Resin composition and method for producing same

By optimizing the composition ratio of the resin composition and combining nanocrystalline magnetic powder with thermosetting resin within a specific particle size range, the problems of magnetic permeability and magnetic loss of the sensor in the low-frequency range were solved, achieving high-performance miniaturization of the sensor and excellent coating properties of the resin composition.

CN118829692APending Publication Date: 2024-10-22AJINOMOTO CO INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380025440.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-17
Filing Date
2023-02-16
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve high relative permeability and low magnetic loss in sensors at low frequencies. Furthermore, the insufficient coatability of resin compositions limits the miniaturization and performance of switching power supplies.

Method used

A resin composition is formed by using nanocrystalline magnetic powder with a specific particle size range and a combination of magnetic powder and thermosetting resin. By controlling the volume ratio and particle size distribution of the nanocrystalline magnetic powder and magnetic powder, the composition ratio of the resin composition is optimized, the magnetic permeability is improved, the magnetic loss is reduced, and the coatability is enhanced.

Benefits of technology

A cured material with high relative permeability and low magnetic loss was achieved in the low-frequency band. At the same time, the resin composition has excellent coatability, which supports the miniaturization of sensors and the high performance of switching power supplies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118829692A_ABST
    Figure CN118829692A_ABST
Patent Text Reader

Abstract

A resin composition containing the following components: (A) nanocrystalline magnetic powder having a particle diameter of 5.5 [mu] m or more and 20 [mu] m or less; (B) magnetic powder having a particle diameter of 2 [mu] m or less; and (D) a thermosetting resin, in which the amount of the component (A) is 23-60% by volume (inclusive) with respect to 100% by volume of the non-volatile components of the resin composition, and the amount of the component (B) is 5-30% by volume (inclusive) with respect to 100% by volume of the non-volatile components of the resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition and a method for producing the same. Furthermore, the present invention relates to a cured product obtained from the resin composition, a resin sheet and a method for producing the same, a circuit board, and a sensor board. Background Art

[0002] With the recent trend of miniaturization and lightness of electronic devices and the popularization of portable devices, the miniaturization and high performance of switching power supply circuits are being promoted. Switching power supply circuits generally include inductors (Patent Documents 1 to 3).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2017-69523;

[0006] Patent document 2: International Publication No. 2006 / 54749;

[0007] Patent document 3: Japanese Patent Application Publication No. 2019-192920. Summary of the invention

[0008] Problems to be solved by the invention

[0009] In order to miniaturize the switching power supply, the miniaturization of the inductor is required (Patent Document 1). At this time, if the switching frequency is increased, it is conducive to the miniaturization of the inductor. However, the magnetic material used to form the inductor usually has a larger magnetic loss caused by eddy current loss inside the magnetic powder in the high frequency band, resulting in a decrease in the efficiency of the switching power supply (Patent Document 2). In addition, when the size of the metal magnetic powder is large, the eddy current loss inside the metal magnetic powder becomes larger. Therefore, in high-speed switching operations such as 50MHz to 100MHz, the loss is large and it is difficult to cope with high frequencies (Patent Document 3).

[0010] In this context, there is a recent demand for inductors that can operate at relatively low frequencies of around 10 MHz. Therefore, in order to simultaneously achieve high functionality and miniaturization of inductors, magnetic materials that can achieve high relative permeability and low magnetic loss at low frequencies are required.

[0011] In addition, the resin composition can be applied when it is used. For example, in the case of manufacturing a resin sheet having a resin composition layer comprising a resin composition, the resin composition is sometimes applied on a support. In addition, for example, in the case of filling a hole formed on a substrate with a resin composition, the resin composition is sometimes applied on a substrate to fill the hole. Therefore, it is required that the resin composition has excellent coating properties.

[0012] The present invention is completed in view of the above-mentioned problems, and its purpose is to provide: a resin composition and a method for producing a cured product that can achieve high relative magnetic permeability and low magnetic loss in a low frequency band and has excellent coating properties; a cured product of the resin composition; a resin sheet containing the resin composition and a method for producing the same; and a circuit substrate and an inductor substrate containing the cured product of the resin composition.

[0013] Means for solving problems

[0014] The inventor has conducted in-depth research to solve the above-mentioned problem. As a result, the inventor has found that a resin composition comprising nanocrystalline magnetic powder with a particle size in a specific range, magnetic powder with a particle size in other specific ranges and a thermosetting resin can solve the above-mentioned problem. In addition, the inventor has found that a resin composition comprising nanocrystalline magnetic powder with an average particle size in a specific range, magnetic powder with an average particle size in other specific ranges and a thermosetting resin can solve the above-mentioned problem. The present invention is an invention completed based on these insights.

[0015] That is, the present invention includes the following contents.

[0016] [1] A resin composition comprising the following components:

[0017] (A) nanocrystalline magnetic powder having a particle size of 5.5 μm or more and 20 μm or less;

[0018] (B) magnetic powder having a particle size of 2 μm or less; and

[0019] (D) thermosetting resin,

[0020] The amount of the component (A) is 23% by volume or more and 60% by volume or less relative to 100% by volume of the non-volatile components of the resin composition.

[0021] The amount of the component (B) is 5% by volume or more and 30% by volume or less relative to 100% by volume of the nonvolatile component of the resin composition.

[0022] [2] The resin composition according to [1], wherein the volume ratio of the component (A) to the component (B) (component (A) / component (B)) is 1 to 12.

[0023] [3] The resin composition described in [1] or [2], further comprising (C) magnetic powder,

[0024] The (C) magnetic powder is a magnetic powder other than the above-mentioned (A) component and has a particle size of more than 2 μm and 20 μm or less.

[0025] [4] The resin composition according to any one of [1] to [3], wherein the component (D) comprises an epoxy resin.

[0026] [5] The resin composition according to any one of [1] to [4], further comprising (E) a curing accelerator.

[0027] [6] The method for producing a resin composition according to any one of [1] to [5], comprising mixing the following components:

[0028] (a) nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less;

[0029] (b) magnetic powder having an average particle size of 2 μm or less; and

[0030] (D) Thermosetting resin.

[0031] [7] A method for producing a resin composition, comprising mixing the following components:

[0032] (a) nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less;

[0033] (b) magnetic powder having an average particle size of 2 μm or less; and

[0034] (D) Thermosetting resin.

[0035] [8] The method for producing a resin composition according to [6] or [7], wherein the amount of the component (a) is 30% by volume or more and 80% by volume or less relative to 100% by volume of the non-volatile components of the resin composition.

[0036] [9] The method for producing a resin composition according to any one of [6] to [8], wherein the 10% particle size D of the component (a) is 10 Greater than 2μm.

[0037]

[10] The method for producing a resin composition according to any one of [6] to [9], wherein the amount of the component (b) is 5% by volume or more and 50% by volume or less relative to 100% by volume of the non-volatile components of the resin composition.

[0038]

[11] The method for producing a resin composition according to any one of [6] to

[10] , wherein the 90% particle size D of the component (b) is 90 Less than 5.5μm.

[0039]

[12] The method for producing a resin composition according to any one of [6] to

[11] , further comprising mixing (c) magnetic powder,

[0040] The magnetic powder (c) has an average particle size of more than 2 μm and less than 20 μm, and smaller than the average particle size of the component (a).

[0041]

[13] The method for producing a resin composition according to

[12] , wherein the amount of the (c) magnetic powder is 34% by volume or less relative to 100% by volume of the non-volatile components of the resin composition.

[0042]

[14] A cured product of the resin composition according to any one of [1] to [5].

[0043]

[15] A resin sheet comprising: a support and a resin composition layer formed on the support,

[0044] The resin composition layer includes the resin composition according to any one of [1] to [5].

[0045]

[16] A method for producing a resin sheet, comprising the following steps:

[0046] A step of producing a resin composition by the production method described in any one of [6] to

[13] ; and

[0047] A step of applying the resin composition onto a support.

[0048]

[17] A circuit board comprising a cured product of the resin composition according to any one of [1] to [5].

[0049]

[18] The circuit board described in

[17] comprises: a substrate having through holes formed therein; and a cured product of a resin composition filled in the through holes.

[0050]

[19] A sensor substrate comprising the circuit substrate described in

[17] or

[18] .

[0051] Effects of the Invention

[0052] According to the present invention, there can be provided: a resin composition capable of obtaining a cured product having high relative magnetic permeability and low magnetic loss in a low frequency band and having excellent coating properties, and a method for producing the same; a cured product of the resin composition; a resin sheet comprising the resin composition, and a method for producing the same; and a circuit substrate and an inductor substrate comprising the cured product of the resin composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] [ Figure 1 ] Figure 1 It is a cross-sectional view schematically showing a core substrate prepared in the method for manufacturing a circuit substrate according to the first example of the fourth embodiment of the present invention.

[0054] [ Figure 2 ] Figure 2 It is a cross-sectional view schematically showing a core substrate in which a through hole is formed in the circuit substrate manufacturing method according to the first example of the fourth embodiment of the present invention.

[0055] [ Figure 3 ] Figure 3 It is a cross-sectional view schematically showing a core substrate in which a plating layer is formed in a through hole in a method for manufacturing a circuit substrate according to a first example of a fourth embodiment of the present invention.

[0056] [ Figure 4 ] Figure 4 This is a cross-sectional view schematically showing a state in which a through hole of a core substrate is filled with a resin composition in the method for manufacturing a circuit substrate according to the first example of the fourth embodiment of the present invention.

[0057] [ Figure 5 ] Figure 5 This is a schematic cross-sectional view for explaining step (2) of the method for manufacturing a circuit board according to the first example of the fourth embodiment of the present invention.

