Zoned TWC catalyst for gasoline engine exhaust gas treatment

By adopting a partitioned Pd layer configuration in the three-way catalyst and controlling the weight ratio of alumina and CeZr oxide carriers, the problem of Pd adhesion and distribution is solved, and the performance of the catalyst is improved, especially significantly during cold start and transient driving stages. Reduced exhaust pollutant emissions.

CN118829482APending Publication Date: 2024-10-22JOHNSON MATTHEY PLC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380021305.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-13
Filing Date
2023-05-11
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

When existing three-way catalysts treat gasoline engine exhaust gas, especially during the cold start stage, it is difficult to effectively control the adhesion and distribution of Pd, resulting in poor catalytic performance and the inability to meet stringent emission regulations.

Method used

The TWC catalyst with partitioned Pd layer configuration is used to control the weight ratio of alumina and CeZr oxide carriers in the inlet and outlet wash layers, forcing most of the Pd substances to land on the carrier, forming a more uniform catalytic layer and improving catalysis. performance.

Benefits of technology

Emissions of exhaust pollutants are significantly reduced, especially during transient driving cycles and cold start phases, achieving better emission targets and improving the overall performance of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118829482A_ABST
    Figure CN118829482A_ABST
Patent Text Reader

Abstract

A catalyst article for treating an exhaust gas, the catalyst article comprising: a substrate comprising an inlet end, an outlet end, having an axial length L; a first catalytic region starting at the inlet end and extending less than the axial length L wherein the first catalytic region comprises a first platinum group metal (PGM) component, a first inorganic oxide, and optionally a first oxygen storage capacity (OSC) material; a second catalytic region starting at the outlet end and extending less than the axial length L wherein the second catalytic region comprises a second PGM component, optionally a second inorganic oxide and a second OSC material; and a third catalytic region; wherein the weight ratio of the first inorganic oxide to the optional first OSC material is greater than 1: 1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to catalytic articles useful for treating exhaust emissions from gasoline engines. Background Art

[0002] Internal combustion engines produce exhaust gases that contain a variety of pollutants, including hydrocarbons (HC), carbon monoxide (CO), and nitrogen oxides (“NO x ”). Emission control systems that include exhaust gas catalytic conversion catalysts are widely used to reduce the amount of these pollutants emitted into the atmosphere. A common catalyst used for gasoline engine exhaust treatment is the TWC (three-way catalyst). The TWC performs three main functions: (1) oxidation of CO; (2) oxidation of unburned HC; and (3) oxidation of NO x of restoration.

[0003] Typically, a three-way catalyst comprises a precious metal (PGM) such as palladium, rhodium, or platinum, or a combination thereof, an oxygen storage material (OSC; oxygen storage component) such as a cerium-zirconium mixed oxide and alumina. In some TWC catalysts, both OSC and alumina are used as support materials for the precious metals to improve dispersion, prevent PGM sintering, and / or prevent alloying if more than one precious metal is used in the same washcoat layer. However, in other TWC catalysts, PGMs are targeted on one of the support materials (alumina or OSC) to play some unique catalytic role in specific situations such as sudden changes in the exhaust air-fuel ratio (λ disturbance), play a light-off function during cold start cycles, etc. Therefore, there is a need to continue to develop catalysts that isolate different PGMs on different support materials to meet more stringent emission regulations, including normal engine operating conditions and special situations.

[0004] It is well known that the performance of TWC catalysts is affected by the oxidation state of the PGM. For example, metallic Rh is more active than rhodium oxide (Rh2O3). There is also much debate in the open literature about the optimal Pd oxidation state. It stands to reason that metallic Pd or palladium oxide is also beneficial, depending on the reaction conditions.

[0005] A typical method of "fixing" PGMs on a target support material is incipient wetness impregnation. That is, a diluted aqueous salt of PGM is impregnated into the pores of the support material, followed by drying and calcination to produce a powder containing PGMs. The powder is then slurried, mixed with another support slurry, wash-coated on a honeycomb substrate, and used as a catalyst through another calcination step. If multiple washcoats on the same substrate are calcined after each coating, two or even more rounds of calcination are performed to achieve initial sintering of the PGM nanoparticles.

[0006] Alternatively, hydrolysis methods are used to convert soluble PGM salts into insoluble species by changing the pH of the washcoat layer, precipitating the PGM onto the target support material. For example, rhodium nitrate can be converted to rhodium hydroxide by adding ammonia and precipitated onto alumina or CeZr oxide supports. However, this hydrolysis method is not sufficient to control Pd attachment, which may be due to the high Pd loading in typical TWC formulations.

[0007] The present invention solves the problem of attaching Pd in ​​a TWC washcoat layer having both alumina and CeZr oxide without using the conventional incipient wetness impregnation method which is not cost effective. Summary of the invention

[0008] One aspect of the present disclosure relates to a catalyst product for treating exhaust gas, the catalyst product comprising: a substrate, the substrate comprising an inlet end, an outlet end, and having an axial length L; a first catalytic region, the first catalytic region starting at the inlet end and extending less than the axial length L, wherein the first catalytic region comprises a first platinum group metal (PGM) component, a first inorganic oxide, and an optional first oxygen storage capacity (OSC) material; a second catalytic region, the second catalytic region starting at the outlet end and extending less than the axial length L, wherein the second catalytic region comprises a second PGM component, a second inorganic oxide, and an optional second OSC material; and a third catalytic region; wherein the weight ratio of the first inorganic oxide to the optional first OSC material is greater than 1:1.

[0009] The present invention also includes an exhaust system for an internal combustion engine, the exhaust system comprising the three-way catalyst composition of the present invention.

[0010] The present invention also includes treating exhaust gas from an internal combustion engine, in particular treating exhaust gas from a gasoline engine. The method comprises contacting the exhaust gas with a three-way catalyst component of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1a It shows that according to one embodiment of the present invention, the first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is equal to the axial length L. The third catalytic region extends 100% of the axial length L and covers the first catalytic region and the second catalytic region as a top layer.

[0012] Figure 1bIt is shown that according to one embodiment of the present invention, the first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is greater than the axial length L. The third catalytic region extends 100% of the axial length L and covers the first catalytic region and the second catalytic region as a top layer.

[0013] Figure 1c Depiction Figure 1b variants.

[0014] Figure 1d It shows that according to one embodiment of the present invention, the first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is less than the axial length L. The third catalytic region extends 100% of the axial length L and covers the first catalytic region and the second catalytic region as a top layer.

[0015] Figure 1e It shows that according to one embodiment of the present invention, the third catalytic region extends 100% of the axial length L as the bottom layer, the first catalytic region extends less than 100% of the axial length L from the inlet end, and the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is equal to (and may be greater than or less than) the axial length L.

[0016] Figure 2a According to one embodiment of the present invention, the first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is equal to (and may be greater than or less than) the axial length L. The third catalytic region extends less than 100% of the axial length L from the outlet end.

[0017] Figure 2b According to one embodiment of the present invention, the first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is equal to (and may be greater than or less than) the axial length L. The third catalytic region extends less than 100% of the axial length L from the inlet end.

[0018] Figure 3aIt is shown that according to one embodiment of the present invention, the first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is equal to (and may be greater than or less than) the axial length L and constitutes the bottom layer. The third catalytic region extends less than 100% of the axial length L from the inlet end, and the fourth catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the third catalytic region and the fourth catalytic region is equal to (and may be greater than or less than) the axial length L and constitutes the top layer.

[0019] Figure 3b According to one embodiment of the present invention, the third catalytic region extends less than 100% of the axial length L from the inlet end, and the fourth catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the third catalytic region and the fourth catalytic region is equal to (and may be greater than or less than) the axial length L and constitutes the bottom layer. The first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is equal to (and may be greater than or less than) the axial length L and constitutes the top layer.

[0020] Figure 4a The NO2 emission of Comparative Catalyst F and Inventive Catalyst 5 during the cold RDE cycle is shown. x Emissions.

[0021] Figure 4b CO emissions of Comparative Catalyst F and Inventive Catalyst 5 during a cold RDE cycle are shown.

