Membrane electrode preparation method and membrane electrode thereof
By printing and photo-curing the adhesive layer on the edge of the membrane electrode, replacing the traditional hot pressing process, the impact of high-temperature curing of the frame film on the durability of the membrane electrode is solved, achieving more efficient production and longer-life membrane electrodes.
Patent Information
- Application Number
- CN202410694639.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In traditional membrane electrode preparation methods, the frame film requires long-term high-temperature curing, resulting in damaged membrane electrode durability and low production efficiency.
The photo-curing adhesive layer is printed on the edge of the three-layer film electrode and cured by ultraviolet irradiation, replacing the traditional hot pressing process, simplifying the frame sealing process, avoiding stress concentration, and eliminating the need for bottom films and protective films.
The service life of the membrane electrode is improved, the production time is shortened, the cost is reduced, and the production efficiency is improved.
Smart Images

Figure CN118825344A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a membrane electrode preparation method and a membrane electrode thereof. Background Art
[0002] Proton exchange membrane fuel cells are energy conversion devices that can directly convert the chemical energy in hydrogen fuel and oxidant into electrical energy through electrochemical reactions. Fuel cells have the characteristics of high energy conversion efficiency and no exhaust gas emissions. They are considered to be one of the most promising solutions to solve the energy crisis and environmental pollution, especially in transportation such as automobiles, ships and backup power supplies. It is precisely because of these outstanding advantages that the development and application of fuel cell technology has received much attention and is considered to be the preferred clean and efficient power generation method in the 21st century.
[0003] Membrane-Electrode Assembly (MEA) is the core of the proton exchange membrane fuel cell assembly. The usual structure of the membrane electrode assembly is: cathode frame membrane-cathode catalyst layer-proton exchange membrane-anode catalyst layer-anode frame membrane, which is called a five-layer membrane electrode, and cathode catalyst layer-proton exchange membrane-anode catalyst layer, which is called a three-layer membrane electrode. The usual method for preparing a five-layer membrane electrode is as follows: first, the frame membrane is cut into corresponding sizes, the protective film is peeled off, and the frame membrane with the hollowed-out middle active area is bonded to the three-layer membrane electrode. The side of the frame membrane with adhesive is in contact with the three-layer membrane electrode, and the frame membrane is in contact with the edge area of the three-layer membrane electrode. Then, the five-layer membrane electrode is prepared by hot pressing. The area where the frame membrane contacts the three-layer membrane electrode is under concentrated stress during the hot pressing process, resulting in a large loss of the proton exchange membrane, which in turn affects the service life of the membrane electrode. In addition, the traditional frame membrane requires long-term high-temperature curing, which will also have an adverse effect on the durability of the membrane electrode. Summary of the invention
[0004] The main purpose of the present invention is to propose a membrane electrode preparation method and a membrane electrode thereof, aiming to solve the problem that the conventional frame film needs to be cured at high temperature for a long time, which will also have an adverse effect on the durability of the membrane electrode.
[0005] To achieve the above object, the present invention provides a method for preparing a membrane electrode in a first aspect, comprising the following steps:
[0006] Provide three-layer membrane electrode;
[0007] Printing a first photocurable adhesive layer on the edge of the first wall surface of the three-layer membrane electrode and curing it;
[0008] A second photocurable adhesive layer is printed on the edge of the second wall surface of the three-layer membrane electrode, and is cured until the second photocurable adhesive layer is bonded to the first photocurable adhesive layer.
[0009] In some embodiments, before printing the first photocurable adhesive layer on the edge of the first wall surface of the three-layer membrane electrode, after providing the three-layer membrane electrode, the following steps are further included:
[0010] The second wall surface of the three-layer membrane electrode is adsorbed by a vacuum adsorption plate.
[0011] In some embodiments, before printing the second photocurable adhesive layer on the edge of the second wall surface of the three-layer membrane electrode and after curing the first photocurable adhesive layer, the following steps are further included:
[0012] The first wall surface of the three-layer membrane electrode is adsorbed by a vacuum adsorption plate.
[0013] In some embodiments, a PTFE coating is provided on the vacuum adsorption plate.
[0014] In some embodiments, printing a first photocurable adhesive layer on the edge of the first wall surface of the three-layer membrane electrode and curing it comprises the following specific steps:
[0015] A first photocurable adhesive layer is printed on the edge of the first wall surface of the three-layer membrane electrode by screen printing, and the first photocurable adhesive layer is irradiated with ultraviolet rays until the first photocurable adhesive layer is cured.
[0016] In some embodiments, printing a second photocurable adhesive layer on the edge of the second wall surface of the three-layer membrane electrode and curing it comprises the following specific steps:
[0017] A second photocurable adhesive layer is printed on the edge of the second wall surface of the three-layer membrane electrode by screen printing, and the second photocurable adhesive layer is irradiated with ultraviolet rays until the second photocurable adhesive layer is cured.