[0058] [ Figure 6 ] Figure 6 This is a schematic cross-sectional view for explaining step (3) of the method for manufacturing a circuit board according to the first example of the fourth embodiment of the present invention.

[0059] [ Figure 7 ] Figure 7 This is a schematic cross-sectional view for explaining step (5) of the method for manufacturing a circuit board according to the first example of the fourth embodiment of the present invention.

[0060] [ Figure 8 ] Figure 8 This is a schematic cross-sectional view for explaining step (5) of the method for manufacturing a circuit board according to the first example of the fourth embodiment of the present invention.

[0061] [ Fig. 9 ] Fig. 9 This is a schematic cross-sectional view for explaining the step (i) in the method for manufacturing a circuit board according to the second example of the fourth embodiment of the present invention.

[0062] [ Fig.10 ] Fig.10 This is a schematic cross-sectional view for explaining the step (i) in the method for manufacturing a circuit board according to the second example of the fourth embodiment of the present invention.

[0063] [ Fig.11 ] Fig.11 This is a schematic cross-sectional view for explaining the step (ii) in the method for manufacturing a circuit board according to the second example of the fourth embodiment of the present invention.

[0064] [ Fig.12 ] Fig.12 This is a schematic cross-sectional view for explaining the step (iv) in the method for manufacturing a circuit board according to the second example of the fourth embodiment of the present invention.

[0065] [ Fig.13 ] Fig.13 This is a schematic plan view of a circuit substrate included in the sensor substrate as viewed from one side in the thickness direction of the sensor substrate.

[0066] [ Fig.14 ] Fig.14 It means in Fig.13 The schematic diagram of the cut end surface of the circuit substrate cut at the position indicated by the II-II dot-dash line is shown.

[0067] [ Fig.15 ] Fig.15 It is a schematic plan view for explaining the structure of a first conductor layer of a circuit board included in the sensor substrate. DETAILED DESCRIPTION

[0068] The present invention is described in detail below according to the preferred embodiments of the present invention. However, the present invention is not limited to the following embodiments and examples, and can be implemented by any changes within the scope of the claims and their equivalents. In addition, in the following description, "magnetic permeability" means "relative magnetic permeability" unless otherwise specified.

[0069] <Overview of the resin composition according to the first embodiment>

[0070] The resin composition involved in the first embodiment of the present invention contains the following components: (A) nanocrystalline magnetic powder having a particle size of 5.5 μm or more and 20 μm or less; (B) magnetic powder having a particle size of 2 μm or less; and (D) thermosetting resin. In the following description, "(A) nanocrystalline magnetic powder having a particle size of 5.5 μm or more and 20 μm or less" is sometimes referred to as "(A) nanocrystalline magnetic powder". In addition, "(B) magnetic powder having a particle size of 2 μm or less" is sometimes referred to as "(B) small particle size magnetic powder". The resin composition involved in the first embodiment of the present invention contains (A) nanocrystalline magnetic powder and (B) small particle size magnetic powder in a specific range of amounts.

[0071] The resin composition involved in the first embodiment of the present invention can be cured by thermally curing the (D) thermosetting resin to provide a cured product. The cured product thus obtained can have high relative magnetic permeability and low magnetic loss in a low frequency band (e.g., 10 MHz). In addition, the resin composition involved in the first embodiment of the present invention can generally have excellent coating properties.

[0072] The present inventors speculate the mechanism by which the above-mentioned effect is obtained by the resin composition according to the first embodiment of the present invention as follows. However, the technical scope of the present invention is not limited to the following mechanism.

[0073] (A) Nanocrystalline magnetic powder has the effect of improving the relative magnetic permeability and magnetic loss of the cured product of the resin composition. Specifically, nanocrystalline magnetic powder with a particle size of 5.5 μm or more can have a larger relative magnetic permeability, and nanocrystalline magnetic powder with a particle size of 20 μm or less can have a smaller magnetic loss, so the cured product of the resin composition containing the (A) nanocrystalline magnetic powder with a particle size in the above range can obtain good relative magnetic permeability and magnetic loss.

[0074] In addition, (B) small particle size magnetic powder has the following effects: improving the coating properties of the resin composition, and further improving the relative magnetic permeability and magnetic loss of the cured product of the resin composition. Specifically, magnetic powder with a particle size of 2 μm or less can reduce the viscosity of the resin composition. In addition, magnetic powder with a particle size of 2 μm or less has a small magnetic loss. Therefore, according to (B) small particle size magnetic powder, the amount of magnetic powder in the resin composition increases, the relative magnetic permeability can be improved, and the increase in magnetic loss can be further suppressed compared to the increase in the relative magnetic permeability.

[0075] It is considered that the mechanism for obtaining the effect according to the present embodiment includes the effect of the combination of the above-mentioned (A) nanocrystalline magnetic powder and (B) small-diameter magnetic powder.

[0076] <(A) Nanocrystalline Magnetic Powder According to the First Embodiment>

[0077] The resin composition involved in the first embodiment of the present invention contains (A) nanocrystalline magnetic powder having a particle size in a specific range as the (A) component. In the specification, the term "nanocrystalline magnetic powder" refers to a magnetic powder containing grains with a particle size of less than 100nm. There is no particular restriction on the lower limit of the particle size of the grains, and it is preferably greater than 1nm. Among them, the maximum particle size of the nanocrystalline magnetic powder is preferably less than 100nm. Usually, a plurality of grains are contained in one particle of the nanocrystalline magnetic powder, and therefore, the particles of the nanocrystalline magnetic powder can be polycrystalline. The size of the grains can be observed, for example, by TEM (transmission electron microscope). Since the nanocrystalline magnetic powder contains grains, a peak indicating crystallinity can usually be shown in the X-ray diffraction pattern. As the crystal structure possessed by the grains, for example, bcc crystal structure (body-centered cubic lattice structure) can be cited, but it can also be a crystal structure other than this.

[0078] (A) The nanocrystalline magnetic powder is usually contained in the resin composition in the form of particles. (A) The nanocrystalline magnetic powder may contain crystal grains in at least a portion of its particles, preferably contain crystal grains in the surface layer of the particles, more preferably contain crystal grains in the entire particle, and particularly preferably consist only of crystal grains.

[0079] (A) The nanocrystalline magnetic powder has a particle size in the range of 5.5 μm or more and 20 μm or less. The particle size of the (A) nanocrystalline magnetic powder can be measured by a laser diffraction / scattering method based on Mie scattering theory. Specifically, a laser diffraction and scattering particle size distribution measuring device can be used to prepare the particle size distribution of the (A) nanocrystalline magnetic powder on a volume basis, and the measurement can be performed based on the particle size distribution. The measurement sample can preferably be a sample in which the magnetic powder is dispersed in pure water using ultrasound. As a laser diffraction and scattering particle size distribution measuring device, the "MT3000II" manufactured by MicrotracBEL; the "LA-960" manufactured by Horiba, Ltd.; the "SALD-2200" manufactured by Shimadzu Corporation, etc. can be used.

[0080] The resin composition involved in the first embodiment of the present invention comprises (A) nanocrystalline magnetic powder having a particle size in the above-mentioned range in an amount within a specific range. Specifically, relative to the non-volatile components of 100% by volume of the resin composition, the amount (volume %) of (A) nanocrystalline magnetic powder is usually more than 23% by volume, preferably more than 25% by volume, more preferably more than 28% by volume, usually less than 60% by volume, preferably less than 50% by volume, more preferably less than 40% by volume. When using such an amount of (A) nanocrystalline magnetic powder, both relative permeability and magnetic loss can be improved in the low frequency band, and the coating property of the resin composition can be made good.

[0081] (A) nanocrystalline magnetic powder can be particles of a magnetic material having a relative magnetic permeability greater than 1. The magnetic material is usually an inorganic material, and can be a soft magnetic material or a hard magnetic material. In addition, one type of magnetic material can be used alone, or two or more types can be used in combination. Among them, from the viewpoint of suppressing the uneven distribution of (A) nanocrystalline magnetic powder, a soft magnetic material is preferably used as the magnetic material contained in (A) nanocrystalline magnetic powder.

[0082] As the magnetic material contained in the (A) nanocrystalline magnetic powder, for example, there can be mentioned: magnetic metal oxides, magnetic metals. Among them, the magnetic material contained in the (A) nanocrystalline magnetic powder preferably contains iron (Fe). Therefore, as the magnetic material contained in the (A) nanocrystalline magnetic powder, there can be mentioned: crystalline iron alloy magnetic materials, crystalline ferrite magnetic materials, etc. From the viewpoint of significantly exerting the effect of the present invention, the magnetic material contained in the (A) nanocrystalline magnetic powder preferably has the following composition: in combination with Fe, it also contains one or more elements selected from Nb, Hf, Zr, Ta, Mo, W and V.

[0083] Preferred examples of the magnetic material contained in the (A) nanocrystalline magnetic powder include magnetic materials described in Japanese Patent Application Publication No. 2021-158343, Japanese Patent Application Publication No. 2021-141267, Japanese Patent Application Publication No. 2019-31463, Japanese Patent Application Publication No. 2021-11602, etc.

[0084] Among the above examples, Fe-Si-Nb-B alloy powder is preferred from the viewpoint of significantly obtaining the desired effect of the present invention. The Fe-Si-Nb-B alloy powder refers to magnetic powder formed of an alloy containing Fe, Si, Nb, and B.

[0085] The (A) nanocrystalline magnetic powder preferably contains the above-mentioned magnetic material, and preferably contains only the above-mentioned magnetic material. The (A) nanocrystalline magnetic powder may be used alone or in combination of two or more.