[0022] Figure 4c THC emissions for Comparative Catalyst F and Inventive Catalyst 5 during a cold RDE cycle are shown. DETAILED DESCRIPTION

[0023] The present invention relates to the catalytic treatment of combustion exhaust gases, such as those produced by gasoline and other engines, and to related catalysts and systems. More particularly, the present invention relates to the simultaneous treatment of NO x , CO and HC. The present inventors have developed a TWC catalyst of a zoned Pd layer configuration, in which most of the Pd species are forced to land on alumina or CeZr oxide by controlling the weight ratio of the two supports in the inlet washcoat layer or the outlet washcoat layer.

[0024] One aspect of the present disclosure relates to a catalyst product for treating exhaust gas, the catalyst product comprising: a substrate, the substrate comprising an inlet end, an outlet end, and having an axial length L; a first catalytic region, the first catalytic region starting at the inlet end and extending less than the axial length L, wherein the first catalytic region comprises a first platinum group metal (PGM) component, a first inorganic oxide, and an optional first oxygen storage capacity (OSC) material; a second catalytic region, the second catalytic region starting at the outlet end and extending less than the axial length L, wherein the second catalytic region comprises a second PGM component, an optional second inorganic oxide, and a second OSC material; and a third catalytic region; wherein the weight ratio of the first inorganic oxide to the optional first OSC material is greater than 1:1.

[0025] The inventors have found that these catalysts coated in this manner exhibit better catalytic performance than conventional uniform Pd layer configurations. The unexpected benefits of the present invention include improved TWC performance, significantly reduced exhaust pollutant emissions, and greater ease of achieving emission targets in transient driving cycles, especially after the cold start phase, compared to conventional TWC catalysts of similar concentration (e.g., washcoat loading).

[0026] The first catalytic zone

[0027] The first catalytic zone may extend from 20% to 90% of the axial length L. Preferably, the first catalytic zone may extend from 25% to 80% of the axial length L, more preferably from 30% to 70%.

[0028] The first PGM component may be Pd, Pt, Rh or a combination thereof. Preferably, the first PGM component may be Pd, Pt or a combination thereof. More preferably, the first PGM component may be Pd. Alternatively, the first PGM component may be Rh.

[0029] The first inorganic oxide is preferably an oxide of an element of Groups 2, 3, 4, 5, 13 and 14. Preferably, the first inorganic oxide is selected from the group consisting of aluminum oxide, magnesium oxide, silicon dioxide, cerium oxide, barium oxide, and mixed oxides or composite oxides thereof. Particularly preferably, the first inorganic oxide is aluminum oxide, lanthanum-aluminum oxide, cerium oxide or magnesium oxide / aluminum oxide composite oxide. A particularly preferred first inorganic oxide is aluminum oxide or a lanthanum-aluminum oxide composite oxide.

[0030] The optional first OSC material, if present, is preferably selected from the group consisting of cerium oxide, ceria-zirconia mixed oxide, and alumina-ceria-zirconia mixed oxide. More preferably, the first OSC material comprises ceria-zirconia mixed oxide. The ceria-zirconia mixed oxide may also contain some dopants, such as lanthanum, neodymium, praseodymium, yttrium oxides, etc.

[0031] The weight ratio of the first inorganic oxide to the optional first OSC material may be at least 3:2; preferably at least 2:1 or at least 5:2.

[0032] Alternatively, the weight ratio of the first inorganic oxide to the first OSC material may be 10:1 to 3:2, preferably 8:1 to 3:2 or 5:1 to 3:2; more preferably 10:1 to 2:1 or 8:1 to 2:1; and most preferably 5:1 to 2:1.

[0033] The weight ratio of zirconium oxide to ceria in the ceria-zirconia mixed oxide may be at least 50:50, preferably higher than 55:45, more preferably at least 60:40, 70:30 or 80:20.

[0034] The first PGM component may be supported on both the first inorganic oxide and the first OSC material.

[0035] The first catalytic zone may contain 0.1 g / ft 3 Up to 300g / ft 3 Preferably, the first catalytic zone may contain 50 g / ft 3 Up to 250g / ft 3 The first PGM component is preferably 100 g / ft 3 Up to 220g / ft 3 Alternatively, the first catalytic zone may contain 0.1 g / ft 3 Up to 20g / ft 3 In some embodiments, the first catalytic zone may contain 1 g / ft 3 Up to 20g / ft 3 or 2g / ft 3 Up to 15g / ft 3 The first PGM component.

[0036] The optional first OSC material loading in the first catalytic zone may be less than 2 g / in 3 In some embodiments, the optional first OSC material loading in the first catalytic zone is no greater than 1.5 g / in 3 、1.2g / in 3 、1.0g / in3 、0.9g / in 3 、0.8g / in 3 or 0.7g / in 3 .

[0037] The total washcoat loading for the first catalyst zone may be less than 4 g / in 3 , preferably less than 3.5g / in 3 、3.0g / in 3 、2.5g / in 3 or 1.5g / in 3 Alternatively, the total washcoat loading for the first catalyst zone may be 0.5 g / in 3 Up to 4g / in 3 、0.5g / in 3 Up to 3.5g / in 3 , preferably 0.5 g / in 3 Up to 3.0g / in 3 、1.0g / in 3 Up to 3.0g / in 3 、1.0g / in 3 Up to 2.5g / in 3 or 1.5g / in 3 Up to 2.5g / in 3 .

[0038] The first catalytic zone may also comprise a first alkali metal or alkaline earth metal component.

[0039] In some embodiments, the first alkali metal or alkaline earth metal may be deposited on the first OSC material. Alternatively or in addition, the first alkali metal or alkaline earth metal may be deposited on the first inorganic oxide. That is, in some embodiments, the first alkali metal or alkaline earth metal may be deposited on (i.e., present on) both the first OSC material and the first inorganic oxide.

[0040] The first alkali metal or alkaline earth metal is usually in contact with the first inorganic oxide. Preferably, the first alkali metal or alkaline earth metal is supported on the first inorganic oxide. Alternatively, the first alkali metal or alkaline earth metal may be in contact with the first OSC material.

[0041] The first alkali metal or alkaline earth metal is preferably barium or strontium and mixed oxides or composite oxides thereof. Preferably, the loading of barium or strontium (when present) is 0.1 wt % to 15 wt %, and more preferably 3 wt % to 10 wt % barium or strontium based on the total weight of the first catalytic region.

[0042] Preferably, the barium is present in the form of BaCO3.

[0043] The second catalytic region

[0044] The second catalytic zone may extend from 20% to 90% of the axial length L. Preferably, the second catalytic zone may extend from 25% to 80% of the axial length L, more preferably from 30% to 70%.

[0045] The second PGM component may be Pd, Pt, Rh or a combination thereof. Preferably, the second PGM component may be Pd, Pt or a combination thereof. More preferably, the second PGM component may be Pd. Alternatively, the second PGM component may be Rh.

[0046] The optional second inorganic oxide, if present, is preferably an oxide of an element of Group 2, Group 3, Group 4, Group 5, Group 13 and Group 14. Preferably, the optional second inorganic oxide is selected from the group consisting of aluminum oxide, magnesium oxide, silicon dioxide, cerium oxide, barium oxide, and mixed oxides or composite oxides thereof. Particularly preferably, the optional second inorganic oxide is aluminum oxide, lanthanum-aluminum oxide, cerium oxide or magnesium oxide / aluminum oxide composite oxide. A particularly preferred second inorganic oxide is aluminum oxide or a lanthanum-aluminum oxide composite oxide.

[0047] The second OSC material is preferably selected from cerium oxide, ceria-zirconia mixed oxide, and alumina-ceria-zirconia mixed oxide. More preferably, the second OSC material comprises ceria-zirconia mixed oxide. The ceria-zirconia mixed oxide may also contain some dopants, such as lanthanum oxide, neodymium oxide, praseodymium oxide, yttrium oxide, etc.

[0048] The weight ratio of the optional second inorganic oxide to the second OSC material may be less than 1:1; preferably no greater than 2:3; more preferably no greater than 1:2 or 2:5.