[0018] In some embodiments, after printing the first photocurable adhesive layer on the edge of the first wall surface of the three-layer membrane electrode and before curing it, the following steps are further included:
[0019] Determining whether the thickness of the first light-curable adhesive layer meets a preset range, and curing it if so;
[0020] If not, printing is continued until the thickness of the first photocurable adhesive layer is within a preset range.
[0021] In some embodiments, after printing the second photocurable adhesive layer on the edge of the second wall surface of the three-layer membrane electrode and before curing it, the following steps are further included:
[0022] Determining whether the thickness of the second light-curable adhesive layer meets a preset range, and curing it if so;
[0023] If not, printing is continued until the thickness of the second photocurable adhesive layer is within a preset range.
[0024] In the second aspect, the present application provides a membrane electrode, including a three-layer membrane electrode, wherein the three-layer membrane electrode has a first wall surface and a second wall surface that are relatively arranged, a first photocurable adhesive layer is arranged at the edge of the first wall surface, and a second photocurable adhesive layer is arranged at the edge of the second wall surface, and the shapes of the first photocurable adhesive layer and the second photocurable adhesive layer are substantially the same.
[0025] In the technical solution of the present invention, a first photocurable adhesive layer is printed on the edge of the first wall surface of the three-layer membrane electrode and cured, and then a second photocurable adhesive layer is printed on the edge of the second wall surface and cured. Since the first photocurable adhesive layer and the second photocurable adhesive layer are respectively bonded to the two sides of the three-layer membrane electrode, the fuel cell frame sealing process is simplified, and the traditional hot pressing process is avoided, thereby avoiding the damage of the three-layer membrane electrode to the three-layer membrane electrode caused by stress concentration in the overlapping area of the frame film and the three-layer membrane electrode, greatly improving the service life of the membrane electrode, shortening the curing time of the traditional frame film adhesive, eliminating the base film and protective film used in the traditional frame film, greatly improving the production efficiency, and reducing the production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 The present invention is a flow chart of the membrane electrode preparation method.
[0028] Figure 2 It is a schematic diagram of the structure of the membrane electrode of the present invention;
[0029] In the figure: 10, three-layer membrane electrode; 20, first wall surface; 30, second wall surface; 40, first photocurable adhesive layer; 50, second photocurable adhesive layer.
[0030] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0032] In addition, the meaning of "and / or" appearing in the full text includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or a solution that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0033] Membrane-Electrode Assembly (MEA) is the core of the proton exchange membrane fuel cell component. The usual structure of the membrane electrode assembly is: cathode frame membrane-cathode catalyst layer-proton exchange membrane-anode catalyst layer-anode frame membrane, which is called a five-layer membrane electrode, and cathode catalyst layer-proton exchange membrane-anode catalyst layer, which is called a three-layer membrane electrode. The usual method for preparing a five-layer membrane electrode is as follows: first, the frame membrane is cut into corresponding sizes, the protective film is peeled off, and the frame membrane with the hollowed-out middle active area is bonded to the three-layer membrane electrode. The side of the frame membrane with adhesive is in contact with the three-layer membrane electrode, and the frame membrane is in contact with the edge area of the three-layer membrane electrode. Then, the five-layer membrane electrode is prepared by hot pressing. The area where the frame membrane contacts the three-layer membrane electrode is under concentrated stress during the hot pressing process, resulting in a large loss of the proton exchange membrane, which in turn affects the service life of the membrane electrode. In addition, traditional frame membranes require long-term high-temperature curing, which will also have an adverse effect on the durability of the membrane electrode.
[0034] In view of this, the present invention proposes a method for preparing a membrane electrode, comprising the following steps:
[0035] S1, providing a three-layer membrane electrode 10;
[0036] S2, printing a first photocurable adhesive layer 40 on the edge of the first wall surface 20 of the three-layer membrane electrode 10, and curing it;
[0037] S3 . Print the second photocurable adhesive layer 50 on the edge of the second wall surface 30 of the three-layer membrane electrode 10 , and cure it until the second photocurable adhesive layer 50 is bonded to the first photocurable adhesive layer 40 .
[0038] Traditional hot pressing itself causes a certain degree of damage to the proton exchange membrane, and the frame membranes on both sides are harder than the proton exchange membrane. There is a shearing effect during the hot pressing process. Photocuring completely avoids these unfavorable factors. The above preparation method is equivalent to using photocuring glue to replace the traditional frame membrane, and using photocuring to replace the traditional hot pressing method, which simplifies the fuel cell frame sealing process and avoids the traditional hot pressing process, thereby avoiding the stress concentration in the overlapping area of the frame membrane and the three-layer membrane electrode to damage the three-layer membrane electrode, greatly improving the service life of the membrane electrode, and shortening the curing time of the traditional frame membrane adhesive, eliminating the base film and protective film used in the traditional frame membrane, greatly improving production efficiency and reducing production costs.
