
[0054] Further areas of applicability of the present disclosure will become apparent from the detailed description, claims and drawings.The detailed description and specific examples are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] The present disclosure will be more fully understood from the detailed description and accompanying drawings, in which:
[0056] Figure 1 is a plan view of an example of a roller pressing multiple strips of lithium metal layers onto a current collector layer to form a wider laminated lithium metal anode layer according to the present disclosure;
[0057] Figure 2 is a perspective view of an example of a roller pressing multiple strips of lithium metal layers onto a current collector layer to form a wider laminated lithium metal anode layer according to the present disclosure;
[0058] Figure 3 is a perspective view of an example of a plurality of rollers pressing a plurality of lithium metal layers onto a current collector layer according to the present disclosure;
[0059] Figure 4A is a perspective view of an example of a roller pressing multiple strips of lithium metal layers onto a current collector layer between coating layers according to the present disclosure;
[0060] Figure 4B is a perspective view of an example of a roller pressing a plurality of lithium metal layers onto an adhesion promoting coating layer on a current collector layer according to the present disclosure;
[0061] Figure 5 is a perspective view of an example of a roller having knives located at opposite axial ends for pressing multiple lithium metal layers onto a current collector layer while kiss cutting the outer edges according to the present disclosure;
[0062] FIG. 6A to FIG. 6C is a perspective view of an example of a roller having raised cylindrical portions at opposite axial ends for pressing multiple strips of lithium metal layers onto a current collector layer according to the present disclosure;
[0063] Fig. 7A is a perspective view of an example of a roller including a raised cylindrical portion located at an interface region of a plurality of lithium metal layers according to the present disclosure;
[0064] Figure 7B and Figure 7C is a side view of an example of a roller including a raised cylindrical portion at an interface region of multiple lithium metal layers according to the present disclosure; and
[0065] Fig.7D is a side view of multiple lithium metal layers and interface regions between the multiple lithium metal layers according to the present disclosure.
[0066] Among the drawings, reference numerals may be repeated to identify similar and / or identical elements. DETAILED DESCRIPTION
[0067] Although an anode electrode including a lithium metal anode and a current collector layer for a battery cell is described below in the context of an electric vehicle, the anode electrodes described herein may be used in battery cells for stationary applications or other applications.
[0068] A battery cell typically includes an anode electrode, a cathode electrode, and a separator. A battery cell including a lithium metal anode has a high specific capacity and a low density. The anode electrode includes a lithium metal anode layer attached or laminated to one or both sides of an anode current collector layer (e.g., copper foil or another material). In some examples, the strips of the lithium metal anode layer and the current collector layer are made of foil.
[0069] Due to processing and / or handling issues, commercially available ultra-thin (e.g., less than 50 μm thick) lithium foil widths are limited to 150 mm. However, large pouch-type battery cells require lithium metal anodes with widths ranging from 550-600 mm, which requires wider lithium foils than are currently available.
[0070] The present disclosure relates to a method for laminating multiple lithium foils in parallel to a current collector layer to provide a wider (e.g., a width greater than 150 mm) laminated lithium metal anode layer. In some examples, the method for manufacturing a lithium metal anode layer according to the present disclosure also uses a coating applied to the current collector layer to control the expansion of the outer edge of the laminated lithium metal anode layer. After performing the pressing, the coating can be removed from the current collector layer.
[0071] In other examples, the roller includes a cylindrical portion at an end thereof defining a shoulder to limit expansion of the lithium metal layer during pressing. In some examples, a method for manufacturing a laminated lithium metal anode layer uses a roller including a cylindrical portion aligned with an interface region of the lithium metal strip to fuse the interface region.
[0072] In some examples, multiple strips of lithium foil are arranged in parallel with a predetermined stack or overlap. In some examples, an adhesion promoting coating is applied to the current collector layer in a predetermined area to promote adhesion of the lithium metal strips in the predetermined area (and to promote removal of lithium foil outside the predetermined area).
[0073] Reference now Figures 1 to 3 , N lithium metal strips 110-1, 110-2, ..., and 110-N are arranged so that their edges are aligned with adjacent strips of the N lithium metal strips 110, where N is an integer greater than one. Figure 1 and Figure 2 A single roller is used to press N strips of lithium metal, but in Figure 3 In some examples, N strips of lithium metal 110 include lithium foil having a thickness of less than 50 μm and a width of less than 150 mm.
