Preparation method of high-porosity polyolefin microporous membrane
Through three-layer co-extrusion technology and material optimization, a polyolefin microporous membrane with high porosity and uniform mechanical properties was prepared, which solved the problem of insufficient battery separator performance and improved porosity, strength and heat resistance, making it suitable for batteries. Diaphragm applications.
Patent Information
- Application Number
- CN202410802470.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-20
AI Technical Summary
Existing microporous membrane preparation technology is difficult to optimize porosity, flexibility, heat resistance and other properties in the battery field, resulting in insufficient battery separator performance and difficulty in meeting high performance and safety requirements.
Using three-layer co-extrusion technology, ultra-high molecular weight polyethylene is used as the surface material. PET and inorganic particles are blended and granulated to prepare the core layer together with polypropylene. By optimizing the material ratio and process conditions, it forms a core layer with high porosity and uniform mechanical properties. of polyolefin microporous membrane.
It achieves a synergistic improvement in the porosity, strength and heat resistance of the microporous membrane, eliminates anisotropic differences, meets the high performance requirements of battery separators, and is convenient and stable, making it suitable for industrial production.
Smart Images

Figure CN118825548A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of battery materials, and in particular to a method for preparing a high-porosity polyolefin microporous membrane that can be used for positive and negative electrode separators of batteries. Background Art
[0002] In recent years, China's microporous membrane industry has entered a period of rapid growth. The scale of engineering applications in the fields of seawater desalination, water treatment, and sewage reuse has expanded rapidly. Many large-scale membrane water supply projects, sewage reuse projects, and seawater desalination projects with landmark significance have been built one after another. At the same time, microporous membranes are used as diaphragms to separate positive and negative electrodes in secondary batteries, becoming one of the four key materials for battery composition. The performance of microporous diaphragms determines the interface structure, internal resistance, and other properties of the battery.
[0003] The battery field has put forward higher requirements for the performance of microporous membranes. The size and size distribution of the porosity of microporous membranes are one of the important factors affecting battery performance. By controlling the porosity of the diaphragm, a balance between battery capacity and cycle life can be achieved. The porosity of the current commercial traditional lithium battery diaphragms is concentrated between 35% and 55%. Low porosity and / or small size affect the fluidity of the electrolyte and the ability of ion shuttles, the battery discharge rate will be reduced, and the battery capacity will decrease. However, excessive porosity and / or excessive size cannot block the flow of dissolved substances in the electrolyte, resulting in poor separation of the positive and negative electrodes, which will affect the cycle life of the battery. In practice, it is difficult to maintain high battery performance. At the same time, the diaphragm will shrink due to excessive porosity, reducing its safety performance. At the same time, the battery production needs to undergo hot and cold deformation and winding processing, and the battery operation process will face battery heat generation. The flexibility, temperature resistance and deformation resistance of the microporous membrane at high porosity also need to meet the requirements. It is also necessary to eliminate the anisotropy difference of the microporous membrane, and the various performance indicators in the horizontal and vertical directions are basically consistent.
[0004] Existing microporous membrane preparation technology makes it difficult to achieve the above-mentioned performance optimization and improvement of microporous membranes in batteries. Extrusion molding is currently the most commonly used and economical preparation technology for microporous membranes. Due to the poor fluidity of polymer raw materials and uneven processing problems such as extrusion molding, the improvement of porosity and flexibility is limited. At the same time, the extrusion process is prone to increase in anisotropy differences, all of which limit the application of microporous membranes as battery separators. Microporous membrane preparation methods and products that are more suitable for battery separators are in urgent need of optimization and development.
[0005] To this end, this application is filed. Summary of the invention
[0006] In view of the above problems in the prior art, the present invention provides a method for preparing a high-porosity polyolefin microporous membrane. The obtained microporous membrane not only has high porosity and high conductivity, but also has low dimensional change and balanced and reliable mechanical properties.
[0007] The method for preparing the high-porosity polyolefin microporous membrane of the present invention comprises the following steps:
[0008] S1: Preparation of surface material: fully mix the surface material including ultra-high molecular weight polyethylene (PE), antioxidant, plasticizer and organic solvent, keep the temperature at 60-100°C, continue to heat to 170-200°C, evacuate after complete dissolution, keep the temperature for later use;
[0009] S2: Preparation of core layer material: blending inorganic particle powder with a particle size of less than 0.05 μm with polyethylene terephthalate (PET) to form a granulation masterbatch, and mixing the granulation masterbatch with polypropylene (PP) for standby use; wherein the mass proportion of inorganic particles in the blended granulation raw materials is 0.5-5%, and the granulation masterbatch accounts for 10-25% of the total mass of the granulation masterbatch and PP;
[0010] S3: adopting a three-layer co-extrusion method to form the surface layer materials on both sides of the core layer material, respectively, to obtain a hot film with a three-layer structure of surface layer-core layer-surface layer, and then longitudinally stretching, transversely stretching and heat setting after cooling and drying to obtain a high-porosity polyolefin microporous membrane; wherein the core layer material accounts for 5-20% of the total mass of the core layer material and the surface layer material;
[0011] There is no particular order in which the above steps S1 and S2 are performed.