[0039] The membrane electrode prepared by the above preparation method includes a three-layer membrane electrode 10, wherein the three-layer membrane electrode 10 has a first wall 20 and a second wall 30 arranged opposite to each other, a first photocurable adhesive layer 40 is arranged at the edge of the first wall 20, and a second photocurable adhesive layer 50 is arranged at the edge of the second wall 30, and the shape of the first photocurable adhesive layer 40 and the second photocurable adhesive layer 5 are roughly the same. Due to certain errors in the process, the shapes of the first photocurable adhesive layer 40 and the second photocurable adhesive layer 50 cannot be exactly the same, and there will be certain deviations.
[0040] The three-layer membrane electrode 10 includes a cathode catalyst layer-a proton exchange membrane-anode catalyst layer. The first photocurable adhesive layer 40 and the second photocurable adhesive layer 50 are symmetrically distributed with the proton exchange membrane as the center line, and a groove is formed between the first photocurable adhesive layer 40 and the second photocurable adhesive layer 50, so that the edges of the cathode catalyst layer and the anode catalyst layer are embedded in the groove. It should be understood that the groove should have a gap so that the proton exchange membrane can extend into the gap.
[0041] Furthermore, between steps S1 and S2, there is also a step of using a vacuum adsorption plate to adsorb the second wall surface 30 of the three-layer membrane electrode 10, and between steps S2 and S3, there is also a step of using a vacuum adsorption plate to adsorb the first wall surface 20 of the three-layer membrane electrode 10.
[0042] The advantage of using a vacuum adsorption plate for adsorption is that during the printing process, the entire three-layer membrane electrode 1 will not be moved due to external forces, thereby causing printing failure. It should be understood that during steps S2 and S3, the order of S2 and S3 can also be swapped. It is only necessary to print a photocurable adhesive layer on the edge of one side of the three-layer membrane electrode 1, and then adsorb the printed side onto the vacuum adsorption plate.
[0043] Furthermore, a PTFE (Polytetra fluoroethylene) coating is provided on the vacuum adsorption plate, which has high lubricity and non-stickiness. In the actual photocuring process, the first photocuring adhesive layer 40 and the second photocuring adhesive layer 50 are slightly larger than the proton exchange membrane. Therefore, in order to avoid the cured adhesive layer sticking to the vacuum adsorption plate and being inconvenient to remove, a PTFE coating is provided on the vacuum adsorption plate.
[0044] Furthermore, in the specific step S20 of step S2, the first photocurable adhesive layer 40 is printed on the edge of the first wall surface 2 of the three-layer membrane electrode 1 by screen printing, and the first photocurable adhesive layer 40 is irradiated with ultraviolet rays until the first photocurable adhesive layer 40 is cured.
[0045] In the present application, screen printing is used for printing. The shape and size of the photocurable adhesive can be controlled by screen printing to prevent glue diffusion. Then, ultraviolet rays are used to irradiate the first photocurable adhesive layer 40 until the first photocurable adhesive layer 40 is cured. The irradiation time can be selected according to the intensity of the ultraviolet rays.
[0046] Correspondingly, in the specific step S30 of step S3, the second photocurable adhesive layer 50 is printed on the edge of the second wall surface 30 of the three-layer membrane electrode 10 by screen printing, and the second photocurable adhesive layer 50 is irradiated with ultraviolet rays until the second photocurable adhesive layer 50 is cured.
[0047] Generally, when printing the second photocurable adhesive layer 50 , the shape, size and printing track of the photocurable adhesive used are the same as those when printing the first photocurable adhesive layer 40 , so as to facilitate the subsequent assembly of the fuel cell.
[0048] In step S2, that is, after printing the first photocurable adhesive layer 4 on the edge of the first wall surface 20 of the three-layer membrane electrode 10 and before curing it, the following steps are also included:
[0049] Determine whether the thickness of the first photocurable adhesive layer 40 meets a preset range, and if so, cure it;
[0050] If not, printing is continued until the thickness of the first photocurable adhesive layer 40 is within a preset range.
[0051] In step S3, that is, after printing the second photocurable adhesive layer 5 on the edge of the second wall surface 30 of the three-layer membrane electrode 10 and before curing it, the following steps are also included:
[0052] Determine whether the thickness of the second photocurable adhesive layer 50 meets a preset range, and if so, cure it;
[0053] If not, printing is continued until the thickness of the second photocurable adhesive layer 50 is within a preset range.