[0086] (A) Nanocrystalline magnetic powder can be manufactured, for example, by an atomization method. As a specific example of the method for manufacturing (A) nanocrystalline magnetic powder, there can be cited: the method described in Japanese Patent Gazette No. 2021-141267 and Japanese Patent Gazette No. 2021-158343. In addition, commercially available (A) nanocrystalline magnetic powder can be used. As commercially available magnetic powders containing (A) nanocrystalline magnetic powder, for example, there can be cited: "KUAMET NC1-38um", "ATFINE-NC1 PF10FA" manufactured by Epson Atmix, etc. However, commercially available magnetic powders generally have a wide particle size distribution, and therefore may contain particles with a particle size that deviates from the range of 5.5μm or more and 20μm or less. Therefore, when obtaining (A) nanocrystalline magnetic powder from the market, the commercially available magnetic powder can be classified and used as needed.

[0087] The (A) nanocrystalline magnetic powder is preferably spherical. The value (aspect ratio) obtained by dividing the major axis length of the particles of the (A) nanocrystalline magnetic powder by the minor axis length is preferably 2 or less, more preferably 1.5 or less, further preferably 1.2 or less, and is usually 1 or more, preferably greater than 1, and more preferably 1.05 or more.

[0088] Relative to 100% by volume of the non-volatile components of the resin composition, the amount (volume %) of (A) nanocrystalline magnetic powder is represented by "V(A)", and the amount (volume %) of (B) small-particle-size magnetic powder is represented by "V(B)". In this case, the volume ratio of (A) nanocrystalline magnetic powder to (B) small-particle-size magnetic powder contained in the resin composition ((A) nanocrystalline magnetic powder / (B) small-particle-size magnetic powder) can be represented by "V(A) / V(B)". The volume ratio V(A) / V(B) is usually greater than 0.8, preferably greater than 1, more preferably greater than 1.2, and particularly preferably greater than 1.4, and is usually less than 12, preferably less than 8.4, more preferably less than 7.0, further preferably less than 6.0, and particularly preferably less than 5.0. When the volume ratio V(A) / V(B) is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0089] In addition, relative to 100 volume % of the non-volatile components of the resin composition, the total amount (volume %) of (A) nanocrystalline magnetic powder and (B) small-particle magnetic powder contained in the resin composition can be expressed as "V(A)+V(B)". The total amount (volume %) V(A)+V(B) is usually more than 28 volume %, preferably more than 34 volume %, more preferably more than 38 volume %, particularly preferably more than 40 volume %, preferably less than 72 volume %, more preferably less than 68 volume %, further preferably less than 64 volume %, particularly preferably less than 60 volume %. When the total amount (volume %) V(A)+V(B) of (A) nanocrystalline magnetic powder and (B) small-particle magnetic powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0090] The total amount (volume %) of all magnetic powders in the resin composition is preferably 30% by volume or more, more preferably 40% by volume or more, particularly preferably 50% by volume or more, and preferably 95% by volume or less, more preferably 90% by volume or less, particularly preferably 85% by volume or less, relative to 100% by volume of the non-volatile components of the resin composition. When the total amount (volume %) of the magnetic powder is within the above range, both the relative permeability and the magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0091] Relative to the total amount of all magnetic powders in the resin composition of 100 volume %, the total amount (volume %) of (A) nanocrystalline magnetic powder and (B) small-particle-diameter magnetic powder is preferably 40 volume % or more, more preferably 50 volume % or more, and particularly preferably 54 volume % or more, for example, it can be 100 volume % or less, 90 volume % or less, 80 volume % or less, etc. When the total amount (volume %) of (A) nanocrystalline magnetic powder and (B) small-particle-diameter magnetic powder is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0092] Relative to the non-volatile components of 100% by mass of the resin composition, the amount (mass %) of the (A) nanocrystalline magnetic powder is preferably 30% by mass or more, more preferably 34% by mass or more, particularly preferably 38% by mass or more, preferably 60% by mass or less, preferably 56% by mass or less, and more preferably 52% by mass or less. When the amount (mass %) of the (A) nanocrystalline magnetic powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0093] Relative to 100% by mass of the non-volatile components of the resin composition, the amount (mass %) of (A) nanocrystalline magnetic powder is represented by "M(A)", and the amount (mass %) of (B) small-particle magnetic powder is represented by "M(B)". In this case, the mass ratio of (A) nanocrystalline magnetic powder to (B) small-particle magnetic powder contained in the resin composition ((A) nanocrystalline magnetic powder / (B) small-particle magnetic powder) can be represented by "M(A) / M(B)". The mass ratio M(A) / M(B) is preferably greater than 1.0, more preferably greater than 1.2, and particularly preferably greater than 1.4, and is preferably less than 10, more preferably less than 8, and particularly preferably less than 6. When the mass ratio M(A) / M(B) is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and the coating properties of the resin composition can be improved.

[0094] In addition, relative to 100% by mass of the non-volatile components of the resin composition, the total amount (mass %) of (A) nanocrystalline magnetic powder and (B) small-particle magnetic powder contained in the resin composition can be expressed as "M(A)+M(B)". The total amount (mass %) M(A)+M(B) is preferably 40% by mass or more, more preferably 45% by mass or more, further preferably 50% by mass or more, particularly preferably 53% by mass or more, preferably 90% by mass or less, more preferably 80% by mass or less, particularly preferably 70% by mass or less. When the total amount (mass %) M(A)+M(B) is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and the coating properties of the resin composition can be made better.

[0095] The total amount (mass%) of all magnetic powders in the resin composition is preferably 80% by mass or more, more preferably 85% by mass or more, particularly preferably 90% by mass or more, preferably 99% by mass or less, more preferably 98% by mass or less, particularly preferably 97% by mass or less, relative to 100% by mass of the non-volatile components of the resin composition. When the total amount (mass%) of the magnetic powder is within the above range, both the relative permeability and the magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0096] Relative to the total amount of all magnetic powders in the resin composition of 100 mass%, the total amount (mass %) of (A) nanocrystalline magnetic powder and (B) small-particle-diameter magnetic powder is preferably 50 mass % or more, more preferably 53 mass % or more, and particularly preferably 55 mass % or more, for example, it can be 100 mass % or less, 90 mass % or less, 80 mass % or less, 70 mass % or less, etc. When the total amount (mass %) of (A) nanocrystalline magnetic powder and (B) small-particle-diameter magnetic powder is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0097] <(B) Small-diameter magnetic powder according to the first embodiment>

[0098] The resin composition involved in the first embodiment of the present invention contains (B) small-particle magnetic powder having a particle size in a specific range as the (B) component. The (B) small-particle magnetic powder is usually contained in the resin composition in the form of particles. The (B) small-particle magnetic powder has a particle size of less than 2 μm. The particle size of the (B) small-particle magnetic powder can be measured by the same method as the particle size of the (A) nanocrystalline magnetic powder.

[0099] The resin composition involved in the first embodiment of the present invention contains (B) small-particle magnetic powder having a particle size in the above-mentioned range in an amount within a specific range. Specifically, relative to 100% by volume of the non-volatile components of the resin composition, the amount (volume %) of (B) small-particle magnetic powder is usually 5% by volume or more, preferably 6% by volume or more, and more preferably 7% by volume or more, and is usually 30% by volume or less, preferably 26% by volume or less, and more preferably 22% by volume or less. When such an amount of (B) small-particle magnetic powder is used, both relative permeability and magnetic loss can be improved in the low frequency band, and the coating property of the resin composition can be improved.

[0100] (B) Small particle size magnetic powder may be nanocrystalline magnetic powder containing crystal grains, may be amorphous magnetic powder without crystal grains, may be crystalline magnetic powder other than nanocrystalline magnetic powder, or may be a combination thereof. Nanocrystalline magnetic powder is as described in the item of (A) nanocrystalline magnetic powder. On the other hand, since amorphous magnetic materials are amorphous, specific peaks indicating crystallinity are usually not shown in the X-ray diffraction pattern. Usually, in the X-ray diffraction pattern of amorphous magnetic powder, a wide pattern without peaks indicating crystallinity appears.

[0101] (B) The small-particle magnetic powder may be particles of a magnetic material having a relative magnetic permeability greater than 1. The magnetic material is usually an inorganic material, and may be a soft magnetic material or a hard magnetic material. In addition, one type of magnetic material may be used alone, or two or more types may be used in combination. Among them, from the viewpoint of suppressing the uneven distribution of the (B) small-particle magnetic powder, a soft magnetic material is preferably used as the magnetic material contained in the (B) small-particle magnetic powder.

[0102] Examples of the magnetic material contained in the (B) small-diameter magnetic powder include magnetic metal oxide materials and magnetic metal materials.

[0103] As magnetic metal oxide materials, for example, there can be mentioned: ferrite-based magnetic materials; and iron oxide materials such as iron oxide powder (III) and iron oxide powder. Among them, ferrite-based magnetic materials are preferred. Ferrite-based magnetic materials are generally composite oxides with iron oxide as the main component and are chemically stable. Therefore, when using ferrite-based magnetic materials, advantages such as high corrosion resistance, low risk of fire, and difficulty in demagnetization are obtained.

[0104] As ferrite-based magnetic materials, for example, there can be mentioned: Fe-Mn ferrite, Fe-Mn-Mg ferrite, Fe-Mn-Mg-Sr ferrite, Fe-Mg-Zn ferrite, Fe-Mg-Sr ferrite, Fe-Zn-Mn ferrite, Fe-Cu-Zn ferrite, Fe-Ni-Zn ferrite, Fe-Ni-Zn-Cu ferrite, Fe-Ba-Zn ferrite, Fe-Ba-Mg ferrite, Fe-Ba-Ni ferrite, Fe-Ba-Co ferrite, Fe-Ba-Ni-Co ferrite, Fe-Y ferrite, etc.