[0012] As some exemplary preferred schemes, the degree of disentanglement of the surface material prepared in step S1, expressed as motor torque, reaches a motor torque of 33.9 to 101.7N.
[0013] As some exemplary preferred embodiments, the ultra-high molecular weight polyethylene is selected from 6 ~2.0×10 6 g / mol, ultra-high molecular weight polyethylene (PE) with an intrinsic viscosity of 5.0 to 15.0 dl / g in decalin at 135°C.
[0014] As some exemplary preferred schemes, in step S1, the stirring rate during the process of fully mixing and dissolving the surface raw materials is 50-80 rpm, and the stirring rate during vacuuming after dissolution is 2-10 rpm.
[0015] As some exemplary preferred schemes, after the surface raw materials are fully mixed and completely dissolved, they are evacuated to 0.0 to -0.05 MPa, which can meet the requirements of good preservation.
[0016] As some exemplary preferred schemes, the antioxidant is selected from one or more of antioxidant 1010, antioxidant 1076, antioxidant 168, antioxidant 300, antioxidant GS, Weston 705, antioxidant 702, antioxidant 3114, and antioxidant 626.
[0017] As some exemplary preferred schemes, the plasticizer is selected from organic acid ester plasticizers, specifically selected from one or more of dioctyl phthalate, dibutyl phthalate, dioctyl sebacate, dioctyl sebacate, dioctyl adipate, acetyl tributyl citrate, dimethyl phthalate, tricresyl phosphate, and diisononyl phthalate.
[0018] As some exemplary preferred embodiments, the organic solvent is selected from hydrogenated naphthalene organic solvents, specifically selected from one or more of decalin and tetralin.
[0019] As some exemplary preferred schemes, the ratio of the surface layer raw materials in S1 of the present invention is, by mass, PE 15-30%, antioxidant 0.075-0.5%, plasticizer 0.045-0.6%, organic solvent 60-90%, and the sum of the mass of the above surface layer raw materials is 100%.
[0020] As some exemplary preferred schemes, in S2 of the present invention, the mass proportion of inorganic particles in the blended granulation raw materials is 0.5-5%, and the granulation masterbatch accounts for 10-25% of the total mass of the granulation masterbatch and PP.
[0021] As some exemplary preferred embodiments, the polypropylene is selected from isotactic polypropylene with an average molecular weight of 0.5×10 6 ~5.0×10 6 , the melt index is 1.0~5.0g / 10min.
[0022] As some exemplary preferred embodiments, the inorganic particles are selected from inorganic ceramic particles, specifically selected from one or more of montmorillonite, kaolinite, talc, sodium bicarbonate, sodium carbonate, calcium carbonate, barium sulfate, aluminum oxide, silicon dioxide, and magnesium oxide.
[0023] As some exemplary preferred schemes, in S3 of the present invention, the temperatures of the surface layer material and the core layer material in the extruder are 120-170° C. and 180-270° C., respectively.
[0024] As some exemplary preferred schemes, in S3 of the present invention, when the surface layer material and the core layer material are co-extruded, the temperature of the co-extrusion die is 170-270°C.
[0025] As some exemplary preferred schemes, in S3 of the present invention, the hot film cooling process adopts a rapid cooling method, and the rapid cooling temperature is 5 to 25°C.
[0026] As some exemplary preferred schemes, in S3 of the present invention, the longitudinal stretching ratio is 4 to 10 times, the temperature is 110 to 150°C, the transverse stretching ratio is 3 to 10 times, the temperature is 120 to 150°C, and the heat setting temperature is 110 to 130°C.
[0027] The present invention also provides a microporous membrane obtained by the above method, which has a porosity of ≥75%, a thickness of 6 to 100 microns, a uniform three-dimensional cross-fiber structure on the surface, a melon-shaped pore shape, a pore diameter between 100 and 600 nm, and a longitudinal and transverse tensile strength greater than 480 kg f / cm 2 The thermal shrinkage in both longitudinal and transverse directions at 120℃×1h is no more than 3%.