[0049] Alternatively, the weight ratio of the second inorganic oxide to the second OSC material may be 2:3 to 1:10, preferably 2:3 to 1:8 or 2:3 to 1:5; more preferably 1:2 to 1:10 or 1:2 to 1:8; and most preferably 1:2 to 1:5.

[0050] The weight ratio of zirconium oxide to ceria in the ceria-zirconia mixed oxide may be at least 20:80, preferably higher than 50:50, more preferably at least 55:45, 60:40, 70:30 or 80:20.

[0051] The second PGM component may be supported on both the second inorganic oxide and the second OSC material.

[0052] The second catalytic zone may contain 0.1 g / ft 3 Up to 300g / ft3 Preferably, the second catalytic zone may contain 50 g / ft 3 Up to 250g / ft 3 The second PGM component is preferably 100 g / ft 3 Up to 220g / ft 3 Alternatively, the second catalytic zone may contain 0.1 g / ft 3 Up to 20g / ft 3 In some embodiments, the second catalytic zone may contain 1 g / ft 3 Up to 20g / ft 3 or 2g / ft 3 Up to 15g / ft 3 The second PGM component.

[0053] The second OSC material loading in the second catalytic zone may be at least 0.5 g / in 3 In some embodiments, the second OSC material loading in the second catalytic zone may be at least 0.7 g / in 3 、0.8g / in 3 、0.9g / in 3 、1.0g / in 3 , 1.5g / in 3 , 2.0g / in 3 or 2.5g / in 3 .

[0054] The total washcoat loading for the second catalyst zone may be less than 4 g / in 3 , preferably less than 3.5g / in 3 、3.0g / in 3 、2.5g / in 3 or 1.5g / in 3 Alternatively, the total washcoat loading for the second catalyst zone may be 0.5 g / in 3 Up to 4.0g / in 3 、0.5g / in 3 Up to 3.5g / in 3 , preferably 0.5 g / in 3 Up to 3.0g / in 3 、1.0g / in 3 Up to 3.0g / in 3 、1.0g / in 3 Up to 2.5g / in 3 or 1.5g / in 3 Up to 2.5g / in 3 .

[0055] The second catalytic zone may also comprise a second alkali metal or alkaline earth metal component.

[0056] In some embodiments, the second alkali metal or alkaline earth metal may be deposited on the second OSC material. Alternatively or in addition, the second alkali metal or alkaline earth metal may be deposited on the second inorganic oxide. That is, in some embodiments, the second alkali metal or alkaline earth metal may be deposited on (i.e., present on) both the second OSC material and the second inorganic oxide.

[0057] The second alkali metal or alkaline earth metal is usually in contact with the second inorganic oxide. Preferably, the second alkali metal or alkaline earth metal is supported on the second inorganic oxide. Alternatively, the second alkali metal or alkaline earth metal may be in contact with the second OSC material.

[0058] The second alkali metal or alkaline earth metal is preferably barium or strontium and mixed oxides or composite oxides thereof. Preferably, the loading of barium or strontium (if present) is 0.1 wt % to 15 wt %, and more preferably 3 wt % to 10 wt % barium or strontium based on the total weight of the second catalytic region.

[0059] Preferably, the barium is present in the form of BaCO3.

[0060] The third catalytic zone

[0061] In some embodiments, the third catalytic region may extend 100% of the axial length L. In other embodiments, the third catalytic region may extend less than 100% of the axial length L, such as less than 95%, 90%, or 85%. Alternatively, the third catalytic region may extend from 50% to 95% or from 60% to 95% of the axial length L.

[0062] The third catalytic zone may comprise a third PGM component, a third OSC material, a third alkali metal or alkaline earth metal component and / or a third inorganic oxide.

[0063] The third PGM component may include Rh. In some embodiments, the third PGM component may also include Pd and / or Pt. In other embodiments, the third catalytic region may be substantially free of PGM metals other than the rhodium component. Alternatively, the third PGM component may include Pt and / or Pd.

[0064] The third catalytic zone may contain 0.1 g / ft 3 Up to 20g / ft 3 In some embodiments, the third catalytic zone may contain 1 g / ft 3 Up to 20g / ft 3 or 2g / ft 3 Up to 15g / ft 3Alternatively, the third catalytic zone may contain 0.1 g / ft 3 Up to 300g / ft 3 Preferably, the third catalytic zone may contain 50 g / ft 3 Up to 250g / ft 3 The third PGM component, more preferably 100 g / ft 3 Up to 220g / ft 3 The third PGM component.

[0065] The total washcoat loading of the third catalyst zone may be less than 4.0 g / in 3 ; preferably less than 3.5g / in 3 、3.0g / in 3 or 2g / in 3 More preferably less than 1.5 g / in 3 or 1.0g / in 3 .

[0066] The third OSC material is preferably selected from the group consisting of cerium oxide, ceria-zirconia mixed oxide, and alumina-ceria-zirconia mixed oxide. Preferably, the third OSC material comprises ceria-zirconium mixed oxide and one or more dopants such as lanthanum, neodymium, yttrium, praseodymium, etc. In addition, the third OSC material can be used as a support material for the third rhodium component.

[0067] The third catalytic zone may also comprise a third alkali metal or alkaline earth metal component and / or a third inorganic oxide.

[0068] The molar ratio of zirconium oxide to ceria in the ceria-zirconia mixed oxide may be at least 50:50; preferably higher than 60:40; and more preferably higher than 80:20.

[0069] The third OSC material may be 10 to 90 wt%; preferably 25 to 75 wt%; more preferably 35 to 65 wt%; based on the total washcoat loading of the third catalytic zone.

[0070] The third OSC material loading in the third catalytic zone may be less than 2 g / in 3 In some embodiments, the third OSC material loading in the third catalytic zone is no greater than 1.5 g / in 3 、1.2g / in 3 、1.0g / in 3 or 0.5g / in 3 .

[0071] The third catalytic region may be substantially free of a third alkali metal or alkaline earth metal. The reference to "substantially free" means that the material may be present in trace amounts in the layer, intentionally or unintentionally. For example, an alkali metal or alkaline earth metal may be present in the first catalytic region and / or the second catalytic region, and some of the alkali metal or alkaline earth metal may inadvertently migrate / infiltrate into the third catalytic region during the coating process.

[0072] The third inorganic oxide is preferably an oxide of an element of Groups 2, 3, 4, 5, 13 and 14. Preferably, the third inorganic oxide is selected from the group consisting of alumina, cerium oxide, magnesium oxide, silicon dioxide, lanthanum, zirconium, neodymium, praseodymium oxides, and mixed oxides or composite oxides thereof. Particularly preferably, the third inorganic oxide is alumina, a lanthanum / aluminum oxide composite oxide, or a zirconium / aluminum oxide composite oxide. A particularly preferred third inorganic oxide is a lanthanum / aluminum oxide composite oxide, or a zirconium / aluminum oxide composite oxide. The third inorganic oxide may be a support material for the third rhodium component and / or the third OSC material.

[0073] The fourth catalytic region

[0074] In some embodiments, the catalyst article may further include a fourth catalytic region. In certain embodiments, the fourth catalytic region may extend less than 100% of the axial length L, such as less than 95%, 90%, or 85%. Alternatively, the fourth catalytic region may extend from 50% to 95% or from 60% to 95% of the axial length L.

[0075] The fourth catalytic zone may comprise a fourth PGM component, a fourth OSC material, a fourth alkali metal or alkaline earth metal component and / or a fourth inorganic oxide.

[0076] The fourth PGM component may include Rh. In some embodiments, the fourth PGM component may also include Pd and / or Pt. In other embodiments, the fourth catalytic zone may be substantially free of PGM metals other than the rhodium component. Alternatively, the fourth PGM component may include Pt and / or Pd.

[0077] The fourth catalytic zone may contain 0.1 g / ft 3 Up to 20g / ft 3 In some embodiments, the fourth catalytic zone may contain 1 g / ft 3 Up to 20g / ft 3 or 2g / ft 3 Up to 15g / ft 3 Alternatively, the fourth catalytic zone may contain 0.1 g / ft 3 Up to 300g / ft 3Preferably, the fourth catalytic zone may contain 50 g / ft 3 Up to 250g / ft 3 The fourth PGM component, more preferably 100 g / ft 3 Up to 220g / ft 3 The fourth PGM component.