[0105] Among the ferrite-based magnetic materials, from the viewpoint of significantly obtaining the desired effect of the present invention, ferrites containing at least one element selected from Mn, Zn, Ni and Cu are preferred, and ferrites containing Mn are particularly preferred. Therefore, as preferred ferrite-based magnetic materials, for example, there can be mentioned: Fe-Mn-based ferrites, Fe-Mn-Mg-based ferrites, Fe-Mn-Mg-Sr-based ferrites, Fe-Mg-Zn-based ferrites, Fe-Zn-Mn-based ferrites, Fe-Cu-Zn-based ferrites, Fe-Ni-Zn-based ferrites, Fe-Ni-Zn-Cu-based ferrites, Fe-Ba-Zn-based ferrites, Fe-Ba-Ni-based ferrites, and Fe-Ba-Ni-Co-based ferrites. Among them, Fe-Mn ferrite, Fe-Mn-Mg ferrite, Fe-Mn-Mg-Sr ferrite and Fe-Zn-Mn ferrite are preferred, and Fe-Mn ferrite is particularly preferred. Fe-Mn ferrite refers to ferrite containing Fe and Mn.

[0106] As magnetic metal materials, for example, pure iron, Fe-Si alloys, Fe-Si-Al alloys, Fe-Cr alloys, Fe-Cr-Si alloys, Fe-Ni-Cr alloys, Fe-Cr-Al alloys, Fe-Ni alloys, Fe-Ni-B alloys, Fe-Ni-Mo alloys, Fe-Ni-Mo-Cu alloys, Fe-Co alloys, Fe-Ni-Co alloys, Co-based amorphous alloys, and other crystalline or amorphous alloy magnetic materials can be cited. Among the magnetic metal materials, iron alloy magnetic materials are more preferred. From the viewpoint of significantly obtaining the desired effect of the present invention, iron alloy magnetic materials containing Fe and at least one element selected from Si, Cr, Al, Ni and Co are preferred, and Fe-Si-Cr alloys are particularly preferred. Fe-Si-Cr alloy materials refer to alloys containing Fe, Si and Cr.

[0107] As the magnetic material contained in the (B) small-particle magnetic powder, the magnetic material described as the magnetic material of the (A) nanocrystalline magnetic powder can be used. The magnetic material contained in the (B) small-particle magnetic powder may be the same as or different from the magnetic material of the (A) nanocrystalline magnetic powder.

[0108] The small-particle-diameter magnetic powder (B) preferably contains the above-mentioned magnetic material, and preferably contains only the above-mentioned magnetic material. The small-particle-diameter magnetic powder (B) may be used alone or in combination of two or more.

[0109] As (B) small-particle magnetic powder, commercially available magnetic powder can be used. Specific examples of commercially available magnetic powder include: "MZ03S", "M05S", "M001", and "MZ05S" manufactured by Powdertech; "PST-S" manufactured by Sanyo Special Steel Co., Ltd.; "AW2-08", "AW2-08PF20F", "AW2-08PF10F", "AW2-08PF3F", "Fe-3.5Si-4.5CrPF20F", "Fe-50NiPF20F", "Fe-80Ni-4MoPF20F", "ATFINE-NC1 "PF5FA", "ATFINE-NC1PF3FA" manufactured by JFE Chemical Co., Ltd.; "CVD iron powder (0.7μm)", "LD-M", "LD-MH", "KNI-106", "KNI-106GSM", "KNI-106GS", "KNI-109", "KNI-109GSM", "KNI-109GS" manufactured by Toda Industry Co., Ltd.; "KNS-415", "BSF-547", "BSF-029", "BSN-125", "BSN-125", "BSN-714", "BSN-828", "S-1281", "S-1641", "S-1651", "S-1470", "S-1511", "S-2430" manufactured by Japan Heavy Chemical Industry Co., Ltd.; "JR09P2" manufactured by Nippon Heavy Chemical Industry Co., Ltd.; "Nanotek" manufactured by CIK NanoTek; KINSEI "JEMK-S" and "JEMK-H" manufactured by MATEC; "Yttrium iron oxide" manufactured by ALDRICH; "MA-RCO-5" manufactured by DOWA ELECTRONICS, etc. However, commercially available magnetic powders generally have a wide particle size distribution, and therefore may contain particles with a particle size that deviates from the range of 2 μm or less. Therefore, when obtaining (B) small-particle-size magnetic powders from the market, the commercially available magnetic powders may be classified and used as needed.

[0110] The (B) small-particle magnetic powder is preferably spherical. The aspect ratio of the (B) small-particle magnetic powder can be in the same range as the aspect ratio of the (A) nanocrystalline magnetic powder. The aspect ratio of the (B) small-particle magnetic powder can be the same as or different from the aspect ratio of the (A) nanocrystalline magnetic powder.

[0111] The amount (mass %) of the small-particle magnetic powder (B) relative to 100 mass % of the non-volatile components of the resin composition is preferably 5 mass % or more, more preferably 7 mass % or more, particularly preferably 9 mass % or more, and preferably 40 mass % or less, preferably 35 mass % or less, and more preferably 30 mass % or less. When the amount (mass %) of the small-particle magnetic powder (B) is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0112] <(C) Intermediate Magnetic Powder According to First Embodiment>

[0113] The resin composition involved in the first embodiment of the present invention may further contain (C) magnetic powder as an optional component. The (C) magnetic powder as the (C) component refers to magnetic powder other than the (A) nanocrystalline magnetic powder having a particle size greater than 2μm and less than 20μm. The (C) magnetic powder is sometimes referred to as "(C) intermediate magnetic powder". The particle size of the (C) intermediate magnetic powder can be measured by the same method as the particle size of the (A) nanocrystalline magnetic powder. The (C) intermediate magnetic powder does not contain (A) nanocrystalline magnetic powder and (B) small particle size magnetic powder. After sorting, the (C) intermediate magnetic powder contains the following (C1) and (C2) magnetic powders.

[0114] (C1) magnetic powder, which is nanocrystalline magnetic powder and has a particle size greater than 2 μm and less than 5.5 μm;

[0115] (C2) Magnetic powder, which is a magnetic powder other than nanocrystalline magnetic powder and has a particle size of more than 2 μm and 20 μm or less.

[0116] According to the intermediate magnetic powder (C), the ratio of the magnetic powder in the resin composition can be increased, so the relative magnetic permeability of the cured product of the resin composition can be increased. Generally, the magnetic loss of the cured product can be increased according to the magnetic powder, but since the intermediate magnetic powder (C) has a small particle size, the increase in the magnetic loss can be suppressed. Therefore, according to the intermediate magnetic powder (C), the increase in magnetic loss can be suppressed and the relative magnetic permeability can be improved.

[0117] The (C) intermediate magnetic powder may be nanocrystalline magnetic powder containing crystal grains, may be amorphous magnetic powder without crystal grains, may be crystalline magnetic powder other than nanocrystalline magnetic powder, or may be a combination of these. The (C) intermediate magnetic powder may be particles of a magnetic material having a relative magnetic permeability greater than 1. As the magnetic material contained in the (C) intermediate magnetic powder, the magnetic material described as the magnetic material of the (B) small particle size magnetic powder may be used. The magnetic material contained in the (C) intermediate magnetic powder may be the same as or different from the magnetic material of the (B) small particle size magnetic powder. The (C) intermediate magnetic powder preferably contains the above-mentioned magnetic material, and preferably contains only the above-mentioned magnetic material. In addition, the (C) intermediate magnetic powder may be used alone or in combination of two or more.

[0118] As (C) intermediate magnetic powder, commercially available magnetic powder can be used. As specific examples of commercially available magnetic powder, the same examples as (B) small-particle-size magnetic powder can be cited. However, commercially available magnetic powder generally has a wide particle size distribution, and therefore may contain particles whose particle size deviates from the range of greater than 2 μm and less than 5.5 μm or the range of greater than 2 μm and less than 20 μm. Therefore, when obtaining (C) intermediate magnetic powder from the market, the commercially available magnetic powder can be classified and used as needed.

[0119] The (C) intermediate magnetic powder is preferably spherical. The range of the aspect ratio of the particles of the (C) intermediate magnetic powder can be the same as the range of the aspect ratio of the (A) nanocrystalline magnetic powder. The aspect ratio of the (C) intermediate magnetic powder can be the same as or different from the aspect ratio of the (A) nanocrystalline magnetic powder. In addition, the aspect ratio of the (C) intermediate magnetic powder can be the same as or different from the aspect ratio of the (B) small particle size magnetic powder.

[0120] The amount (volume %) of the intermediate magnetic powder (C) relative to 100% by volume of the non-volatile components of the resin composition may be 0% by volume or more than 0% by volume, preferably 1% by volume or more, more preferably 3% by volume or more, particularly preferably 5% by volume or more, and preferably 25% by volume or less, more preferably 15% by volume or less, particularly preferably 13% by volume or less. When the amount (volume %) of the intermediate magnetic powder (C) is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be improved.

[0121] The amount (volume %) of the (C) intermediate magnetic powder relative to 100% by volume of the non-volatile components of the resin composition is represented by "V(C)". In this case, the volume ratio of the (A) nanocrystalline magnetic powder to the (C) intermediate magnetic powder contained in the resin composition ((C) intermediate magnetic powder / (A) nanocrystalline magnetic powder) can be represented by "V(C) / V(A)". The volume ratio V(C) / V(A) can be 0 or greater than 0, preferably greater than 0.01, more preferably greater than 0.1, preferably less than 1.0, more preferably less than 0.9, and particularly preferably less than 0.8. When the volume ratio V(C) / V(A) is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and the coating properties of the resin composition can be improved.