[0028] Compared with the prior art, the present invention has at least the following beneficial effects:
[0029] The present invention combines three-layer co-extrusion technology, uses ultra-high molecular weight PE as the main material to prepare the surface layer, and simultaneously PET+inorganic particles are blended and granulated with PP to prepare the core layer, and optimizes the material ratio and two-stage process conditions, successfully achieving a synergistic improvement in the porosity, strength, and heat resistance of the microporous membrane, and effectively eliminating anisotropy differences, and highly improving the comprehensive performance, so that the microporous membrane obtained by the method of the present invention can particularly meet the high performance requirements of the battery separator, and the preparation method also has convenience and stability, which is conducive to industrial production, and at the same time has a wider application potential and value. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0031] Figure 1 The figure is a comparison of the appearance of a conventional commercial wet-process diaphragm and the microporous membrane of the present invention. Among them, a is the appearance of a conventional commercial wet-process diaphragm, and b is the appearance of a microporous membrane of the present invention.
[0032] Figure 2 This is a diagram of the pore structure formed by the enlarged gap between the PET and PP phases in the core layer of the present invention. DETAILED DESCRIPTION
[0033] For ease of understanding, the microporous membrane of the present invention will be described more comprehensively below, and examples of the present invention will be given, but the scope of the present invention is not limited thereby.
[0034] It should be pointed out that although the microporous membrane of the present invention is optimized and designed based on the application direction of battery separators, so that it can achieve more advantageous performance effects in batteries (such as lithium-ion batteries, semi-solid batteries, etc.) than general microporous membranes, its application is not limited to this. In related fields such as seawater desalination, medical selective filtration membranes, reverse osmosis membranes, etc., if the microporous membrane has performance indicators that are basically equivalent to those of the present invention, it can also be well applied.
[0035] The method for preparing a high-porosity polyolefin microporous membrane provided by the present invention comprises the following steps:
[0036] S1: Preparation of surface material: fully mix the surface material including ultra-high molecular weight polyethylene (PE), antioxidant, plasticizer and organic solvent, keep the temperature at 60-100°C, continue to heat to 170-200°C, evacuate after complete dissolution, keep the temperature for later use;
[0037] S2: Preparation of core layer material: Inorganic particle powder with a particle size of less than 0.05 μm is blended with polyethylene terephthalate (PET) to form a granulation masterbatch, and the granulation masterbatch is mixed with polypropylene (PP) for standby use;
[0038] S3: adopting a three-layer co-extrusion method to form the surface layer materials on both sides of the core layer material, respectively, to obtain a hot film with a three-layer structure of surface layer-core layer-surface layer, and then longitudinally stretching, transversely stretching and heat setting after cooling and drying to obtain a high-porosity polyolefin microporous membrane; wherein the core layer material accounts for 5-20% of the total mass of the core layer material and the surface layer material;
[0039] There is no particular order in which the above steps S1 and S2 are performed.
[0040] The microporous membrane of the present invention adopts a three-layer structure design, and the selection and proportion of the three-layer structure materials are designed at the same time. On the basis of ensuring the high porosity of the surface layer, the core layer has good heat resistance and mechanical properties to ensure the performance balance of the microporous membrane. The surface layer accounts for a large proportion, ensuring a high porosity, contributing to most of the porosity of the entire microporous membrane, which can ensure the fluidity of the electrolyte and make the battery have excellent ionic conductivity. The core layer accounts for a relatively thin proportion and has a smaller porosity than the surface layer, which is conducive to blocking the flow of solutes in the electrolyte and plays a good isolation effect. Therefore, the reasonable structural difference design enables the battery to achieve a good balance between safety and performance indicators.
[0041] The surface layer uses ultra-high molecular weight PE as the main material. The ultra-high molecular weight ensures the flexibility and later mechanical properties of the material. Through the two-stage heating and insulation design (after insulation at 60-100℃, continue to heat up to 170-200℃ for insulation), the polymer raw material can achieve good swelling in the first stage and good dissolution in the second stage. It can swell and dissolve in high-boiling point solvents and fully disentangle, which provides a guarantee for the ultra-high molecular weight PE to have good processing fluidity in the extrusion process. In the subsequent stretching process, the excellent disentanglement between molecules ensures the generation of high porosity. At the same time, because PE does not have a branched structure, it brings good copolymer orientation and avoids the anisotropic difference of the microporous membrane.