[0078] The total washcoat loading of the fourth catalyst zone may be less than 4.0 g / in 3 ; preferably less than 3.5g / in 3 、3.0g / in 3 or 2g / in 3 More preferably less than 1.5 g / in 3 or 1.0g / in 3 .

[0079] The fourth OSC material is preferably selected from the group consisting of cerium oxide, ceria-zirconia mixed oxide, and alumina-ceria-zirconia mixed oxide. Preferably, the fourth OSC material comprises ceria-zirconium mixed oxide and one or more dopants such as lanthanum, neodymium, yttrium, praseodymium, etc. In addition, the fourth OSC material can be used as a support material for the fourth rhodium component.

[0080] The fourth catalytic zone may also comprise a fourth alkali metal or alkaline earth metal component and / or a fourth inorganic oxide.

[0081] The molar ratio of zirconium oxide to ceria in the ceria-zirconia mixed oxide may be at least 50:50; preferably higher than 60:40; and more preferably higher than 80:20.

[0082] The fourth OSC material may be 10 to 90 wt%; preferably 25 to 75 wt%; more preferably 35 to 65 wt%; based on the total washcoat loading of the fourth catalytic zone.

[0083] The fourth OSC material loading in the fourth catalytic zone may be less than 2 g / in 3 In some embodiments, the fourth OSC material loading in the fourth catalytic zone is no greater than 1.5 g / in 3 、1.2g / in 3 、1.0g / in 3 or 0.5g / in 3 .

[0084] The fourth catalytic region may be substantially free of a fourth alkali metal or alkaline earth metal. Reference to "substantially free" means that the material may be present in trace amounts in the layer, intentionally or unintentionally. For example, an alkali metal or alkaline earth metal may be present in the first catalytic region and / or the second catalytic region, and some of the alkali metal or alkaline earth metal may inadvertently migrate / infiltrate into the fourth catalytic region during the coating process.

[0085] The fourth inorganic oxide is preferably an oxide of an element of Groups 2, 3, 4, 5, 13 and 14. Preferably, the fourth inorganic oxide is selected from the group consisting of alumina, cerium oxide, magnesium oxide, silicon dioxide, lanthanum, zirconium, neodymium, praseodymium oxides, and mixed oxides or composite oxides thereof. Particularly preferably, the fourth inorganic oxide is alumina, a lanthanum / aluminum oxide composite oxide or a zirconium / aluminum oxide composite oxide. A particularly preferred fourth inorganic oxide is a lanthanum / aluminum oxide composite oxide or a zirconium / aluminum oxide composite oxide. The fourth inorganic oxide may be a support material for the fourth rhodium component and / or the fourth OSC material.

[0086] The catalyst preparation of the present invention may comprise additional components known to the skilled person. For example, the composition of the present invention may further comprise at least one binder and / or at least one surfactant. In the case of a binder, a dispersible alumina binder is preferred.

[0087] Configuration of the first catalytic region, the second catalytic region, the third catalytic region, and the fourth catalytic region

[0088] The second catalytic region may overlap the first catalytic region by 1% to 70% of the axial length L; preferably, by 2% to 60%, 2% to 50%, 2% to 40%, 2% to 30%, 2% to 20%, 3% to 20%, or 3% to 10% of the axial length L (see, e.g., Figure 1b , Figure 1c ; The first catalyst region may cover the second catalyst region, or the second catalyst region may cover the first catalyst region). Alternatively, the total length of the second catalyst region and the first catalyst region may be equal to the axial length L (for example, see Figure 1a , Figure 2a , Figure 2b , Figure 3a , Figure 3b In yet another alternative, the combined length of the second catalytic region and the first catalytic region may be less than the axial length L, for example, no greater than 95%, 90%, 80% or 70% of the axial length L (see, for example, Figure 2a , Figure 2b ).

[0089] In one aspect of the present invention, various configurations of catalyst articles comprising a first catalytic region, a second catalytic region, a third catalytic region, and a fourth catalytic region can be prepared as follows.

[0090] Figure 1a It shows that according to one embodiment of the present invention, the first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is equal to the axial length L. The third catalytic region extends 100% of the axial length L and covers the first catalytic region and the second catalytic region as a top layer.

[0091] Figure 1b It is shown that according to one embodiment of the present invention, the first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is greater than the axial length L. The third catalytic region extends 100% of the axial length L and covers the first catalytic region and the second catalytic region as a top layer.

[0092] Figure 1c Depiction Figure 1b variants.

[0093] Figure 1d It shows that according to one embodiment of the present invention, the first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is less than the axial length L. The third catalytic region extends 100% of the axial length L and covers the first catalytic region and the second catalytic region as a top layer.

[0094] Figure 1e It shows that according to one embodiment of the present invention, the third catalytic region extends 100% of the axial length L as the bottom layer, the first catalytic region extends less than 100% of the axial length L from the inlet end, and the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is equal to (and may be greater than or less than) the axial length L.

[0095] Figure 2a According to one embodiment of the present invention, the first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is equal to (and may be greater than or less than) the axial length L. The third catalytic region extends less than 100% of the axial length L from the outlet end.

[0096] Figure 2bAccording to one embodiment of the present invention, the first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is equal to (and may be greater than or less than) the axial length L. The third catalytic region extends less than 100% of the axial length L from the inlet end.

[0097] Figure 3a It is shown that according to one embodiment of the present invention, the first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is equal to (and may be greater than or less than) the axial length L and constitutes the bottom layer. The third catalytic region extends less than 100% of the axial length L from the inlet end, and the fourth catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the third catalytic region and the fourth catalytic region is equal to (and may be greater than or less than) the axial length L and constitutes the top layer.

[0098] Figure 3b According to one embodiment of the present invention, the third catalytic region extends less than 100% of the axial length L from the inlet end, and the fourth catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the third catalytic region and the fourth catalytic region is equal to (and may be greater than or less than) the axial length L and constitutes the bottom layer. The first catalytic region extends less than 100% of the axial length L from the inlet end; the second catalytic region extends less than 100% of the axial length L to form the outlet end. The total length of the second catalytic region and the first catalytic region is equal to (and may be greater than or less than) the axial length L and constitutes the top layer.

[0099] The flow-through monolith substrate has a first face and a second face defining a longitudinal direction therebetween. The flow-through monolith substrate has a plurality of channels extending between the first face and the second face. The plurality of channels extend in the longitudinal direction and provide a plurality of interior surfaces (e.g., surfaces defining the walls of each channel). Each channel of the plurality of channels has an opening at the first face and an opening at the second face. For the avoidance of doubt, the flow-through monolith substrate is not a wall flow filter.

[0100] The first face is typically at the inlet end of the substrate and the second face is at the outlet end of the substrate.

[0101] The channel may have a constant width, and the plurality of channels may each have a uniform channel width.

[0102] Preferably, in a plane orthogonal to the longitudinal direction, the monolithic substrate has 300 to 900 channels / square inch, preferably 400 to 800 channels / square inch. For example, on the first side, the density of the open first channels and the closed second channels is 600 to 700 channels / square inch. The channels may have a cross section of: rectangular, square, circular, elliptical, triangular, hexagonal, or other polygonal shapes.

[0103] The monolith substrate acts as a support for holding the catalytic material. Suitable materials for forming the monolith substrate include ceramic-like materials such as cordierite, silicon carbide, silicon nitride, zirconium oxide, mullite, spodumene, alumina-silica magnesia or zirconium silicate, or porous refractory metals. Such materials and their use in making porous monolith substrates are well known in the art.

[0104] It should be noted that the flow-through monolithic substrate described herein is a single component (i.e., a single brick). Nevertheless, when forming an emission treatment system, the substrate used can be formed by adhering multiple channels together or by adhering multiple smaller substrates together, as described herein. Such techniques, as well as suitable housings and configurations for emission treatment systems, are well known in the art.