[0122] In addition, the volume ratio of the (B) small-particle magnetic powder to the (C) intermediate magnetic powder contained in the resin composition ((C) intermediate magnetic powder / (B) small-particle magnetic powder) can be expressed as "V(C) / V(B)". The volume ratio V(C) / V(B) can be 0 or greater than 0, and is preferably 0.01 or more, more preferably 0.1 or more, preferably 8 or less, more preferably 5 or less, and particularly preferably 2 or less. When the volume ratio V(C) / V(B) is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be improved.

[0123] The total amount (volume %) of (A) nanocrystalline magnetic powder, (B) small-particle magnetic powder and (C) intermediate magnetic powder relative to 100% by volume of the non-volatile component of the resin composition is preferably 30% by volume or more, preferably 40% by volume or more, particularly preferably 50% by volume or more, preferably 90% by volume or less, more preferably 80% by volume or less, particularly preferably 70% by volume or less. When the total amount (volume %) of (A) nanocrystalline magnetic powder, (B) small-particle magnetic powder and (C) intermediate magnetic powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0124] Relative to the total amount of all magnetic powders in the resin composition of 100 volume %, the total amount (volume %) of (A) nanocrystalline magnetic powder, (B) small-particle magnetic powder and (C) intermediate magnetic powder is preferably 50 volume % or more, more preferably 60 volume % or more, particularly preferably 70 volume % or more, and usually 100 volume % or less. This value is large, indicating that there are few giant magnetic powders with a particle size greater than 20 μm in the resin composition. When the total amount (volume %) of (A) nanocrystalline magnetic powder, (B) small-particle magnetic powder and (C) intermediate magnetic powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0125] The amount (mass %) of the intermediate magnetic powder (C) relative to 100 mass % of the non-volatile components of the resin composition may be 0 mass % or more, preferably 1 mass % or more, more preferably 3 mass % or more, particularly preferably 5 mass % or more, preferably 40 mass % or less, more preferably 35 mass % or less, particularly preferably 30 mass % or less. When the amount (mass %) of the intermediate magnetic powder (C) is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be improved.

[0126] The amount (mass %) of the (C) intermediate magnetic powder relative to 100 mass % of the non-volatile components of the resin composition is represented by "M(C)". In this case, the mass ratio of the (A) nanocrystalline magnetic powder to the (C) intermediate magnetic powder contained in the resin composition ((C) intermediate magnetic powder / (A) nanocrystalline magnetic powder) can be represented by "M(C) / M(A)". The mass ratio M(C) / M(A) can be 0 or greater than 0, preferably greater than 0.01, more preferably greater than 0.1, preferably less than 1.0, more preferably less than 0.9, and particularly preferably less than 0.8. When the mass ratio M(C) / M(A) is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and the coating properties of the resin composition can be improved.

[0127] In addition, the mass ratio of the (B) small-particle magnetic powder to the (C) intermediate magnetic powder contained in the resin composition ((C) intermediate magnetic powder / (B) small-particle magnetic powder) can be expressed as "M(C) / M(B)". The mass ratio M(C) / M(B) can be 0 or greater than 0, and is preferably 0.01 or more, more preferably 0.1 or more, preferably 8 or less, more preferably 5 or less, and particularly preferably 2 or less. When the mass ratio M(C) / M(B) is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and the coating properties of the resin composition can be improved.

[0128] The total amount (mass %) of (A) nanocrystalline magnetic powder, (B) small-particle magnetic powder and (C) intermediate magnetic powder relative to 100% by mass of the non-volatile components of the resin composition is preferably 40% by mass or more, preferably 50% by mass or more, particularly preferably 60% by mass or more, preferably 99% by mass or less, and more preferably 98% by mass or less. When the total amount (mass %) of (A) nanocrystalline magnetic powder, (B) small-particle magnetic powder and (C) intermediate magnetic powder is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0129] Relative to the total amount of all magnetic powders in the resin composition of 100 mass %, the total amount (mass %) of (A) nanocrystalline magnetic powder, (B) small-particle magnetic powder and (C) intermediate magnetic powder is preferably 50 mass % or more, more preferably 60 mass % or more, particularly preferably 70 mass % or more, and usually 100 mass % or less. This value is large, indicating that there are few giant magnetic powders with a particle size greater than 20 μm in the resin composition. When the total amount (mass %) of (A) nanocrystalline magnetic powder, (B) small-particle magnetic powder and (C) intermediate magnetic powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0130] <(D) Thermosetting resin according to the first embodiment>

[0131] The resin composition according to the first embodiment of the present invention contains a (D) thermosetting resin as the (D) component. Examples of the (D) thermosetting resin include epoxy resins, phenolic resins, thiol resins, benzoic acid resins, and the like. Oxazine resins, active ester resins, cyanate resins, carbodiimide resins, amine resins, acid anhydride resins, epoxy acrylate resins, urethane acrylate resins, urethane resins, polyimide resins, unsaturated polyester resins, melamine resins, silicone resins, phenoxy resins, etc. In addition, the (D) thermosetting resin may be used alone or in combination of two or more.

[0132] The (D) thermosetting resin preferably includes an epoxy resin. An epoxy resin is a resin having an epoxy group. When the (D) thermosetting resin includes an epoxy resin, the coating property of the resin composition can be particularly good, and the relative magnetic permeability and magnetic loss of the cured product can be particularly excellent.

[0133] Examples of the epoxy resin include biphenylol epoxy resins, bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, bisphenol AF epoxy resins, dicyclopentadiene epoxy resins, trisphenol epoxy resins, naphthol novolac epoxy resins, phenol novolac epoxy resins, tert-butylcatechol epoxy resins, naphthalene epoxy resins, naphthol epoxy resins, anthracene epoxy resins, glycidylamine epoxy resins, glycidyl Ester type epoxy resin, cresol novolac type epoxy resin, biphenyl type epoxy resin, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexane type epoxy resin, cyclohexanedimethanol type epoxy resin, naphthylene ether type epoxy resin, trimethylol type epoxy resin, tetraphenylethane type epoxy resin, glycidyl ether type aliphatic epoxy resin, glycidyl ether type aromatic epoxy resin, etc. The epoxy resin may be used alone or in combination of two or more.

[0134] The resin composition preferably contains an epoxy resin having two or more epoxy groups in one molecule as the epoxy resin. From the viewpoint of significantly obtaining the desired effect of the present invention, the amount of the epoxy resin having two or more epoxy groups in one molecule is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more relative to 100% by mass of the non-volatile component of the epoxy resin.

[0135] The epoxy resin preferably has an aromatic structure. When two or more epoxy resins are used, preferably one or more epoxy resins have an aromatic structure. The aromatic structure refers to a chemical structure generally defined as aromatic, and also includes polycyclic aromatics and aromatic heterocycles.

[0136] The epoxy resin includes an epoxy resin that is liquid at a temperature of 25°C (hereinafter sometimes referred to as "liquid epoxy resin") and an epoxy resin that is solid at a temperature of 25°C (hereinafter sometimes referred to as "solid epoxy resin"). The resin composition may include only a liquid epoxy resin, only a solid epoxy resin, or a combination of a liquid epoxy resin and a solid epoxy resin as the epoxy resin. Among them, it is preferred that the epoxy resin includes only a liquid epoxy resin.

[0137] The amount of the liquid epoxy resin relative to 100% by mass of the total epoxy resin is preferably 60% by mass or more, more preferably 80% by mass or more, further preferably 90% by mass or more, and particularly preferably 100% by mass.

[0138] As the liquid epoxy resin, a liquid epoxy resin having two or more epoxy groups in one molecule is preferred.

[0139] As the liquid epoxy resin, preferred are glycyrrhizin type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ether type aliphatic epoxy resin, glycidyl ether type aromatic epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexanedimethanol type epoxy resin, dicyclopentadiene type epoxy resin and epoxy resin having a butadiene structure, and more preferred are bisphenol A type epoxy resin, bisphenol F type epoxy resin, glycidyl ether type aliphatic epoxy resin and glycidyl ether type aromatic epoxy resin.

[0140] Specific examples of liquid epoxy resins include: "HP4032", "HP4032D", and "HP4032SS" (naphthalene-type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL" (bisphenol A-type epoxy resins), "jER807" (bisphenol F-type epoxy resins), and "jER152" (phenol novolac-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "630" and "630LSD" (glycidyl ether-type aromatic epoxy resins) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (liquidoxyl alcohol-type epoxy resin (ADEKA Corporation); "ZX-1059" (a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin) manufactured by Nippon Steel Chemicals Co., Ltd.; "EX-721" (glycidyl ester epoxy resin) manufactured by Nagase ChemteX; "Celloxide 2021P" (alicyclic epoxy resin with ester skeleton) and "PB-3600" (epoxy resin with butadiene structure) manufactured by Daicel Corporation; "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane) manufactured by Nippon Steel Chemicals Co., Ltd.

[0141] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferred, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferred.

[0142] As solid epoxy resins, preferred are biphenylol-type epoxy resins, naphthalene-type epoxy resins, naphthalene-type tetrafunctional epoxy resins, naphthol novolac-type epoxy resins, cresol novolac-type epoxy resins, dicyclopentadiene-type epoxy resins, trisphenol-type epoxy resins, naphthol-type epoxy resins, biphenyl-type epoxy resins, naphthylene ether-type epoxy resins, anthracene-type epoxy resins, bisphenol A-type epoxy resins, bisphenol AF-type epoxy resins, phenol aralkyl-type epoxy resins, tetraphenylethane-type epoxy resins, phenol phthalimide-type epoxy resins, and phenolphthalein-type epoxy resins.

