MOF-derived bimetallic oxide / nitrogen-doped carbon material and preparation method thereof
The MOF-derived bimetal oxide/nitrogen-doped carbon material inhibits the shuttle of polysulfides in lithium-sulfur batteries, solves the problem that traditional separators cannot effectively block, and significantly improves the electrochemical performance and capacity stability of lithium-sulfur batteries.
Patent Information
- Application Number
- CN202411000892.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-22
AI Technical Summary
Traditional commercial polyolefin separators cannot effectively block the shuttle of polysulfides between the positive and negative electrodes, resulting in rapid capacity fading of lithium-sulfur batteries.
Design a MOF-derived bimetal oxide/nitrogen-doped carbon material to inhibit the dissolution of polysulfides in the electrolyte through the nitrogen-doped carbon system and the polarity of oxygen atoms, thereby inhibiting the shuttle of polysulfides. CoNi ZIFs are used as precursors to prepare nanocube composites through heat treatment.
It effectively suppresses the shuttle effect of polysulfides and improves the electrochemical performance and capacity stability of lithium-sulfur batteries.
Smart Images

Figure CN118825451A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery separator materials, and in particular to a MOF-derived bimetallic oxide / nitrogen-doped carbon material and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have become widely used batteries in the commercial market due to their high safety and stability. However, limited energy density and severe lithium shortage make it difficult to meet the growing demand for energy storage. Lithium-sulfur batteries are one of the candidates to replace lithium batteries and have attracted much attention due to their high theoretical specific energy, low cost, and environmental friendliness. However, the shuttle effect caused by the dissolution of lithium polysulfides in organic electrolytes and the slow kinetics of LiPSs over-cycling conversion have seriously hindered the practical application of lithium-sulfur batteries.
[0003] In order to improve the electrochemical performance of lithium-sulfur batteries, researchers have made a lot of efforts in recent years, such as designing suitable sulfur carriers, designing materials for diaphragm modification, and developing new electrolyte design materials for the protection of lithium metal anodes. In particular, the modification of diaphragms has been proven to be an effective method to inhibit the shuttle effect. Traditional commercial polyolefin diaphragms cannot effectively block the shuttle of polysulfides between the positive and negative electrodes, resulting in rapid capacity decay of lithium-sulfur batteries.
[0004] In recent years, metal organic frameworks have become common precursors for the preparation of porous carbon, metal oxides, metal sulfides and metal selenides due to their high specific surface area and designability. These derivatives have been widely studied in the field of lithium-sulfur batteries and have shown excellent performance.
[0005] Based on this, the present application aims to design a MOF-derived bimetallic oxide / nitrogen-doped carbon material for lithium-sulfur battery separator modification, utilizing the polarity of the nitrogen-doped carbon system and oxygen atoms to inhibit the dissolution of polysulfides in the electrolyte to a certain extent, thereby inhibiting the shuttling of polysulfides. Summary of the invention
[0006] The object of the present invention is to provide a MOF-derived bimetallic oxide / nitrogen-doped carbon material and a preparation method thereof to inhibit the shuttling of polysulfides.
[0007] The present application discloses a MOF-derived bimetallic oxide / nitrogen-doped carbon material and a preparation method thereof, comprising the following steps: S1 Co(NO3)2·6H2O and Ni(NO3)2·6H2O were weighed in proportion and placed in a beaker containing methanol, and then dispersed by ultrasonication until fully dissolved to obtain solution A; S2: Weigh 2-methylimidazole in proportion and dissolve it in methanol, and perform ultrasonication until it is completely dissolved to obtain solution B; S3: Solution A and Solution B were mixed, stirred at room temperature for 12 h to obtain a new solution, and then centrifuged to obtain a dark purple slurry, which was washed three times with ethanol; S4 dries the product of S3 in an oven to obtain the precursor CoNi ZIFs; S5 The CoNi ZIFs are placed in a crucible and heat treated to obtain a nanocube composite material.
[0008] Preferably, in step S1, the molar ratio of Co(NO3)2·6H2O to Ni(NO3)2·6H2O is 1:1.
[0009] Preferably, the mass volume ratio of 2-methylimidazole to methanol in step S2 is 9-10 g:10-15 ml.
[0010] Preferably, the centrifugation system in step S3 is: centrifugal speed is 7500-8500 r / min, and the centrifugal time is 5-15 min.
[0011] Preferably, the drying temperature in step S4 is 60-80° C., and the reaction time is 10-18 hours.
[0012] Preferably, the heat treatment system in step S5 is: in an air atmosphere, the temperature is raised to 300-400° C. at a rate of 1° C. / min, and the reaction time is 2-4 hours.