[0105] In embodiments where the catalyst article of the invention comprises a ceramic substrate, the ceramic substrate may be made of any suitable refractory material, such as alumina, silica, ceria, zirconium oxide, magnesium oxide, zeolites, silicon nitride, silicon carbide, zirconium silicate, magnesium silicate, aluminosilicates, and metal aluminosilicates (such as cordierite and spodumene), or mixtures or mixed oxides of any two or more thereof. Cordierite, magnesium aluminosilicate, and silicon carbide are particularly preferred.

[0106] In embodiments where the catalyst article of the present invention comprises a metal substrate, the metal substrate may be made of any suitable metal, and in particular, of heat-resistant metals and metal alloys, such as titanium and stainless steel, and ferritic alloys containing iron, nickel, chromium and / or aluminum in addition to other trace metals.

[0107] In some embodiments, the first catalytic region can be directly supported / deposited on a substrate (e.g., see Figure 1a to Figure 1d In certain embodiments, the second catalytic region may be directly supported / deposited on a substrate (e.g., see Figure 1a to Figure 1d In other embodiments, the third catalytic region is directly supported / deposited on the substrate (e.g., see Figure 1e , Figure 3b ).

[0108] In certain embodiments, at least 50% of the first catalytic region is not covered by the second catalytic region and / or the third catalytic region. In a preferred embodiment, at least 60%, 70% or 80% of the first catalytic region is not covered by the second catalytic region and / or the third catalytic region. In a more preferred embodiment, at least 90% or 95% of the first catalytic region is not covered by the second catalytic region and / or the third catalytic region. In a most preferred embodiment, 100% of the first catalytic region is not covered by the second catalytic region and / or the third catalytic region.

[0109] Another aspect of the present disclosure relates to using the catalyst articles described herein to treat x A catalytic converter equipped with a TWC made according to the method shows improved performance compared to a conventional TWC (at the same PGM loading), and also shows particularly improved performance under those transient conditions after the cold start / light-off phase.

[0110] Another aspect of the present disclosure relates to a system for treating vehicle exhaust, the system comprising a catalyst article as described herein, together with a conduit for transferring the exhaust through the system.

[0111] definition

[0112] As used herein, the term "region" refers to an area on a substrate, which is generally obtained by drying and / or calcining a washcoat. For example, a "region" can be arranged or carried on a substrate in the form of a "layer" or "zone". The region or arrangement on the substrate is generally controlled during the application of the washcoat to the substrate. A "region" generally has distinct boundaries or edges (i.e., one region can be distinguished from another region using conventional analytical techniques).

[0113] Typically, a "region" has a substantially uniform length. In this context, reference to a "substantially uniform length" refers to a length that does not deviate from its average value (e.g., the difference between the maximum length and the minimum length) by more than 10%, preferably does not deviate by more than 5%, more preferably does not deviate by more than 1%.

[0114] Preferably, each "region" has a substantially uniform composition (i.e., the composition of the washcoat layer does not differ significantly when one portion of the region is compared to another portion of the region). In this context, a substantially uniform composition refers to a material (e.g., region) in which the difference in composition when one portion of the region is compared to another portion of the region is 5% or less, typically 2.5% or less, and most typically 1% or less.

[0115] As used herein, the term "region" refers to an area having a length less than the total length of a substrate, such as ≤75% of the total length of the substrate."Regions" typically have a length (i.e., substantially uniform length) of at least 5% (e.g., ≥5%) of the total length of the substrate.

[0116] The overall length of a substrate is the distance between its inlet end and its outlet end (eg, opposite ends of the substrate).

[0117] As used herein, any reference to a "zone disposed at the inlet end of a substrate" refers to a zone disposed or carried on a substrate, wherein the zone is closer to the inlet end of the substrate than a zone near the outlet end of the substrate. Thus, the midpoint of the zone is closer to the inlet end of the substrate than the midpoint near the outlet end of the substrate (i.e., at half its length). Similarly, as used herein, any reference to a "zone disposed at the outlet end of a substrate" refers to a zone disposed or carried on a substrate, wherein the zone is closer to the outlet end of the substrate than a zone near the inlet end of the substrate. Thus, the midpoint of the zone is closer to the outlet end of the substrate than the midpoint near the inlet end of the substrate (i.e., at half its length).

[0118] When the substrate is a wall flow filter, generally speaking, any reference to a "zone disposed at the inlet end of the substrate" refers to a zone disposed or carried on the substrate that:

[0119] (a) a region closer to the inlet end (e.g., open end) of an inlet channel of the substrate than a region closer to the closed end (e.g., plugged end or blocked end) of the inlet channel, and / or

[0120] (b) A closed end (eg, a plugged or blocked end) of an outlet channel of the substrate is closer than a region closer to the outlet end (eg, an open end) of the outlet channel.

[0121] Thus, the midpoint of the zone (i.e., at half its length) is (a) closer to the inlet end of the inlet channel of the substrate than the midpoint near the closed end of the inlet channel, and / or (b) closer to the closed end of the outlet channel of the substrate than the midpoint near the outlet end of the outlet channel.

[0122] Similarly, when the substrate is a wall flow filter, any reference to a "zone disposed at the outlet end of the substrate" refers to a zone disposed or carried on the substrate that:

[0123] (a) a region closer to the outlet end (e.g., the open end) of the outlet channel of the substrate than a region closer to the closed end (e.g., the blocked end or the plugged end) of the outlet channel, and / or

[0124] (b) A closed end (eg, a plugged or blocked end) of an inlet channel of the substrate is closer than a region closer to the inlet end (eg, an open end) of the inlet channel.

[0125] Thus, the midpoint of the zone (i.e., at half its length) is (a) closer to the outlet end of the outlet channel of the substrate than the midpoint near the closed end of the outlet channel, and / or (b) closer to the closed end of the inlet channel of the substrate than the midpoint near the inlet end of the inlet channel.

[0126] When the washcoat layer is present in the wall of a wall flow filter (ie, the zone is in the wall), the zone may satisfy both (a) and (b) simultaneously.

[0127] The term "washcoat" is well known in the art and refers to an adherent coating typically applied to a substrate during catalyst production.

[0128] As used herein, the acronym "PGM" refers to "platinum group metals". The term "platinum group metals" generally refers to metals selected from Ru, Rh, Pd, Os, Ir and Pt, preferably metals selected from Ru, Rh, Pd, Ir and Pt. Generally speaking, the term "PGM" preferably refers to metals selected from Rh, Pt and Pd.

[0129] As used herein, the term "mixed oxide" generally refers to a mixture of oxides in a single phase, as generally known in the art. As used herein, the term "composite oxide" generally refers to a composition of oxides having more than one phase, as generally known in the art.

[0130] As used herein, the expression "consisting essentially of limits the scope of a feature to include the specified materials or steps, and any other materials or steps that do not materially affect the basic characteristics of the feature, such as trace impurities. The expression "consisting essentially of encompasses the expression "consisting of.

[0131] As used herein, the expression "substantially free" used for a material in the context of the content of a region, layer or zone generally refers to a small amount of material, such as ≤5 wt%, preferably ≤2 wt%, more preferably ≤1 wt%. The expression "substantially free" encompasses the expression "does not comprise".

[0132] As used herein, the expression "substantially free" used for a material in the context of the content of a region, layer or zone generally means that the material is in trace amounts, such as ≤1 wt%, preferably ≤0.5 wt%, more preferably ≤0.1 wt%. The expression "substantially free" encompasses the expression "does not comprise".

[0133] As used herein, any reference to the amount of dopant (particularly the total amount) expressed as wt % refers to the weight of the support material or refractory metal oxide thereof.

[0134] As used herein, the term "loading" refers to the weight of the metal in g / ft. 3 The measurement result is in units of .

[0135] The following examples merely illustrate the present invention. Those skilled in the art will recognize many variations within the spirit of the present invention and the scope of the claims.

[0136] Example

[0137] Material

[0138] Unless otherwise noted, all materials are commercially available and can be purchased from known suppliers.