[0042] The core layer firstly blends PET with small-size inorganic particles (particle size less than 0.05μm) to form granules. During the processing, the inorganic particles play a heterogeneous nucleation role on PET, which improves the crystallization behavior of PET and makes the particle size of the PET crystal system smaller at a lower temperature. When the granulation masterbatch is blended with PP, PET as a dispersed phase carries the inorganic particles and is evenly dispersed in the PP phase. Due to the incompatibility between the PET and PP crystal regions and amorphous regions, there is only a weak interfacial force between the two phases. Under the subsequent tensile force, the gap between the PET and PP phases is enlarged, forming more pores around the PET dispersed phase (such as Figure 2 ), further increasing the porosity of the core layer. At the same time, the PP resin forms a good coating effect with PET in this process. After stretching, the benzene rings and inorganic particles in the PET structure play a good rigidity role in the core layer, further improving the toughness and heat resistance of the microporous membrane. The PP of the core layer also has a polymer structure closer to the PE of the surface layer, so that the surface layer and the core layer have good compatibility in the three-layer co-extrusion molding, and the interlayer matching is better. At the same time, the presence of more side chains in PP promotes its cross-linking with PET and PP respectively, so that both the inner layer and the interlayer have good cohesion.
[0043] On the basis of the above, the appropriate mass ratio of each layer of material ensures the good processability of each layer of material and the reasonable matching between layers, which provides the premise and guarantee for obtaining a microporous membrane with improved comprehensive performance.
[0044] As some exemplary preferred schemes, the degree of disentanglement of the surface material prepared in step S1 is expressed by the motor torque, and the torsion fraction is 15% to 45% under the extruder screw motor torque of 226N, that is, the motor torque reaches 33.9 to 101.7N.
[0045] The degree of disentanglement of the surface material mainly refers to the disentanglement of PE. The energy required for the molecules to gather due to mutual attraction is called cohesive energy. Cohesive energy is the intermolecular force generated by van der Waals force and hydrogen bond, and is often used as the magnitude of intermolecular force. The dissolution process of high molecular polymers can be understood as the process in which the intermolecular forces are broken up by solvent molecules. The dissolution process of high molecular polymers generally takes a long time, especially the dissolution process of ultra-high molecular weight PE. The small solvent molecules slowly penetrate into the interior of the resin particles at a certain temperature, which is manifested as the particles swelling due to the entry of the solvent. This process is called the swelling stage. As the temperature rises, the solvent further penetrates into the molecular chains, weakening the strong interaction between the macromolecular chains. The more fully the solvation is, the system enters the uniform dissolution stage. Finally, after the molecules of ultra-high molecular weight PE are largely disentangled under the action of solvation, it presents a transparent state with a certain flow state. The degree of disentanglement not only affects the difficulty of extrusion processing, but also affects whether the film forming process is affected by the tendency of extrusion force and produces anisotropic differences due to its correlation with molecular cohesion. The appropriate degree of disentanglement is also conducive to cross-linking with the core layer PP, while also taking into account the toughness and strength of the surface layer itself. The present invention selects two-stage suitable insulation temperature sections to promote PE to achieve the target degree of disentanglement.
[0046] As some exemplary preferred solutions, we also optimized the matching selection of ultra-high molecular weight polyethylene that can achieve the target disentanglement degree, and selected the ultra-high molecular weight polyethylene with an average molecular weight of 0.5×10 6 ~2.0×10 6 g / mol, ultra-high molecular weight polyethylene (PE) with an intrinsic viscosity of 5.0 to 15.0 dl / g in decalin at 135° C. Suitable PE raw material selection is conducive to ensuring sufficient disentanglement under the conditions of the present invention that are easier to operate.
[0047] As some exemplary preferred schemes, in order to promote the mixing of the raw materials during the untangling process, a certain stirring rate can be maintained. In step S1, the stirring rate can be 50-80 rpm during the process of sufficient mixing and dissolution of the surface raw materials, and the stirring rate of vacuuming after dissolution is 2-10 rpm.
[0048] The type of antioxidant in S1 of the present invention is generally not limited, and materials with good antioxidant effects on PE can be selected from the prior art. As some exemplary preferred schemes, one or more of antioxidant 1010, antioxidant 1076, antioxidant 168, antioxidant 300, antioxidant GS, Weston 705, antioxidant 702, antioxidant 3114, and antioxidant 626 can be selected.
[0049] The type of plasticizer in S1 of the present invention is generally not limited, and materials with good plasticizing effect on PE can be selected from the prior art. Among them, organic acid ester plasticizers belong to external plasticizers, which have the characteristics of high boiling point, low volatility, and the ability to form a solid solution with PE. They can be used as a preferred plasticizer of the present invention. As some exemplary preferred schemes, they can be selected from one or more of dioctyl phthalate, dibutyl phthalate, dioctyl sebacate, dioctyl sebacate, dioctyl adipate, tributyl acetylcitrate, dimethyl phthalate, tricresyl phosphate, and diisononyl phthalate.