[0054] It is judged whether the printing thickness of the first photocurable adhesive layer 40 and the second photocurable adhesive layer 50 is within a preset range. The specific judgment method can generally be detected by a thickness detection device. The printing thickness is generally between 10μm and 100μm. If the thickness of the first photocurable adhesive layer 40 and the second photocurable adhesive layer 50 is less than 10μm, the mechanical strength of the membrane electrode frame film is insufficient, resulting in easy deformation of the membrane electrode structure. When the fuel cell stack is assembled, the gas diffusion layer of the fuel cell will be compressed, resulting in fewer water vapor transmission channels, thereby failing to supply fuel and reducing the performance of the fuel cell; and if the thickness of the first photocurable adhesive layer 40 and the second photocurable adhesive layer 50 is greater than 100μm, the impedance between the gas diffusion layer and the bipolar plate will increase due to insufficient compression rate of the gas diffusion layer, which will also reduce the performance of the fuel cell. Specifically, it can be 20μm, 30μm, 40μm, etc. The specific values are not limited here and are set according to actual conditions.
[0055] In the present application, a first photocurable adhesive layer 40 is printed on the edge of the first wall 20 of the three-layer membrane electrode 10 and cured, and then a second photocurable adhesive layer 50 is printed on the edge of the second wall 30 and cured. Since the first photocurable adhesive layer 40 and the second photocurable adhesive layer 50 are respectively bonded to the two sides of the three-layer membrane electrode 10, the fuel cell frame sealing process is simplified, and the traditional hot pressing process is avoided, thereby avoiding the damage of the three-layer membrane electrode to the three-layer membrane electrode due to stress concentration in the overlapping area of the frame film and the three-layer membrane electrode 10, greatly improving the service life of the membrane electrode, shortening the curing time of the traditional frame film adhesive, eliminating the base film and protective film used in the traditional frame film, greatly improving production efficiency, and reducing production costs.
[0056] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A method for preparing a membrane electrode, characterized in that: The following steps are involved: Provide three-layer membrane electrode; Printing a first photocurable adhesive layer on the edge of the first wall surface of the three-layer membrane electrode and curing it; A second photocurable adhesive layer is printed on the edge of the second wall surface of the three-layer membrane electrode and then cured.
2. The method for preparing a membrane electrode according to claim 1, characterized in that: Before printing the first photocurable adhesive layer on the edge of the first wall surface of the three-layer membrane electrode and after providing the three-layer membrane electrode, the step further includes: The second wall surface of the three-layer membrane electrode is adsorbed by a vacuum adsorption plate.
3. The method for preparing a membrane electrode according to claim 1, characterized in that: Before printing the second photocurable adhesive layer on the edge of the second wall surface of the three-layer membrane electrode and after curing the first photocurable adhesive layer, the method further includes the following steps: The first wall surface of the three-layer membrane electrode is adsorbed by a vacuum adsorption plate.
4. The method for preparing a membrane electrode according to claim 2 or 3, characterized in that: The vacuum adsorption plate is provided with a PTFE coating.
5. The method for preparing a membrane electrode according to claim 1, characterized in that: Printing a first photocurable adhesive layer on the edge of the first wall surface of the three-layer membrane electrode and curing it includes the following specific steps: A first photocurable adhesive layer is printed on the edge of the first wall surface of the three-layer membrane electrode by screen printing, and the first photocurable adhesive layer is irradiated with ultraviolet rays until the first photocurable adhesive layer is cured.
6. The method for preparing a membrane electrode according to claim 1, characterized in that: Printing a second light-curable adhesive layer on the edge of the second wall surface of the three-layer membrane electrode and curing it includes the following specific steps: A second photocurable adhesive layer is printed on the edge of the second wall surface of the three-layer membrane electrode by screen printing, and the second photocurable adhesive layer is irradiated with ultraviolet rays until the second photocurable adhesive layer is cured.
7. The method for preparing a membrane electrode according to claim 1, characterized in that: After printing the first photocurable adhesive layer on the edge of the first wall surface of the three-layer membrane electrode and before curing it, the method further includes the following steps: Determining whether the thickness of the first light-curable adhesive layer meets a preset range, and curing it if so; If not, printing is continued until the thickness of the first photocurable adhesive layer is within a preset range.
8. The method for preparing a membrane electrode according to claim 1, characterized in that: After printing the second photocurable adhesive layer on the edge of the second wall surface of the three-layer membrane electrode and before curing it, the method further includes the following steps: Determining whether the thickness of the second light-curable adhesive layer meets a preset range, and curing it if so; If not, printing is continued until the thickness of the second photocurable adhesive layer is within a preset range.
9. A membrane electrode prepared by the method according to any one of claims 1 to 8, characterized in that: include: A three-layer membrane electrode, wherein the three-layer membrane electrode has a first wall surface and a second wall surface that are arranged opposite to each other, a first photocurable adhesive layer is arranged at the edge of the first wall surface, and a second photocurable adhesive layer is arranged at the edge of the second wall surface, and the first photocurable adhesive layer and the second photocurable adhesive layer have substantially the same shape.