[0139] Comparative Catalyst A :

[0140] Comparative Catalyst A is a commercial ternary (Pd-Rh) catalyst with a double layer structure. The bottom layer consists of Pd supported on a washcoat layer of a first CeZr mixed oxide, La stabilized alumina, and a Ba promoter. The washcoat layer loading of the bottom layer is about 2.4 g / in 3 , where Pd loading is 131 g / ft 3 Among them, the La-stabilized alumina loading or the first CeZr mixed oxide loading is 1.0 g / in 3 , so that the weight ratio of the two Pd support materials is 1:1. The first CeZr mixed oxide contains about 40% ceria. The washcoat layer is applied from the inlet and outlet faces of the ceramic substrate (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure, wherein the target coating depth is 50% of the substrate length, followed by drying and calcination.

[0141] The top layer consisted of Rh supported on a washcoat layer consisting of a second CeZr mixed oxide, La stabilized alumina. The washcoat loading for the top layer was about 1.5 g / in 3 , where the Rh loading is 9g / ft 3 The washcoats were applied from above to the inlet and outlet faces of the ceramic substrates (750 cpsi, 3.0 mil wall thickness) containing the base washcoat using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying and calcination.

[0142] Creative Catalyst 1 :

[0143] The first catalytic zone :

[0144] The first catalytic zone consisted of Pd supported on a washcoat layer of La-stabilized alumina and Ba promoter. The washcoat loading of the first catalytic zone was about 2.8 g / in 3 , where Pd is 131g / ft 3Among them, the La-stabilized alumina loading is 2.0 g / in 3 , and it is substantially free of CeZr mixed oxide.

[0145] The first washcoat layer was coated from above the inlet face of the ceramic substrate containing the first catalytic region (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying.

[0146] The second catalytic region :

[0147] The second catalytic zone consisted of Pd supported on a washcoat layer of the first CeZr mixed oxide and alumina binder. The washcoat loading of the second catalytic zone was about 2.3 g / in 3 , and the Pd loading is 131 g / ft 3 Among them, the first CeZr mixed oxide loading is 2.0g / in 3 , and it is substantially free of La-stabilized alumina. The first CeZr mixed oxide contains about 40% ceria.

[0148] A second washcoat layer was applied from the outlet face of a ceramic substrate (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying and calcination.

[0149] The third catalytic zone :

[0150] The third catalytic zone was prepared and coated in the same manner as the top layer of Comparative Catalyst A.

[0151] Comparative Catalyst B :

[0152] Comparative Catalyst B was prepared and coated in the same manner as Inventive Catalyst 1, except that the second washcoat layer was applied from the inlet face of a ceramic substrate (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure, and the first washcoat layer was applied from the outlet face of the ceramic substrate, wherein the target coating depth was 50% of the substrate length.

[0153] Creative Catalyst 2 :

[0154] The first catalytic zone :

[0155] The first catalytic zone consisted of Pd supported on a washcoat layer of a first CeZr mixed oxide, La stabilized alumina, and a Ba promoter. The washcoat loading of the first catalytic zone was about 2.6 g / in 3 , where Pd is 131g / ft 3Among them, the La-stabilized alumina loading is 1.5 g / in 3 , and the first CeZr mixed oxide loading is 0.5 g / in 3 , so that the weight ratio of La-stabilized alumina to the first CeZr mixed oxide is 3: 1. The first CeZr mixed oxide contains about 40% ceria.

[0156] The first washcoat layer was coated from above the inlet face of the ceramic substrate containing the first catalytic region (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying.

[0157] The second catalytic region :

[0158] The second catalytic zone consisted of Pd supported on a washcoat layer of the first CeZr mixed oxide, La stabilized alumina, and Ba promoter. The washcoat loading of the second catalytic zone was about 2.3 g / in 3 , and the Pd loading is 131 g / ft 3 Among them, the La-stabilized alumina loading is 0.5 g / in 3 , and the first CeZr mixed oxide loading is 1.5 g / in 3 , so that the weight ratio of La-stabilized alumina to the first CeZr mixed oxide is 1:3. The first CeZr mixed oxide contains about 40% ceria.

[0159] A second washcoat layer was applied from the outlet face of a ceramic substrate (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying and calcination.

[0160] The third catalytic zone :

[0161] The third catalytic zone was prepared and coated in the same manner as the top layer of Comparative Catalyst A.

[0162] Comparative Catalyst C :

[0163] Comparative Catalyst C was prepared and coated in the same manner as Inventive Catalyst 2, except that the second washcoat layer was applied from the inlet face of a ceramic substrate (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure, and the first washcoat layer was applied from the outlet face of the ceramic substrate, wherein the target coating depth was 50% of the substrate length.

[0164] Creative Catalyst 3 :

[0165] Inventive catalyst 3 was prepared according to a similar procedure as inventive catalyst 1, except that the coating depth of the first catalytic region and the second catalytic region was at least 75% but less than 100% of the length of the substrate.

[0166] Comparative Catalyst D :

[0167] Comparative Catalyst D was prepared according to a similar procedure as Comparative Catalyst B, except that the coating depth of the first catalytic region and the second catalytic region was at least 75% but less than 100% of the length of the substrate.

[0168] Creative Catalyst 4 :

[0169] Inventive catalyst 4 was prepared according to a similar procedure as inventive catalyst 2, except that the coating depth of the first catalytic region and the second catalytic region was at least 75% but less than 100% of the length of the substrate.

[0170] Comparative Catalyst E :

[0171] Comparative Catalyst E was prepared according to a procedure similar to Comparative Catalyst C, except that the coating depth of the first catalytic region and the second catalytic region was at least 75% but less than 100% of the length of the substrate.

[0172] Comparative Catalyst F :

[0173] Comparative Catalyst F is a commercial ternary (Pd-Rh) catalyst with a double layer structure. The bottom layer consists of Pd supported on a washcoat layer of a first CeZr mixed oxide, La stabilized alumina, and a Ba promoter. The washcoat layer loading of the bottom layer is about 2.4 g / in 3 , where Pd loading is 112g / ft 3 Among them, the La-stabilized alumina loading or the first CeZr mixed oxide loading is 1.0 g / in 3 , so that the weight ratio of the two Pd support materials is 1:1. The first CeZr mixed oxide contains about 20% ceria. The washcoat layer is applied from the inlet and outlet faces of the ceramic substrate (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure, wherein the target coating depth is 50% of the substrate length, followed by drying and calcination.

[0174] The top layer consisted of Rh supported on a washcoat layer consisting of a second CeZr mixed oxide, La stabilized alumina. The washcoat loading for the top layer was about 2.0 g / in 3 , where the Rh loading is 8g / ft 3The washcoats were applied from above to the inlet and outlet faces of the ceramic substrates (750 cpsi, 3.0 mil wall thickness) containing the base washcoat using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying and calcination.

[0175] Creative Catalyst 5 :

[0176] The first catalytic zone :

[0177] The first catalytic zone consisted of Pd supported on a washcoat layer of a first CeZr mixed oxide, La stabilized alumina, and a Ba promoter. The washcoat loading of the first catalytic zone was about 2.4 g / in 3 , where Pd is 112g / ft 3 Among them, the La-stabilized alumina loading is 1.5 g / in 3 , and the first CeZr mixed oxide loading is 0.5 g / in 3 , so that the weight ratio of La-stabilized alumina to the first CeZr mixed oxide is 3: 1. The first CeZr mixed oxide contains about 20% ceria.

[0178] The first washcoat layer was coated from above the inlet face of the ceramic substrate containing the first catalytic region (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying.

[0179] The second catalytic region :

[0180] The second catalytic zone consisted of Pd supported on a washcoat layer of the first CeZr mixed oxide, La stabilized alumina, and Ba promoter. The washcoat loading of the second catalytic zone was about 2.3 g / in 3 , and the Pd loading is 131 g / ft 3 Among them, the La-stabilized alumina loading is 0.5 g / in 3 , and the first CeZr mixed oxide loading is 1.5 g / in 3 , so that the weight ratio of La-stabilized alumina to the first CeZr mixed oxide is 1:3. The first CeZr mixed oxide contains about 20% ceria.

[0181] A second washcoat layer was applied from the outlet face of a ceramic substrate (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying and calcination.