[0074] exist Figure 1 and Figure 2 , roller 120 includes a cylindrical body 122 and an axis 124. Roller 120 presses N strips of lithium metal 110 against a current collector layer 114 supported on a rolling surface (such as another roller or a flat surface). The laminated lithium metal anode layer 112 produced by pressing is wider than a single strip of lithium metal. In some examples, the laminated lithium metal anode layer 112 is approximately N times the width of a strip of lithium metal 110 (minus overlap and / or material removed by trimming).
[0075] exist Figure 3In some examples, a first strip of N lithium metal strips is pressed onto the current collector layer 114 by the first of rollers 120-1, 120-2, ... and 120-N. A second strip of N lithium metal strips is pressed onto the current collector layer 114 by the second of rollers 120-1, 120-2, ... and 120-N. An Nth strip of N lithium metal strips is pressed onto the current collector layer 114 by the Nth of rollers 120-1, 120-2, ... and 120-N. The edges of the N lithium metal strips touch and / or overlap. As can be appreciated, the order of pressing the N lithium metal strips can be changed when the N lithium metal strips are pressed from one side to the other.
[0076] In some examples, the current collector layer 114 has a width of 630 mm, each lithium metal strip 110 has a width of 150 mm, and N = 4. In some examples, the outermost lithium metal strip 110 is arranged to have a first gap and a second gap, respectively, relative to the edge of the current collector layer 114. In some examples, the first gap is 5 mm and the second gap is 25 mm.
[0077] Referring now to FIG. 4 , coatings 200-1 and 200-2 are applied to the current collector layer 114 prior to pressing to control the expansion of the laminated lithium metal anode layer 112 during pressing. In some examples, the coatings 200-1 and 200-1 include a polymer layer (e.g., polyimide). In some examples, the opposing edges of the roller 120 are placed on the coatings 200-1 and 200-2 during lamination. The coatings 200-1 and 200-2 act as edge stops to prevent the expansion of the laminated lithium metal anode layer 112 during pressing. After pressing, the coatings can be removed (e.g., using a solvent such as acetone).
[0078] In some examples, coatings 200-1 and 200-2 include an adhesion limiting coating that limits the adhesion of the lithium metal foil to the current collector layer 114 to allow removal of the lithium metal foil outside the inner edge of coatings 200-1 and 200-2. In some examples, the adhesion limiting coating includes poly(methyl methacrylate) (PMMA) or oil to enable removal of the lithium foil on the adhesion limiting coating. After pressing, a solvent is used to remove coatings 200-1 and 200-2.
[0079] exist Figure 4B In the embodiment, the current collector layer 114 includes a lithium adhesion promoting coating 230 disposed in a predetermined area 232 of the lithium metal anode layer 112 to be laminated. The lithium adhesion promoting coating 230 includes a material that promotes lithium adhesion in the predetermined area 232 and allows the lithium metal foil to be easily removed outside the predetermined area 232. In some examples, the lithium adhesion promoting coating 230 includes a carbon coating.
[0080] Reference now Figure 5 , roller 220 includes a cylindrical body 222 and a shaft 224. A circular knife 226 is arranged at opposite axial ends of roller 220. The circular knife 226 extends radially outward from the cylindrical body 222 by a predetermined distance. In some examples, the predetermined distance is within 80% to 120% of the thickness of the lithium metal strip. The circular knife 226 cuts the laminated lithium metal anode layer 112 to control the width of the laminated lithium metal anode layer. In some examples, the circular knife 226 cuts the laminated lithium metal anode layer 112 without cutting through the current collector layer 114 arranged below.
[0081] Reference now FIG. 6A to FIG. 6C , the roller 320 includes a cylindrical body 324 and a shaft 322. A cylindrical portion 326 is located at the end of the cylindrical body 324. The cylindrical portion 326 has a larger diameter than the cylindrical body 324. For example, the cylindrical portion 326 has a radius that is 80% to 120% of the thickness of the laminated lithium metal anode layer 112 greater than the cylindrical body 324. The cylindrical portion 326 defines a shoulder 327 relative to the cylindrical body 324. The shoulder 327 limits the expansion of the laminated lithium metal anode layer 112 during pressing.
[0082] In some examples, the cylindrical portion 326 located at the axial end of the cylindrical body 324 includes a bearing 332 to allow the cylindrical portion 326 to roll independently of the cylindrical body 324. The cylindrical portion 326 rotates while maintaining a predetermined gap (e.g., <5 μm) relative to the cylindrical body 324. In some examples, the cylindrical portion 326 is made of a different material than the cylindrical body 324. In some examples, the cylindrical portion 326 is made of a softer material than the material used for the cylindrical body 324.