[0143] Specific examples of solid epoxy resins include: "HP4032H" manufactured by DIC Corporation (naphthalene-type epoxy resin); "HP-4700" and "HP-4710" manufactured by DIC Corporation (naphthalene-type tetrafunctional epoxy resin); "N-690" manufactured by DIC Corporation (cresol novolac-type epoxy resin); "N-695" manufactured by DIC Corporation (cresol novolac-type epoxy resin); "HP-7200", "HP-7200HH", "HP-7200H", and "HP-7200L" manufactured by DIC Corporation (dicyclopentadiene-type epoxy resin); DIC "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000" (naphthylene ether type epoxy resin) manufactured by Company C; "EPPN-502H" (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC7000L" (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC3000H", "NC3000", "NC3000L", "NC3000FH", "NC3100" (biphenyl type epoxy resin) manufactured by Nippon Kayaku Co., Ltd. ); "ESN475V" manufactured by Nippon Steel Chemicals (naphthalene type epoxy resin); "ESN485" manufactured by Nippon Steel Chemicals (naphthol type epoxy resin); "ESN375" manufactured by Nippon Steel Chemicals (dihydroxynaphthalene type epoxy resin); "YX4000H", "YX4000", "YX4000HK", "YL7890" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YX7700" (phenol aralkyl type epoxy resin) manufactured by Osaka Gas Chemical Co., Ltd.; "PG-100" and "CG-500" manufactured by Osaka Gas Chemical Co., Ltd.; "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "jER1010" (bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "WHR991S" (phenol phthalimide type epoxy resin) manufactured by Nippon Kayaku Co., Ltd., etc. These can be used alone or in combination of two or more.

[0144] As the epoxy resin, when a solid epoxy resin and a liquid epoxy resin are used in combination, the mass ratio of the solid epoxy resin to the liquid epoxy resin (solid epoxy resin / liquid epoxy resin) is not particularly limited, but is preferably 1 or less, more preferably 0.5 or less, further preferably 0.1 or less, further preferably 0.05 or less, and particularly preferably 0.01 or less.

[0145] The epoxy equivalent of the epoxy resin is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., further preferably 80 g / eq. to 2000 g / eq., and further preferably 110 g / eq. to 1000 g / eq. The epoxy equivalent is the mass of the resin per 1 equivalent of epoxy group. The epoxy equivalent can be measured according to JIS K7236.

[0146] From the viewpoint of significantly obtaining the desired effects of the present invention, the weight average molecular weight (Mw) of the epoxy resin is preferably 100 to 5000, more preferably 250 to 3000, and even more preferably 400 to 1500. The weight average molecular weight of the resin can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).

[0147] The amount (volume %) of the epoxy resin relative to 100% by volume of the non-volatile components in the resin composition is preferably 2.5% by volume or more, more preferably 4.0% by volume or more, particularly preferably 4.5% by volume or more, and preferably 10.0% by volume or less, more preferably 9.0% by volume or less, particularly preferably 8.0% by volume or less. When the amount (volume %) of the epoxy resin is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0148] The amount (mass %) of the epoxy resin relative to 100 mass % of the non-volatile components in the resin composition is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, particularly preferably 1.0 mass % or more, preferably 20 mass % or less, more preferably 15 mass % or less, and further preferably 10 mass % or less. When the amount (mass %) of the epoxy resin is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0149] When the (D) thermosetting resin includes an epoxy resin, the (D) thermosetting resin may further include an epoxy curing agent. The epoxy curing agent refers to a thermosetting resin that can react with the epoxy resin to cure the resin composition. Examples of the epoxy curing agent include phenolic resins, carbodiimide resins, acid anhydride resins, amine resins, benzoic acid resins, and the like. Oxazine-based resins, active ester-based resins, cyanate-based resins, thiol-based resins, etc. The epoxy curing agent may be used alone or in combination of two or more.

[0150] As the phenolic resin, a resin having one or more, preferably two or more, hydroxyl groups bonded to an aromatic ring such as a benzene ring or a naphthalene ring in one molecule can be used. As the phenolic resin, biphenyl type resins, naphthalene type resins, phenol novolac type resins, naphthylene ether type resins, and phenolic resins containing a triazine skeleton are preferred. Specific examples include: biphenyl resins "MEH-7700", "MEH-7810", "MEH-7851" (manufactured by Meiwa Chemicals); naphthalene resins "NHN", "CBN", "GPH" (manufactured by Nippon Kayaku); "SN170", "SN180", "SN190", "SN475", "SN485", "SN495", "SN375", "SN395" (manufactured by Nippon Steel Chemical); "EXB9500" (manufactured by DIC); phenol novolac resin "TD2090" (manufactured by DIC); naphthylene ether resin "EXB-6000" (manufactured by DIC). Specific examples of phenolic resins containing a triazine skeleton include: "LA3018", "LA7052", "LA7054", "LA1356" (manufactured by DIC). In particular, naphthalene resins and phenolic resins containing a triazine skeleton are more suitable.

[0151] As the carbodiimide resin, a resin having one or more, preferably two or more carbodiimide structures in one molecule can be used. Examples of the carbodiimide resin include aliphatic biscarbodiimides such as tetramethylene-bis(tert-butylcarbodiimide) and cyclohexanebis(methylene-tert-butylcarbodiimide); biscarbodiimides such as aromatic biscarbodiimides such as phenylene-bis(xylylcarbodiimide); aliphatic polycarbodiimides such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), poly(isophoronecarbodiimide); poly(phenylenecarbodiimide), poly(xylylenecarbodiimide); Polycarbodiimides such as aromatic polycarbodiimides such as naphthyl carbodiimide), poly(tolylene carbodiimide), poly(methyl diisopropyl phenylene carbodiimide), poly(triethyl phenylene carbodiimide), poly(diethyl phenylene carbodiimide), poly(triisopropyl phenylene carbodiimide), poly(diisopropyl phenylene carbodiimide), poly(xylylene carbodiimide), poly(tetramethyl xylylene carbodiimide), poly(methylene diphenylene carbodiimide), poly[methylene bis(methyl phenylene) carbodiimide], etc. Examples of commercially available carbodiimide resins include "CARBODILITE V-02B", "CARBODILITE V-03", "CARBODILITE V-04K", "CARBODILITE V-07" and "CARBODILITE V-09" manufactured by Nisshinbo Chemical Co., Ltd.; and "Stabaxol P", "Stabaxol P400" and "Hycasyl 510" manufactured by Rhein-Chemie.

[0152] As the acid anhydride resin, a curing agent having one or more acid anhydride groups in one molecule can be used, preferably a resin having two or more acid anhydride groups in one molecule. Specific examples of the acid anhydride resin include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, Acid anhydrides of polymer type such as benzophenonetetracarboxylic acid dianhydride, biphenyltetracarboxylic acid dianhydride, naphthalenetetracarboxylic acid dianhydride, oxydiphthalic acid dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic acid dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(trimellitic anhydride ester), styrene-maleic acid resin obtained by copolymerization of styrene and maleic acid, etc. Examples of commercially available acid anhydride resins include "HNA-100", "MH-700", "MTA-15", "DDSA", and "OSA" manufactured by Shin Nippon Rika Co., Ltd.; "YH-306" and "YH-307" manufactured by Mitsubishi Chemical Corporation; and "HN-2200" and "HN-5500" manufactured by Hitachi Chemical Co., Ltd.

[0153] As the amine resin, a resin having one or more, preferably two or more, amino groups in one molecule can be used. Examples of the amine resin include aliphatic amines, polyether amines, alicyclic amines, aromatic amines, and the like, among which aromatic amines are preferred. The amine resin is preferably a primary amine or a secondary amine, and more preferably a primary amine. Specific examples of the amine resin include 4,4'-methylenebis(2,6-dimethylaniline), 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, metaphenylenediamine, metaphenylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino-4-hydroxy phenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, etc. Amine resins that can be used are commercially available products, for example, "SEIKACURE-S" manufactured by SEIKA Corporation; "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARDA-A", "KAYAHARD AB", and "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd.; and "EPICURE W" manufactured by Mitsubishi Chemical Corporation.

[0154] As benzo Specific examples of the oxazine-based resin include "JBZ-OP100D" and "ODA-BOZ" manufactured by JFE Chemical Co., Ltd.; "HFB2006M" manufactured by Showa Highpolymer Co., Ltd.; and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.

[0155] As active ester resin, resins having more than one, preferably more than two active ester groups in one molecule can be used. Among them, as active ester resin, resins having more than two highly reactive ester groups in one molecule, such as phenolic esters, thiophenolic esters, N-hydroxylamine esters, and esters of heterocyclic hydroxy compounds, are preferred. The active ester resin is preferably obtained by the condensation reaction of a carboxylic acid compound and / or a thiocarboxylic acid compound with a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, active ester resins obtained from carboxylic acid compounds and hydroxy compounds are preferred, and active ester resins obtained from carboxylic acid compounds and phenolic compounds and / or naphthol compounds are more preferred. As carboxylic acid compounds, for example, benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, pyromellitic acid, etc. can be cited. Examples of the phenol compound or naphthol compound include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalein, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucinol, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the "dicyclopentadiene-type diphenol compound" refers to a diphenol compound obtained by condensing two molecules of phenol with one molecule of dicyclopentadiene.