[0182] The third catalytic zone :

[0183] The third catalytic zone was prepared and coated in the same manner as the top layer of Comparative Catalyst F.

[0184] Comparative Catalyst G :

[0185] Comparative Catalyst G is a commercial ternary (Pd-Rh) catalyst with a double layer structure. The bottom layer consists of Pd supported on a washcoat layer of a second CeZr mixed oxide, La stabilized alumina, and a Ba promoter. The washcoat loading of the bottom layer is about 2.4 g / in 3 , where Pd loading is 133 g / ft 3 Among them, the La-stabilized alumina loading or the second CeZr mixed oxide loading is 1.0 g / in 3 , so that the weight ratio of the two Pd support materials is 1:1. The second CeZr mixed oxide contains about 20% ceria. The washcoat layer is applied from the inlet and outlet faces of the ceramic substrate (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure, wherein the target coating depth is 50% of the substrate length, followed by drying and calcination.

[0186] The top layer consisted of Rh, La stabilized alumina supported on a washcoat layer of the first CeZr mixed oxide. The washcoat loading of the top layer was about 2.0 g / in 3 , where the Rh loading is 7g / ft 3 The washcoats were applied from above to the inlet and outlet faces of the ceramic substrates (750 cpsi, 3.0 mil wall thickness) containing the base washcoat using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying and calcination.

[0187] Creative Catalyst 6 :

[0188] The first catalytic zone :

[0189] The first catalytic zone consisted of Rh supported on a washcoat layer of La-stabilized alumina. The washcoat loading of the first catalytic zone was about 2.0 g / in 3 , where Rh is 7g / ft 3 Among them, the La-stabilized alumina loading is 2.0 g / in 3 , and it is substantially free of CeZr mixed oxide.

[0190] The first washcoat layer was coated from above the inlet face of the ceramic substrate containing the first catalytic region (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying.

[0191] The second catalytic region :

[0192] The second catalytic zone consisted of Rh supported on the first CeZr mixed oxide and alumina binder. The washcoat loading of the second catalytic zone was about 2.2 g / in 3 , where the Rh loading is 7g / ft 3 Among them, the first CeZr mixed oxide loading is 2.0g / in 3 , and it is substantially free of La-stabilized alumina. The first CeZr mixed oxide contains about 20% ceria.

[0193] A second washcoat layer was applied from the outlet face of a ceramic substrate (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying and calcination.

[0194] The third catalytic zone :

[0195] The third catalytic zone was prepared and coated in the same manner as the Pd underlayer of Comparative Catalyst G.

[0196] The design of the inventive catalyst 6 is shown in Figure 1e The third catalytic region is first coated on the ceramic substrate, followed by drying and calcination. Then, the first catalytic region and the second catalytic region are coated from the inlet and outlet, with a drying step in between. Finally, the finished catalyst is calcined a second time.

[0197] Creative Catalyst 7 :

[0198] The first catalytic zone :

[0199] The first catalytic zone consisted of Rh supported on a washcoat layer of a first CeZr mixed oxide and La stabilized alumina. The washcoat loading of the first catalytic zone was about 2.0 g / in 3 , where Rh is 7g / ft 3 Among them, the La-stabilized alumina loading is 1.5 g / in 3 , and the first CeZr mixed oxide loading is 0.5 g / in 3 , so that the weight ratio of La-stabilized alumina to the first CeZr mixed oxide is 3: 1. The first CeZr mixed oxide contains about 20% ceria.

[0200] The first washcoat layer was coated from above the inlet face of the ceramic substrate containing the first catalytic region (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying.

[0201] The second catalytic region :

[0202] The second catalytic zone consisted of Rh supported on a washcoat layer of the first CeZr mixed oxide and La stabilized alumina. The washcoat loading of the second catalytic zone was about 2.0 g / in 3 , where the Rh loading is 7g / ft 3 Among them, the La-stabilized alumina loading is 0.5 g / in 3 , and the first CeZr mixed oxide loading is 1.5 g / in 3 , so that the weight ratio of La-stabilized alumina to the first CeZr mixed oxide is 1:3. The first CeZr mixed oxide contains about 20% ceria.

[0203] A second washcoat layer was applied from the outlet face of a ceramic substrate (750 cpsi, 3.0 mil wall thickness) using a standard coating procedure with a target coating depth of 50% of the substrate length followed by drying and calcination.

[0204] The third catalytic zone :

[0205] The third catalytic zone was prepared and coated in the same manner as the Pd underlayer of Comparative Catalyst G.

[0206] The design of the inventive catalyst 7 is shown in Figure 1e The third catalytic region is first coated on the ceramic substrate, followed by drying and calcination. Then, the first catalytic region and the second catalytic region are coated from the inlet and outlet, with a drying step in between. Finally, the finished catalyst is calcined a second time.

[0207] Table 1 Summary of all catalysts

[0208]

[0209]

[0210] Example 1: Engine Bench Test Procedure and Results

[0211] Comparative Catalysts A to E and Inventive Catalysts 1 to 4 were subjected to engine bench aging for 100 hours using a stoichiometric / fuel cut-off aging cycle targeting a peak catalyst bed temperature of 1000°C. The catalysts were tested using a 2.0L engine bench dynamometer that performed a custom OEM designed real world driving (RDE) cycle that included acceleration and fuel cut-off conditions representing cold city, rural, highway, and hot city speed phases. The cycle time from ambient soak conditions was 2700 seconds, reaching a peak catalyst bed temperature of approximately 700°C and a mass air flow rate of 250kg / h. A cold RDE test was used as a preconditioning cycle. Afterwards, three hot RDE cycles were repeated with a 5 minute soak time in between. This was when the engine was at operating temperature, but the catalyst bed temperature was still hot. The advantage of running the hot RDE using cold RDE as a precondition is that the reproducibility of the engine off emissions is very good due to the inconsistent temperatures during the cold start cycle. To further improve data accuracy, the accumulated NO x The conversion rates of CO, THC and NO were compared with different catalysts, as shown in Table 2. The NO x , CO and THC emissions, and calculate the cumulative mass of each substance over the entire cycle. The cumulative conversion is calculated based on the cumulative post-catalyst emissions and the cumulative engine-off emissions. The results of the three hot RDE runs are averaged and shown in Table 2.

[0212] The data in Table 2 clearly show that all of the inventive catalysts of the present invention provide some NO compared to Comparative Catalyst A. x When the catalytic region rich in alumina is on the inlet side, those configurations have a significant NO and CO performance benefit compared to the catalytic region with a CeZr oxide-rich region on the inlet side. x Beneficial effects. For example, the NOx conversion rate of the inventive catalyst 1 is higher than that of the comparative catalyst B, and the NOx conversion rate of the inventive catalyst 2 is x The conversion rate is higher than that of Comparative Catalyst C, and the trend is the same for Inventive Catalyst 3 and Comparative Catalyst D. Inventive Catalyst 4 and Comparative Catalyst E show comparable NO x This may be due to the long dose length and having both alumina and CeZr oxide in the first and second catalytic zones, making it mostly similar to comparative catalyst A. Among the total 4 inventive formulations, the best catalyst was inventive catalyst 2, with an alumina-rich dose on the inlet side and a weight ratio of La-stabilized alumina to CeZr oxide of 3:1.

[0213] Table 2 compares the average cumulative CO conversion of all catalysts. CO conversion is more sensitive to dose length. A regular dose length (50%) with alumina-rich dose in the inlet is more favorable for CO conversion than a dose length with CeZr oxide on the inlet side. For example, the CO conversion of inventive catalyst 1 is higher than that of comparative catalyst B, and the CO conversion of inventive catalyst 2 is higher than that of comparative catalyst C.

[0214] During the entire hot RDE cycle, the catalyst bed temperature was above 450°C, so the THC conversion of all catalysts was equally large due to the hot bed temperature.