[0050] The type of organic solvent in S1 of the present invention is generally not limited, and materials with good compatibility with PE can be selected from the prior art. Among them, hydrogenated naphthalene organic solvents can be used as a preferred organic solvent of the present invention because they have certain plasticizing and modifying effects on PE, can assist in adjusting the flexibility and hardness of PE, are environmentally friendly and easy to recycle, and can be selected from one or more of decalin and tetralin as some exemplary preferred schemes.
[0051] As some exemplary preferred schemes, the ratio of the surface layer raw materials in S1 of the present invention is, by mass, PE 15-30%, antioxidant 0.075-0.5%, plasticizer 0.045-0.6%, organic solvent 60-90%, and the sum of the mass of the above surface layer raw materials is 100%.
[0052] As some exemplary preferred solutions, in S2 of the present invention, the mass proportion of inorganic particles in the blended granulation raw materials is 0.5-5%, and the granulation masterbatch accounts for 10-25% of the total mass of the granulation masterbatch and PP. A suitable ratio of PP to inorganic particles is conducive to forming a granulation masterbatch with a good coating structure.
[0053] As some exemplary preferred solutions, we also optimized the PP that can better match the PE of S1, specifically isotactic polypropylene with an average molecular weight of 0.5×10 6 ~5.0×10 6 The melt index is 1.0-5.0 g / 10 min, which can achieve good interlayer bonding with the dissolved and disentangled PE during the three-layer co-extrusion process.
[0054] The types of inorganic particles in S2 of the present invention are generally not limited, and materials with good particle size and stable electrical properties can be selected from the prior art. Among them, inorganic ceramic particles can be used as a preferred material due to their excellent performance stability. As some exemplary preferred schemes, they can be selected from one or more of montmorillonite, kaolinite, talc, sodium bicarbonate, sodium carbonate, calcium carbonate, barium sulfate, aluminum oxide, silicon dioxide, and magnesium oxide.
[0055] In order to further ensure the safe and stable formation of the microporous membrane structure during the three-layer co-extrusion process, the present invention further studies the optimized operating conditions of the three-layer co-extrusion process.
[0056] As some exemplary preferred schemes, in S3 of the present invention, the temperatures of the surface layer material and the core layer material in the extruder are maintained at 120-170°C and 180-270°C, respectively, so that the materials have good matching fluidity, formability, and interlayer bonding during extrusion.
[0057] As some exemplary preferred schemes, in S3 of the present invention, when the surface layer material and the core layer material are co-extruded, in order to balance the temperature between different materials, the temperature of the co-extrusion die can be maintained at 170-270°C.
[0058] As some exemplary preferred schemes, in S3 of the present invention, the hot film cooling process can adopt a rapid cooling method, and the temperature of the rapid cooling roller can be maintained at 5 to 25° C., which is convenient for the hot film to cool and shape quickly without causing cold brittleness.
[0059] As some exemplary preferred schemes, in S3 of the present invention, the longitudinal stretching, transverse stretching and heat setting processes are also the processes of forming high porosity. In order to facilitate the stable formation and stable retention of high porosity while taking into account the pore size and mechanical properties after film formation, the longitudinal stretching multiple is selected to be 4 to 10 times, the temperature is 110 to 150°C, the transverse stretching multiple is selected to be 3 to 10 times, the temperature is 120 to 150°C, and the heat setting temperature is 110 to 130°C.
[0060] According to the test, the microporous membrane obtained by the present invention can achieve a porosity of ≥75%, a thickness of 6 to 100 microns, a uniform three-dimensional cross-fiber structure on the surface, a melon-shaped pore shape, a pore diameter between 100 and 600 nm, and a longitudinal and transverse tensile strength greater than 480 kg f / cm 2 The thermal shrinkage in both longitudinal and transverse directions at 120℃×1h is no more than 3%.
[0061] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0062] The chemical raw materials involved in the following examples and comparative examples are all prior art and are commercially available. The experimental devices, test devices, etc. involved in the following examples and comparative examples are all conventional devices in the art, without special requirements and limitations.
[0063] Example 1
[0064] S1: Preparation of surface layer material: a material containing an average molecular weight of 0.5×10 6 Polyethylene (PE), antioxidant 1010, dioctyl phthalate, and tetralin are added into a premixing kettle in a ratio of 30%, 0.3%, 0.2%, and 69.5% by mass and mixed thoroughly. The stirring rate is 50 rpm. After being kept at 70°C for 2 h, the temperature is further increased to 175°C at a heating rate of 10°C / 0.5h for full dissolution. After complete dissolution, the stirring rate is reduced to 5 rpm, and the mixture is quickly evacuated to -0.05 MPa and kept warm for standby use.