[0083] Reference now 7A to 7D , the roller 340 includes a cylindrical body 344 and a shaft 342. FIG. 7A to FIG. 7C In the embodiment, (N-1) cylindrical portions 346 are located between the axial ends of the roller 340 and are located between (N-1) interface regions 360 (such as Fig.7D The (N-1) cylindrical portions 346 have a larger diameter than the cylindrical body 324.
[0084] The (N-1) cylindrical portions 346 can be designed to enhance the quality of the (N-1) interface regions 360. The (N-1) cylindrical portions 346 add pressure to the (N-1) interface regions 360 to smooth the (N-1) interface regions 360 and improve the lamination quality. In some examples, the (N-1) cylindrical portions 346 are made of a different material than the cylindrical body 344. In some examples, the (N-1) cylindrical portions 346 are made of a softer material than the material used for the cylindrical body 344.
[0085] The foregoing description is essentially illustrative only, and is not intended to limit the present disclosure, its application or use in any way. The broad teachings of the present disclosure can be implemented in various forms. Therefore, although the present disclosure includes specific examples, the true scope of the disclosure should not be so limited, because based on the study of the drawings, the specification and the appended claims, other modifications will become apparent. It should be understood that, without changing the principles of the present disclosure, one or more steps in the method can be implemented in different orders (or simultaneously). In addition, although each embodiment is described above as having certain features, any one or more of those features described in any embodiment of the present disclosure can be implemented in any other embodiment and / or in combination with the features of any other embodiment, even if the combination is not explicitly described. In other words, the described embodiments are not mutually exclusive, and the arrangement of one or more embodiments with each other remains within the scope of the present disclosure.
[0086] Spatial and functional relationships between elements (e.g., between modules, circuit elements, semiconductor layers, etc.) are described using various terms, including "connected," "engaged," "coupled," "adjacent," "immediately adjacent," "on top of," "above," "below," and "disposed." Unless explicitly described as "direct," when describing a relationship between a first element and a second element in the above disclosure, the relationship may be a direct relationship between the first element and the second element with no other intervening elements, but may also be an indirect relationship with one or more intervening elements (spatially or functionally) between the first element and the second element. As used herein, the phrase at least one of A, B, and C should be interpreted as meaning a logical (A OR B OR C) using a non-exclusive logical OR, and should not be interpreted as meaning "at least one of A, at least one of B, and at least one of C."
[0087] In the diagram, as indicated by the arrow head, the direction of the arrow generally shows the flow of information (such as data or instructions) of interest to the diagram. For example, when element A and element B exchange various information but the information transmitted from element A to element B is relevant to the diagram, the arrow may point from element A to element B. This unidirectional arrow does not imply that no other information is transmitted from element B to element A. In addition, for information sent from element A to element B, element B may send a request or a receipt confirmation to element A for the information.
Claims
1. A method for manufacturing an anode electrode, include: Disposing a current collector layer on the rolling surface; Arranging N lithium metal strips parallel to each other on the current collector layer, wherein N is an integer greater than one; and The N strips of lithium metal are pressed against the rolling surface to form a laminated lithium metal anode layer on the current collector layer.
2. The method according to claim 1, in, The pressing of the N strips of lithium metal is performed by rollers.
3. The method according to claim 1, in, Pressing the N bars of lithium metal is performed by N rollers.
4. The method according to claim 3, in: A first one of the N strips of lithium metal is laminated by a first one of the N rollers, A second one of the N strips of lithium metal is laminated by a second one of the N rollers, and The Nth of the N lithium metal strips is laminated by the Nth of the N rollers.
5. The method of claim 1, further comprising applying a first coating on the current collector layer and applying a second coating on the current collector layer parallel to and spaced apart from the first coating, in, The N strips of lithium metal are laminated to the current collector layer between the first coating layer and the second coating layer.
6. The method according to claim 5, in, The first coating and the second coating include polymer coatings.
7. The method according to claim 2, in: The roller includes a first cylindrical portion and a second cylindrical portion disposed at opposite axial ends of the roller; and The first cylindrical portion and the second cylindrical portion have a diameter greater than a diameter of the cylindrical body of the roller.
8. The method according to claim 7, in, The first cylindrical portion and the second cylindrical portion are made of a softer material than the material used for the cylindrical body of the roller.
9. The method according to claim 2, in: The roller comprises a first cylindrical cutter and a second cylindrical cutter arranged at opposite axial ends of the roller; and The first cylindrical cutter and the second cylindrical cutter have a diameter in the range from 80% to 120% of the diameter of the cylindrical body of the roller.
10. The method according to claim 9, in, The diameters of the first cylindrical knife and the second cylindrical knife are larger than the diameter of the cylindrical body of the roller by 80% to 120% of the thickness of the laminated lithium metal anode layer.