[0013] The advantage of the present invention is that the bimetallic center is used to provide more active sites for the reaction, and the polarity of the nitrogen-doped carbon system and oxygen atoms is used to inhibit the dissolution of polysulfides in the electrolyte to a certain extent, thereby inhibiting the shuttling of polysulfides. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0015] Figure 1 Shown is a schematic diagram of the material synthesis route of the present application; Figure 2 Shown is the XRD pattern of the composite material obtained in Example 1; Figure 3 Shown is the SEM spectrum of the material obtained in Example 1; In the figure: Figure 3 (a) is the spectrum of CoNi ZIFs; Figure 3(b) is the spectrum of Co3O4-NiO / NC. DETAILED DESCRIPTION
[0016] The following will describe the technical solutions in the embodiments of the present invention in detail in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] Example 1 S1 Weigh 291.0 mg Co(NO3)2·6H2O and 297.5 mg Ni(NO3)2·6H2O into a beaker containing 10 ml methanol and disperse them under ultrasonic until fully dissolved to obtain solution A; S2 Weigh 9.08 g of 2-methylimidazole and dissolve it in 10 ml of methanol, and sonicate until it is completely dissolved to obtain solution B; S3: Solution A and Solution B were mixed, stirred at room temperature for 12 h to obtain a new solution, centrifuged at 8000 r / min for 5 min to obtain a dark purple slurry, and washed three times with ethanol; S4 dried the product of S3 in an oven at 60 °C for 12 h to obtain the precursor CoNi ZIFs; S5 CoNi ZIFs were placed in a crucible, and the temperature was raised to 350°C at a rate of 1°C / min in an air atmosphere for 2 h to obtain a Co3O4-NiO / NC composite material. Example 2
[0018] S1 Co(NO3)2·6H2O and Ni(NO3)2·6H2O were weighed in a molar ratio of 1:1 and placed in a beaker containing methanol, and then dispersed by ultrasonic until fully dissolved to obtain solution A; S2: Weigh 2-methylimidazole in a mass volume ratio of 9 g:10 ml and dissolve it in methanol, and ultrasonicate until it is completely dissolved to obtain solution B; S3: Solution A and Solution B were mixed, stirred at room temperature for 12 h to obtain a new solution, centrifuged at 7500 r / min for 10 min to obtain a dark purple slurry, and washed three times with ethanol; S4 dried the product of S3 in an oven at 70 °C for 10 h to obtain the precursor CoNi ZIFs; S5 CoNi ZIFs were placed in a crucible, and the temperature was raised to 350°C at a rate of 1°C / min in an air atmosphere for 3 h to obtain a Co3O4-NiO / NC composite material. Example 3
[0019] S1 Co(NO3)2·6H2O and Ni(NO3)2·6H2O were weighed in a molar ratio of 1:1 and placed in a beaker containing methanol, and then dispersed by ultrasonic until fully dissolved to obtain solution A; S2: Weigh 2-methylimidazole in a mass volume ratio of 10 g:15 ml and dissolve it in methanol, and ultrasonicate until it is completely dissolved to obtain solution B; S3: Solution A and Solution B were mixed, stirred at room temperature for 12 h to obtain a new solution, centrifuged at 8000 r / min for 5 min to obtain a dark purple slurry, and washed three times with ethanol; S4 dried the product of S3 in an oven at 60 °C for 12 h to obtain the precursor CoNi ZIFs; S5 CoNi ZIFs were placed in a crucible, and the temperature was raised to 350°C at a rate of 1°C / min in an air atmosphere for 2 h to obtain a Co3O4-NiO / NC composite material.
[0020] The Co3O4-NiO / NC composite material of Example 1 was subjected to XRD test. Figure 2 The results shown show that Co3O4-NiO / NC has multiple peaks, which are attributed to Co3O4 (PDF No. 65-3103) and NiO (PDF No. 65-2901), respectively, which preliminarily confirms the existence of two phases Co3O4 and NiO in the Co3O4-NiO / NC structure.
[0021] Then, SEM test was performed on Example 1. Figure 3 The results show that the morphology of CoNi ZIFs is as follows: Figure 3 As shown in (a), it presents a regular dodecahedron with a smooth surface. Figure 3 (b) shows the morphology of the Co3O4-NiO / NC material after oxidation. It can be seen that after oxidation, the specific surface area of Co3O4-NiO / NC increases, the surface becomes rough, and the pores increase accordingly. The porous nature of the material can increase the active sites in the battery reaction and has a good capture effect on polysulfides, thereby improving the electrochemical performance of lithium-sulfur batteries.
[0022] This implementation mode is only an exemplary description of this patent and does not limit its protection scope. Personnel in this field may also make partial changes to it. As long as it does not exceed the spirit of this patent, it shall be regarded as an equivalent replacement of this patent and shall be within the protection scope of this patent.
Claims
1. A MOF-derived bimetallic oxide / nitrogen-doped carbon material and a method for preparing the same, characterized in that: The steps include: S1 Co(NO3)2·6H2O and Ni(NO3)2·6H2O were weighed in proportion and placed in a beaker containing methanol, and then dispersed by ultrasonication until fully dissolved to obtain solution A; S2: Weigh 2-methylimidazole in proportion and dissolve it in methanol, and perform ultrasonication until it is completely dissolved to obtain solution B; S3: Solution A and Solution B were mixed, stirred at room temperature for 12 h to obtain a new solution, and then centrifuged to obtain a dark purple slurry, which was washed three times with ethanol; S4 dries the product of S3 in an oven to obtain the precursor CoNi ZIFs; S5 The CoNi ZIFs are placed in a crucible and heat treated to obtain a nanocube composite material.
2. The method for preparing a composite material according to claim 1, characterized in that: In the step S1, the molar ratio of Co(NO3)2·6H2O to Ni(NO3)2·6H2O is 1:
1.
3. The method for preparing a composite material according to claim 1, characterized in that: The mass volume ratio of 2-methylimidazole to methanol in step S2 is 9-10 g:10-15 ml.
4. The method for preparing a composite material according to claim 1, characterized in that: The centrifugation system in step S3 is: centrifugal speed is 7500-8500 r / min, and the centrifugal time is 5-15 min.
5. The method for preparing a composite material according to claim 1, characterized in that: The drying temperature in step S4 is 60-80° C., and the reaction time is 10-18 hours.
6. The method for preparing a composite material according to claim 1, characterized in that: The heat treatment system in step S5 is: in an air atmosphere, the temperature is raised to 300-400° C. at a rate of 1° C. / min, and the reaction time is 2-4 hours.