[0065] S2: Preparation of core layer material: montmorillonite granules with a particle size of less than 0.05 μm and polyethylene terephthalate (PET) are blended and granulated at a mass ratio of 1.8:98.2 to form a granulation masterbatch, and the granulation masterbatch is mixed with polypropylene (PP) at a mass ratio of 1:9 for standby use;
[0066] S3: The surface layer material obtained in step S1 and the core layer material obtained in step S2 are respectively sent to an extruder for melt extrusion. The extruder uses a three-layer die for co-extrusion. The temperature of the die is set to 180°C. The surface layer material at the three-layer die is symmetrically formed on both sides of the core layer material to obtain a hot film with a three-layer structure of surface layer-core layer-surface layer. The ratio of the surface layer material to the core layer material is 85:15. The hot film is cast into a primary sheet on a 20°C rapid cooling roller. The primary sheet after casting is sent to a hot air drying system to remove the solvent from the surface layer, and then the primary sheet is longitudinally stretched, transversely stretched and heat-set respectively. The longitudinal stretching ratio is 30 times, the temperature is 120°C, the transverse stretching ratio is 6 times, the temperature is 130°C, and the heat setting temperature is 110°C. Then, it is cooled and rolled up, and slit to obtain a high-porosity polyolefin microporous membrane. The thickness of the obtained microporous membrane is 6 microns.
[0067] Embodiments 2 to 8
[0068] The preparation parameters of Example 1 were changed to obtain surface materials with different compositions, and the differences in the disentanglement degrees of the surface materials with different compositions were detected.
[0069] Comparative Examples 1-2
[0070] The preparation parameters of Example 1 were changed to obtain surface materials with different compositions, and the differences in the disentanglement degrees of the surface materials with different compositions were detected.
[0071] The differences in the preparation of the surface layer materials of Examples 1 to 8 and Comparative Examples 1 to 2 and the evaluation results of the degree of disentanglement are shown in Table 1.
[0072] Table 1
[0073]
[0074]
[0075] Table 1 provides the effects of different surface material compositions and preparation conditions on the degree of PE disentanglement. The torque of the surface extruder screw motor at full torque used in the present invention is 226N, and the appropriate degree of disentanglement enables the surface material to be extruded and molded at an appropriate torque. As shown in Examples 1 to 8, the surface material composition selected by the present invention can obtain an appropriate degree of disentanglement through a two-stage insulation method, and is molded under an appropriate torque. The torque is moderate to ensure that the surface molding eliminates the orientation effect and maintains sufficient toughness and strength of the surface itself. Comparative Examples 1 to 2 show that inappropriate material composition and preparation conditions lead to excessive torque in the molding process. Although excessive force ensures smooth molding of the surface, it easily leads to molecular reorientation in the extrusion molding direction, which is not conducive to the uniformity of tensile strength in MD and TD.
[0076] Figure 1 The surface morphology of the traditional commercial wet-process diaphragm is shown. Figure 1 a) and the apparent morphology of the microporous membrane of the present invention ( Figure 1 b) Structural differences. It can be seen that the PE surface layer prepared by the traditional commercial wet-process diaphragm has a coarser continuous polymer bundle, the degree of PE molecular disentanglement is poor, and the pores are larger and the porosity is lower after stretching and shaping. The continuous polymer bundles (three-dimensional cross-fiber structure) of the microporous membrane of the present invention are fewer and thinner, which provides sufficient strength support and introduces more pores. The pore morphology is melon-shaped, matching good tensile elasticity, and the major diameter of the pores is between 100-600nm.
[0077] Embodiments 9 to 19
[0078] The preparation parameters of Example 1 were changed to obtain core layer materials with different compositions, and the effects of the core layer materials with different compositions on the comprehensive properties of the microporous membrane were detected.
[0079] Comparative Examples 3-4
[0080] The preparation parameters of Example 1 were changed to obtain core layer materials with different compositions, and the effects of the core layer materials with different compositions on the comprehensive properties of the microporous membrane were detected.
[0081] The differences in the preparation of the core layer materials of Examples 1, 9 to 19 and Comparative Examples 3 to 4 and the effects on the comprehensive properties of the microporous membrane are shown in Table 2. In the present invention, the porosity, tensile strength and thermal shrinkage of the microporous membrane are all in accordance with GB / T36363-2018.