[0156] Specifically, as the active ester resin, preferred are dicyclopentadiene type active ester resins, naphthalene type active ester resins containing a naphthalene structure, active ester resins containing acetylated products of phenol novolac, and active ester resins containing benzoylated products of phenol novolac. As the dicyclopentadiene type active ester resin, preferred are active ester resins containing a dicyclopentadiene type diphenol structure. Commercially available active ester resins include, for example, "EXB9451", "EXB9460", "EXB9460S", "EXB-8000L", "EXB-8000L-65M", "EXB-8000L-65TM", "HPC-8000L-65TM", "HPC-8000", "HPC-8000-65T", "HPC-8000H", and "HPC-8000H-65TM" (manufactured by DIC Corporation) as active ester resins containing a dicyclopentadiene-type diphenol structure; and "HP-B-8151-62T", "HP-C-8151-62T", "EXB-8100L-65T", and "EXB-815 As for the active ester resin containing phosphorus, "EXB9401" (manufactured by DIC Corporation) can be cited; as for the active ester resin which is an acetylated product of phenol novolac, "DC808" (manufactured by Mitsubishi Chemical Corporation) can be cited; as for the active ester resin which is a benzoylated product of phenol novolac, "YLH1026", "YLH1030" and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) can be cited; as for the active ester resin which is a benzoylated product of phenol novolac, "PC1300-02-65MA" (manufactured by AIR WATER Corporation) and the like can be cited.

[0157] Examples of the cyanate resin include difunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenylcyanate), 4,4'-ethylenediphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanatephenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanatephenyl-1-(methylethylene))benzene, bis(4-cyanatephenyl)sulfide, and bis(4-cyanatephenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers obtained by partially triazinizing these cyanate resins. Specific examples of cyanate ester resins include "PT30" and "PT60" manufactured by Lonza Japan (both are phenol novolac-type multifunctional cyanate resins), "BA230" and "BA230S75" (prepolymers in which a part or all of bisphenol A dicyanate is triazine-formulated to become trimers), etc.

[0158] Examples of the thiol resin include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), and tris(3-mercaptopropyl)isocyanurate.

[0159] The reactive group equivalent of the epoxy curing agent is preferably 50 g / eq. to 3000 g / eq., more preferably 100 g / eq. to 1000 g / eq., further preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The reactive group equivalent indicates the mass of the epoxy curing agent per 1 equivalent of reactive groups.

[0160] The amount of the epoxy curing agent relative to 100% by mass of the non-volatile components in the resin composition is preferably 40% by mass or less, more preferably 30% by mass or less, further preferably 20% by mass or less, and particularly preferably 10% by mass or less. The lower limit may be, for example, 0% by mass or more, 0.01% by mass or more, 0.1% by mass or more, etc.

[0161] The amount (volume %) of the thermosetting resin (D) relative to 100% by volume of the non-volatile components in the resin composition is preferably 2.5% by volume or more, more preferably 4.0% by volume or more, particularly preferably 4.5% by volume or more, and preferably 10.0% by volume or less, more preferably 9.0% by volume or less, particularly preferably 8.0% by volume or less. When the amount (volume %) of the thermosetting resin (D) is within the above range, both the relative permeability and the magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0162] The amount (mass %) of the thermosetting resin (D) relative to 100 mass % of the non-volatile components in the resin composition is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, particularly preferably 1.0 mass % or more, preferably 20 mass % or less, more preferably 15 mass % or less, and further preferably 10 mass % or less. When the amount (mass %) of the thermosetting resin (D) is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0163] Relative to 100% by mass of the resin component in the resin composition, the amount of (D) thermosetting resin is preferably in the range of 50% by mass or more, more preferably 60% by mass or more, particularly preferably 70% by mass or more, and preferably 100% by mass or less, more preferably 95% by mass or less, particularly preferably 90% by mass or less. When the amount of (D) thermosetting resin is in the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better. The resin component of the resin composition refers to the components other than inorganic fillers such as magnetic powder in the non-volatile components of the resin composition.

[0164] <(E) Curing Accelerator According to the First Embodiment>

[0165] The resin composition involved in the first embodiment of the present invention may further include (E) a curing accelerator as an optional component. The (E) curing accelerator as the (E) component does not include substances equivalent to the above-mentioned (A) to (D) components. Since the (E) curing accelerator has the function of being a catalyst for the reaction of the (D) thermosetting resin, it can promote the curing of the resin composition. For example, when the (D) thermosetting resin includes an epoxy resin, the (E) curing accelerator preferably has the function of promoting the curing of the epoxy resin.

[0166] Examples of the curing accelerator (E) include imidazole-based curing accelerators, phosphorus-based curing accelerators, urea-based curing accelerators, guanidine-based curing accelerators, metal-based curing accelerators, and amine-based curing accelerators. Among them, the curing accelerator (E) preferably includes an imidazole-based curing accelerator. The curing accelerator (E) may be used alone or in combination of two or more.

[0167] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazole trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1' imidazole compounds such as 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, 2-phenylimidazoline, and adducts of imidazole compounds with epoxy resins. As the imidazole-based curing accelerator, a commercially available product may be used, and examples thereof include "1B2PZ", "2MZA-PW", and "2PHZ-PW" manufactured by Shikoku Chemical Industries, Ltd. and "P200-H50" manufactured by Mitsubishi Chemical Corporation.

[0168] Examples of phosphorus-based curing accelerators include tetrabutylphosphonium bromide, tetrabutylphosphonium chloride, tetrabutylphosphonium acetate, tetrabutylphosphonium decanoate, tetrabutylphosphonium laurate, bis(tetrabutylphosphonium)pyromellitic acid salt, tetrabutylphosphonium hexahydrophthalate, and tetrabutylphosphonium bis(tetrabutylphosphonium) pyromellitic acid salt. aliphatic phosphonium salts such as phosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate and di-tert-butylmethylphosphonium tetraphenylborate; methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, propyltriphenylphosphonium bromide, Aromatic phosphonium salts such as butyltriphenylphosphonium, benzyltriphenylphosphonium chloride, tetraphenylphosphonium bromide, p-tolyltriphenylphosphonium tetra-p-tolylborate, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone addition products such as triphenylphosphine-p-benzoquinone addition products reactants; aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine; dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tri(4-ethylphenyl)phosphine, tri(4-propylphenyl)phosphine, tri(4-isopropylphenyl)phosphine, tri(4-butylphenyl)phosphine, tri(4-tert-butylphenyl)phosphine, tri(2,4-dimethylphenyl)phosphine, tri(2,5-dimethylphenyl)phosphine phenyl)phosphine, tri(2,6-dimethylphenyl)phosphine, tri(3,5-dimethylphenyl)phosphine, tri(2,4,6-trimethylphenyl)phosphine, tri(2,6-dimethyl-4-ethoxyphenyl)phosphine, tri(2-methoxyphenyl)phosphine, tri(4-methoxyphenyl)phosphine, tri(4-ethoxyphenyl)phosphine, tri(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, 2,2'-bis(diphenylphosphino)diphenyl ether and the like.

[0169] Examples of the urea curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, 3-(3,4-dimethylphenyl)-1, Aromatic dimethyl urea such as 1-dimethyl urea, 3-(4-isopropylphenyl)-1,1-dimethyl urea, 3-(4-methoxyphenyl)-1,1-dimethyl urea, 3-(4-nitrophenyl)-1,1-dimethyl urea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethyl urea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethyl urea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethyl urea, N,N-(1,4-phenylene)bis(N',N'-dimethyl urea), N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethyl urea)[toluene bis(dimethyl urea)].

[0170] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanidine, 1-ethylbiguanidine, 1-n-butylbiguanidine, 1-n-octadecylbiguanidine, 1,1-dimethylbiguanidine, 1,1-diethylbiguanidine, 1-cyclohexylbiguanidine, 1-allylbiguanidine, 1-phenylbiguanidine, and 1-(o-tolyl)biguanidine.

[0171] As metal curing accelerators, for example, organic metal complexes or organic metal salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin can be cited. Specific examples of organic metal complexes include organic cobalt complexes such as cobalt acetylacetonate (II) and cobalt acetylacetonate (III), organic copper complexes such as copper acetylacetonate (II), organic zinc complexes such as zinc acetylacetonate (II), organic iron complexes such as iron acetylacetonate (III), organic nickel complexes such as nickel acetylacetonate (II), and organic manganese complexes such as manganese acetylacetonate (II). As organic metal salts, for example, zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, zinc stearate, and the like can be cited.

[0172] Examples of the amine-based curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene. A commercially available amine-based curing accelerator may be used, and examples thereof include "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd.

[0173] The amount (volume %) of the curing accelerator (E) relative to 100 volume % of the non-volatile components in the resin composition can range from 0 volume % to more than 0 volume %, and is preferably 0.1 volume % or more, more preferably 0.2 volume % or more, and particularly preferably 0.3 volume % or more, and is preferably 2.0 volume % or less, more preferably 1.0 volume % or less, and particularly preferably 0.7 volume % or less.

[0174] The amount (mass %) of the curing accelerator (E) relative to 100 mass % of the non-volatile components in the resin composition can preferably range from 0 mass % to more than 0 mass %, preferably from 0.01 mass % or more, more preferably from 0.05 mass % or more, particularly preferably from 0.1 mass % or more, preferably from 5 mass % or less, more preferably from 3 mass % or less, particularly preferably from 1 mass % or less.

[0175] The amount (mass %) of the curing accelerator (E) relative to 100 mass % of the resin component in the resin composition can preferably range from 0 mass % to more than 0 mass %, preferably from 0.1 mass % or more, more preferably from 1 mass % or more, particularly preferably from 3 mass % or more, preferably from 20 mass % or less, more preferably from 15 mass % or less, particularly preferably from 10 mass % or less.