[0215] Table 2 Average cumulative conversion results of engine test bench hot RDE cycle

[0216]

[0217] Example 2: Cold RDE test in engine testing

[0218] Comparative Catalyst F and Inventive Catalyst 5 were subjected to engine bench aging for 150 hours using a stoichiometric / fuel cut aging cycle targeting a peak catalyst bed temperature of 1000°C. The catalysts were tested using a 2.0L twin-turbo, 4-cylinder, Eu(VI)b calibrated engine bench dynamometer that executed a custom OEM designed real world driving (RDE) cycle that included acceleration and fuel cut conditions representative of cold start city, highway, and hot city speed phases. The cycle time from ambient soak conditions was 2700 seconds at a vehicle speed of approximately 140 km / hr and a mass air flow rate of approximately 400 kg / hr, reaching a peak catalyst temperature of approximately 700°C. NO was measured at a post-catalyst location. x , CO and THC emissions, and the cumulative mass of each substance over the entire cycle was calculated. Three runs were performed for each catalyst formulation, and the cumulative emissions of the three runs were plotted versus time and are shown in the figure below.

[0219] Figure 4a is the NO of comparative catalyst F and inventive catalyst 5 during cold RDE cycle x It is clear that the inventive catalyst 5 with a zoned configuration having an alumina-rich dosage on the inlet side and a CeZr-rich mixed oxide dosage on the outlet side has a higher NO x The emissions are lower. CO emissions and THC emissions are shown in Figure 4b and Figure 4c The two catalysts showed comparable CO and THC emissions.

[0220] Example 3: Engine Bench Test Procedure and Results

[0221] Comparative Catalyst G and Inventive Catalysts 6 and 7 were subjected to engine bench aging for 50 hours using a stoichiometric / fuel cut-off aging cycle targeting a peak catalyst bed temperature of 1000°C. The catalysts were tested using a 2.0L engine bench dynamometer that performed a custom OEM designed real world driving (RDE) cycle that included acceleration and fuel cut-off conditions representing cold city, rural, highway, and hot city speed phases. The cycle time from ambient soak conditions was 2700 seconds, reaching a peak catalyst bed temperature of approximately 700°C and a mass air flow rate of 250kg / h. A cold RDE test was used as a preconditioning cycle. Afterwards, three hot RDE cycles were repeated with a 5 minute soak time in between. This was when the engine was at operating temperature, but the catalyst bed temperature was still hot. The advantage of running the hot RDE using cold RDE as a precondition is that the reproducibility of the engine off emissions is very good due to the inconsistent temperatures during the cold start cycle. To further improve data accuracy, the accumulated NO x The conversion rates of CO, THC and NO were compared with different catalysts, as shown in Table 3. x , CO and THC emissions, and calculate the cumulative mass of each substance in the entire cycle. The cumulative conversion rate is calculated based on the cumulative post-catalyst emissions and the cumulative engine off emissions. The results of the three hot RDE runs are averaged and shown in Table 3. In addition, for each sample, the cumulative mass of ammonia produced throughout the three hot RDE cycles is averaged and listed in Table 3.

[0222] While inventive catalyst 6 showed comparable performance to comparative catalyst G, inventive catalyst 7 of the present invention showed a slight beneficial effect compared to comparative catalyst G, and inventive catalyst 7 also produced less NH 3 .

[0223] Table 3 Average cumulative conversion results of engine test bench hot RDE cycle

[0224]

Claims

1. A catalyst product for treating exhaust gas, the catalyst product comprising: A substrate, the substrate comprising an inlet end, an outlet end, and an axial length L; a first catalytic region beginning at the inlet end and extending less than the axial length L, wherein the first catalytic region comprises a first platinum group metal (PGM) component, a first inorganic oxide, and optionally a first oxygen storage capacity (OSC) material; a second catalytic region beginning at the outlet end and extending less than the axial length L, wherein the second catalytic region comprises a second PGM component, an optional second inorganic oxide, and a second OSC material; and The third catalytic region; Wherein the weight ratio of the first inorganic oxide to the optional first OSC material is greater than 1:

1. 2 . The catalyst article according to claim 1 , wherein the first catalytic region extends from 20% to 90% of the axial length L. 3 .

3. The catalyst article according to claim 1 or claim 2, wherein the second catalytic zone extends from 20% to 90% of the axial length L.

4. The catalyst article according to any one of the preceding claims, wherein the second catalytic region overlaps the first catalytic region by 1% to 15% of the axial length L.

5. The catalyst article according to any one of claims 1 to 3, wherein the total length of the second catalytic region and the first catalytic region is equal to the axial length L.

6. The catalyst article according to any one of claims 1 to 3, wherein the total length of the second catalytic region and the first catalytic region is less than the axial length L.

7. The catalyst article according to any one of the preceding claims, wherein the weight ratio of the first inorganic oxide to the optional first OSC material is at least 2:

1.

8. The catalyst article according to any one of the preceding claims, wherein the weight ratio of the optional second inorganic oxide to the second OSC material is less than 1:

1.

9. The catalyst article according to any one of the preceding claims, wherein the weight ratio of the optional second inorganic oxide to the second OSC material does not exceed 1 :

2.

10. The catalyst article according to any one of the preceding claims, wherein the third catalytic zone extends over 100% of the axial length L.

11. The catalyst article according to any one of claims 1 to 9, wherein the third catalytic zone extends less than 100% of the axial length L.

12. The catalyst article of any one of the preceding claims, wherein the first PGM component is Pd, Pt, Rh, or a combination thereof.

13. The catalyst article of claim 12, wherein the first PGM component is Pd, Pt, or a combination thereof.

14. The catalyst article according to any one of the preceding claims, wherein the optional first OSC material is selected from the group consisting of cerium oxides, ceria-zirconia mixed oxides, and alumina-ceria-zirconia mixed oxides.

15. The catalyst article of claim 14, wherein the optional first OSC material comprises the ceria-zirconia mixed oxide.

16. The catalyst article according to any one of the preceding claims, wherein the first inorganic oxide is selected from the group consisting of alumina, ceria, magnesia, silica, lanthanum, neodymium, praseodymium, yttrium oxides, and mixed oxides or composite oxides thereof.

17. The catalyst article according to claim 16, wherein the first inorganic oxide is alumina, a lanthanum oxide / aluminum oxide composite oxide, or a magnesium oxide / aluminum oxide composite oxide.

18. The catalyst article of any one of the preceding claims, wherein the second PGM component is Pd, Pt, Rh, or a combination thereof.

19. The catalyst article of claim 18, wherein the second PGM component is Pd, Pt, or a combination thereof.

20. The catalyst article according to any one of the preceding claims, wherein the second OSC material is selected from the group consisting of cerium oxide, ceria-zirconia mixed oxide, and alumina-ceria-zirconia mixed oxide.

21. The catalyst article of claim 20, wherein the second OSC material comprises the ceria-zirconia mixed oxide.

22. The catalyst article according to any one of the preceding claims, wherein the optional second inorganic oxide is selected from the group consisting of alumina, ceria, magnesia, silica, lanthanum, neodymium, praseodymium, yttrium oxides, and mixed or composite oxides thereof.

23. The catalyst article of claim 22, wherein the optional second inorganic oxide is alumina, a lanthanum oxide / aluminum oxide composite oxide, or a magnesium oxide / aluminum oxide composite oxide.

24. The catalyst article of any one of the preceding claims, wherein the third catalytic region comprises a third PGM component, a third OSC material, a third alkali or alkaline earth metal component and / or a third inorganic oxide.

25. The catalyst article of any one of claim 24, wherein the third PGM component comprises Rh.

26. The catalyst article of any one of the preceding claims, wherein the substrate is a flow-through monolith.

27. The catalyst article according to any one of the preceding claims, wherein the first catalytic region is directly supported / deposited on the substrate.

28. The catalyst article according to any one of the preceding claims, wherein the second catalytic region is directly supported / deposited on the substrate.

29. The catalyst article according to any one of claims 1 to 26, wherein the third catalytic region is directly supported / deposited on the substrate.

30. An emission treatment system for treating a combustion exhaust gas stream, the emission treatment system comprising the catalyst article of any one of claims 1 to 29.

31. A method of treating exhaust gas from an internal combustion engine, the method comprising: The exhaust gas is contacted with a catalyst article according to any one of claims 1 to 29.

Citation Information

Cited By

  • Layered three-way conversion catalytic article with zoned configuration

    WO2026153363A1