[0082] Table 2
[0083]
[0084]
[0085] Table 2 confirms the effect of pre-granulating inorganic particles by PET on the comprehensive performance of microporous membranes. Examples 9 to 19 show that the granulated masterbatch obtained within the control range of the present invention can bring higher porosity, tensile strength, and thermal shrinkage, and the performance difference between MD and TD is small. Comparative Example 3 is the case where inorganic particles are added in a non-granulated form, that is, montmorillonite, PET and PP are directly blended and extruded. Since PET has not successfully coated the inorganic particles in advance, and the two-phase interface of PET and PP supported by the dispersed phase cannot be formed, the dispersibility and crystallization behavior of the material are changed, and more inorganic particles are directly in contact with PP, resulting in a greatly reduced ability to form and orderly expand pores. Not only the porosity is reduced, but also the tensile strength and thermal shrinkage performance of the material are simultaneously reduced, and the anisotropy difference is also significantly increased. Comparative Example 4 is the case where inorganic particles are not introduced into the core layer material, so that the point dispersion and support effect of the inorganic particles in the core layer disappear, the crystallization behavior of PET is also reduced, the interface effect with PP is weakened, and the difficulty of dispersibility of PP resin becomes the dominant influencing factor. The performance indicators of the obtained membrane structure in various aspects are also greatly reduced.
[0086] Examples 20 to 27
[0087] In order to further comprehensively evaluate the influence of the surface layer and the core layer on the overall comprehensive performance within the control range of the present invention, the preparation parameters of Example 1 are further changed to obtain surface layer materials and core layer materials of different compositions, and the influence of different material compositions on the comprehensive performance of the microporous membrane is detected.
[0088] Comparative Examples 5 to 7
[0089] The preparation parameters of Example 1 were changed to obtain surface layer materials and core layer materials with different compositions, and the effects of different material compositions on the comprehensive properties of the microporous membrane were detected.
[0090] The differences in material preparation between Examples 20 to 27 and Comparative Examples 5 to 7 and their effects on the comprehensive properties of the microporous membrane are shown in Table 3.
[0091] Table 3
[0092]
[0093]
[0094] Table 3 confirms that within the control range of the present invention, a microporous membrane material with excellent comprehensive performance can be obtained, and high porosity is guaranteed and improved. As a battery separator, it shows excellent ionic conductivity, indicating that the stable structure and suitable pores promote the efficient transmission of ions in the separator. Comparative Examples 5-6 respectively show the impact of excessive matching on performance. Among them, the change in molecular weight in Comparative Example 5 may cause changes in the degree of disentanglement and the compatible matching between layers in the three-layer co-extrusion process. The imbalance in the proportion of the surface layer and the core layer material in Comparative Example 6 may lead to insufficient porosity. Furthermore, Comparative Example 7 uses PE to replace PET to coat and granulate the inorganic particles, and the interface effect of PET and PP disappears. It can be seen that the intermediate interface effect of PET and its special structure and performance also play an irreplaceable role in the microporous membrane system of the present invention and cannot be easily replaced.
[0095] The technical features of the above-described embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above-described embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. Although the embodiments of the present invention have been shown and described above, it can be understood that the above-described embodiments are exemplary and cannot be understood as limitations of the present invention. Those of ordinary skill in the art can change, modify, replace and deform the above-described embodiments within the scope of the present invention. In addition, those of ordinary skill in the art can combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples without contradiction.
Claims
1. A method for preparing a high-porosity polyolefin microporous membrane, comprising the following steps: S1: Preparation of surface material: fully mix the surface material including ultra-high molecular weight polyethylene (PE), antioxidant, plasticizer and organic solvent, keep the temperature at 60-100°C, continue to heat to 170-200°C, evacuate after complete dissolution, keep the temperature for later use; S2: Preparation of core layer material: Inorganic particle powder with a particle size of less than 0.05 μm is blended with polyethylene terephthalate (PET) to form a granulation masterbatch, and the granulation masterbatch is mixed with polypropylene (PP) for standby use; S3: A three-layer co-extrusion method is adopted to form the surface layer material on both sides of the core layer material to obtain a thermal film with a three-layer structure of surface layer-core layer-surface layer, and after cooling and drying, longitudinal stretching, transverse stretching and heat setting are performed to obtain a high-porosity polyolefin microporous membrane; wherein, The core material accounts for 5-20% of the total mass of the core material and the surface material; There is no particular order in which the above steps S1 and S2 are performed.
2. The method for preparing a high porosity polyolefin microporous membrane according to claim 1, characterized in that: The degree of disentanglement of the surface material prepared in step S1 is expressed by motor torque, reaching a motor torque of 33.9 to 101.7N.
3. The method for preparing a high porosity polyolefin microporous membrane according to claim 1, characterized in that: Ultra-high molecular weight polyethylene is selected from the average molecular weight of 0.5×10 6 ~2.0×10 6 g / mol, ultra-high molecular weight polyethylene (PE) with an intrinsic viscosity of 5.0 to 15.0 dl / g in decalin at 135°C.
4. The method for preparing a high-porosity polyolefin microporous membrane according to claim 1, characterized in that: In step S1, the stirring rate during the process of fully mixing and dissolving the surface raw materials is 50-80 rpm, and the stirring rate during vacuuming after dissolution is 2-10 rpm.
5. The method for preparing a high-porosity polyolefin microporous membrane according to claim 1, characterized in that: In step S1, the surface raw materials are fully mixed and completely dissolved, and then vacuumed to 0.0 to -0.05 MPa.
6. The method for preparing a high-porosity polyolefin microporous membrane according to claim 1, characterized in that: The antioxidant is selected from one or more of antioxidant 1010, antioxidant 1076, antioxidant 168, antioxidant 300, antioxidant GS, Weston 705, antioxidant 702, antioxidant 3114, and antioxidant 626; As some exemplary preferred embodiments, the plasticizer is selected from organic acid ester plasticizers, specifically selected from one or more of dioctyl phthalate, dibutyl phthalate, dioctyl sebacate, dioctyl sebacate, dioctyl adipate, tributyl acetyl citrate, dimethyl phthalate, tricresyl phosphate, and diisononyl phthalate; As some exemplary preferred embodiments, the organic solvent is selected from hydrogenated naphthalene organic solvents, specifically selected from one or more of decahydronaphthalene and tetrahydronaphthalene; As some exemplary preferred schemes, the ratio of the surface layer raw materials in S1 of the present invention is, by mass, PE 15-30%, antioxidant 0.075-0.5%, plasticizer 0.045-0.6%, organic solvent 60-90%, and the sum of the mass of the above surface layer raw materials is 100%; As some exemplary preferred solutions, in S2 of the present invention, the mass proportion of inorganic particles in the blended granulation raw materials is 0.5-5%, and the granulation masterbatch accounts for 10-25% of the total mass of the granulation masterbatch and PP; As some exemplary preferred embodiments, the inorganic particles are selected from inorganic ceramic particles, specifically selected from one or more of montmorillonite, kaolinite, talc, sodium bicarbonate, sodium carbonate, calcium carbonate, barium sulfate, aluminum oxide, silicon dioxide, and magnesium oxide.
7. The method for preparing a high-porosity polyolefin microporous membrane according to claim 1, characterized in that: Polypropylene is selected from isotactic polypropylene with an average molecular weight of 0.5×10 6 ~5.0×10 6 , the melt index is 1.0~5.0g / 10min.
8. The method for preparing a high-porosity polyolefin microporous membrane according to claim 1, characterized in that: In S3 of the present invention, the temperatures of the surface layer material and the core layer material in the extruder are 120-170° C. and 180-270° C., respectively; As some exemplary preferred embodiments, in S3 of the present invention, when the surface layer material and the core layer material are co-extruded, the temperature of the co-extrusion die is 170 to 270°C; As some exemplary preferred solutions, in S3 of the present invention, the hot film cooling process adopts a rapid cooling method, and the rapid cooling temperature is 5 to 25°C; As some exemplary preferred schemes, in S3 of the present invention, the longitudinal stretching ratio is 4 to 10 times, the temperature is 110 to 150°C, the transverse stretching ratio is 3 to 10 times, the temperature is 120 to 150°C, and the heat setting temperature is 110 to 130°C.
9. The microporous membrane obtained by the preparation method according to any one of claims 1 to 8 has a porosity of ≥75%, a thickness of 6 to 100 microns, a surface layer having a uniform three-dimensional cross-fiber structure, a melon-shaped pore morphology, a pore size between 100 and 600 nm, and a longitudinal and transverse tensile strength greater than 480 kg f / cm 2 The thermal shrinkage in both longitudinal and transverse directions at 120℃×1h is no more than 3%.
10. Use of the microporous membrane obtained by the preparation method according to any one of claims 1 to 8 in batteries and / or battery separators.
Citation Information
Patent Citations
Preparation method of three-layer composite lithium battery membrane
CN105024028A
Three-layer co-extruded lithium ionic battery diaphragm and preparation method thereof
CN107732100A
Microlayer membranes, battery separators, batteries, and related methods
CN112534635A
Three-layer lithium battery diaphragm and preparation method thereof
CN115764159A
Separator for electrochemical apparatus, electrochemical apparatus, and electronic apparatus
EP3965215A1