[0176] <(F) Dispersant According to the First Embodiment>

[0177] The resin composition involved in the first embodiment of the present invention may further include (F) a dispersant as an optional component. The (F) dispersant as the (F) component does not include substances corresponding to the above-mentioned (A) to (E) components. The (F) dispersant can improve the dispersibility of magnetic powders such as (A) nanocrystalline magnetic powder, (B) small particle size magnetic powder, and (C) intermediate magnetic powder.

[0178] There is no limitation on the type of (F) dispersant. For example, as the (F) dispersant, there can be used a dispersant that contains a functional group capable of adsorbing magnetic powder and disperses the magnetic powder by mutual repulsion (e.g., electrostatic repulsion, steric repulsion, etc.) of the (F) dispersants when adsorbed to the magnetic powder. Examples of such (F) dispersants include acidic dispersants and alkaline dispersants.

[0179] Acidic dispersants usually contain acidic functional groups such as carboxyl, sulfonic (-SO3H), sulfate (-OSO3H), phosphonyl (-PO(OH)2), phosphonyloxy (-OPO(OH)2), hydroxyphosphoryl (-PO(OH)-), and sulfanyl (-SH). Acidic functional groups usually have dissociated protons and can be neutralized by bases such as amines and hydroxide ions. Preferred acidic dispersants include, for example, acidic polymer dispersants containing polymer chains such as polyoxyalkylene chains and polyether chains. Preferred examples of the acidic dispersant include: "C-2093I" and "SC-1015F (a multifunctional comb-type functional polymer having an ionic group in the main chain and a polyoxyalkylene chain in the graft chain)" manufactured by NOF Corporation; "ED152", "ED153", "ED154", "ED118", "ED174", "ED251", and "DA-375" (polyether-type phosphate-based dispersants) manufactured by Kusumoto Chemicals Co., Ltd.; "RS-410", "RS-610", and "RS-710" (pH 1.9) of the "PHOSPHANOL" series manufactured by Toho Chemical Industry Co., Ltd. (phosphate-based dispersants); "AKM-0531", "AFB-1521", "SC-0505K", and "SC-0708A" of the "Malialim" series manufactured by NOF Corporation.

[0180] Alkaline dispersants usually contain the following basic functional groups: primary, secondary and tertiary amino groups; ammonium groups; imino groups; and nitrogen-containing heterocyclic groups such as pyridine, pyrimidine, pyrazine, imidazole, triazole, etc. The basic functional groups can be neutralized by acids such as organic acids and inorganic acids. As preferred alkaline dispersants, for example, alkaline polymer dispersants containing polymer chains such as polyester chains can be mentioned. As preferred examples of alkaline dispersants, "PB-881" (dispersant containing polyester chains) manufactured by Ajinomoto Fine-techno Co., Ltd. can be mentioned.

[0181] (F) The dispersant may be used alone or in combination of two or more.

[0182] The amount (volume %) of the dispersant (F) relative to 100 volume % of the non-volatile components in the resin composition may range from 0 volume % to more than 0 volume %, and is preferably 0.3 volume % or more, more preferably 0.6 volume % or more, and particularly preferably 1.2 volume % or more, and is preferably 6 volume % or less, more preferably 4 volume % or less, and particularly preferably 3 volume % or less.

[0183] The amount (mass %) of the dispersant (F) relative to 100 mass % of the non-volatile components in the resin composition is preferably in the range of 0 mass % or greater than 0 mass %, preferably 0.01 mass % or greater, more preferably 0.05 mass % or greater, particularly preferably 0.1 mass % or greater, and preferably 5 mass % or less, more preferably 3 mass % or less, particularly preferably 1 mass % or less.

[0184] The amount (mass %) of the dispersant (F) relative to 100 mass % of the resin component in the resin composition may preferably be in the range of 0 mass % or greater than 0 mass %, preferably 0.1 mass % or greater, more preferably 1 mass % or greater, particularly preferably 5 mass % or greater, and preferably 30 mass % or less, more preferably 25 mass % or less, particularly preferably 20 mass % or less.

[0185] <(G) Optional Additives According to the First Embodiment>

[0186] The resin composition involved in the first embodiment of the present invention may be combined with the above-mentioned components and further include (G) optional additives. Examples of the optional additives (G) include: free radical polymerization initiators such as peroxide-based free radical polymerization initiators and azo-based free radical polymerization initiators; organic fillers such as rubber particles; organic metal compounds such as organic copper compounds and organic zinc compounds; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; thickeners such as Benton and montmorillonite; defoamers such as silicone-based defoamers, acrylic defoamers, fluorine-based defoamers, and vinyl resin-based defoamers; ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers; adhesion enhancers such as urea silane; and triazole-based adhesion imparting agents , tetrazole-based adhesion-imparting agents, triazine-based adhesion-imparting agents and other adhesion-imparting agents; antioxidants such as hindered phenol-based antioxidants and hindered amine-based antioxidants; fluorescent whitening agents such as stilbene derivatives; surfactants such as fluorine-based surfactants and silicone-based surfactants; flame retardants such as phosphorus-based flame retardants (such as phosphate compounds, phosphazene compounds, phosphinic acid compounds, and red phosphorus), nitrogen-based flame retardants (such as melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (such as antimony trioxide); stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers, etc. (G) The optional additives may be used alone or in combination of two or more.

[0187] <(H) Solvent According to the First Embodiment>

[0188] The resin composition according to the first embodiment of the present invention may further contain an optional (H) solvent as a volatile component in addition to the non-volatile components such as the above-mentioned (A) to (G) components.

[0189] As the (H) solvent, an organic solvent is generally used. As the organic solvent, a solvent that can dissolve the resin component contained in the non-volatile component is preferred. Examples of the organic solvent include: ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; tetrahydropyran, tetrahydrofuran, 1,4-dihydropyran, and 1,4-dihydrofuran. Ether solvents such as alkane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether; alcohol solvents such as methanol, ethanol, propanol, butanol, ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, carbitol acetate (ethyl diglycolacetate), γ-butyrolactone, methoxypropionic acid methyl ester and the like; ester alcohol solvents such as methyl lactate, ethyl lactate, 2-hydroxyisobutyrate and the like; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, diethylene glycol monobutyl ether (butyl carbitol) and the like; amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and the like; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile, propionitrile and the like; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, methylcyclohexane and the like; aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, trimethylbenzene and the like. In addition, the (H) solvent may be used alone or in combination of two or more in any ratio.

[0190] In the case of a resin composition made into a paste, the range of the amount of (H) solvent is preferably less. For example, relative to the non-volatile components in the resin composition of 100% by mass, the amount of (H) solvent can be less than 5.5% by mass, less than 4% by mass, less than 3% by mass, less than 2% by mass or less than 1% by mass. Wherein, it is preferred that the resin composition does not contain (H) solvent. That is, the amount of (H) solvent is preferably 0% by mass. In the case where the content of (H) solvent in the resin composition is few and in the case where (H) solvent is not present, the generation of the void caused by the volatilization of (H) solvent can be suppressed, and then the handling property and operability can also be excellent.

[0191] <Characteristics of the resin composition according to the first embodiment>

[0192] The resin composition involved in the first embodiment of the present invention can be cured by heat. Therefore, by thermally curing the resin composition, a cured product of the resin composition can be obtained. Generally, among the components contained in the resin composition, volatile components such as (H) solvents can be volatilized by heat during thermal curing, but non-volatile components such as (A) to (G) components will not volatilize due to heat during thermal curing. Therefore, the cured product of the resin composition may include the non-volatile components of the resin composition or their reaction products.

[0193] According to the resin composition involved in the first embodiment of the present invention, a cured product with improved relative magnetic permeability and magnetic loss can be obtained. Specifically, the cured product of the resin composition can have high relative magnetic permeability and low magnetic loss in a low frequency band (eg, 10 MHz).

[0194] In one example, when the relative magnetic permeability of the cured product of the resin composition is measured under the conditions of a measurement frequency of 10 MHz and a room temperature of 23° C., the relative magnetic permeability is preferably in the range of 25 or more, more preferably in the range of 30 or more, and particularly preferably in the range of 35 or more. There is no particular limitation on the upper limit, and for example, it may be 80 or less, 75 or less, 70 or less, etc. The relative magnetic permeability of the cured product of the resin composition can be measured by the method described in <Test Example 2: Measurement and Evaluation of Relative Magnetic Permeability> of the Examples described later.

[0195] In one example, when the loss coefficient (tan δ) of a cured product of a resin composition is measured at a measurement frequency of 10 MHz and a room temperature of 23°C, the range of the loss coefficient is preferably 0.13 or more, more preferably 0.10 or less, and particularly preferably 0.07 or less. The lower limit may be, for example, 0.000 or more, 0.001 or more, etc. Generally, the smaller the loss coefficient (tan δ), the lower the magnetic loss. The loss coefficient (tan δ) of the cured product of the resin composition can be measured by the method described in <Test Example 3: Measurement and Evaluation of Loss Coefficient (tan δ)> of the embodiments described later.

[0196] The resin combination involved in the first embodiment of the present invention can have excellent coating properties. Specifically, even when the amount of solvent is small, the resin combination can also have high fluidity, so it can be smoothly coated. Therefore, the resin combination can preferably reduce the content of the solvent, and can more preferably be solvent-free. Therefore, the formation of the gap caused by the solvent can be suppressed, so a cured product with excellent mechanical strength and uniformity can be obtained generally.

[0197] There is no particular restriction on the properties of the resin composition, and preferably the resin composition has a fluid paste state. For example, the resin composition can be made into a paste-like resin composition using a solvent. In addition, for example, the resin composition can be made into a solvent-free paste-like resin composition by using a liquid thermosetting resin such as a liquid epoxy resin. In the case where the solvent content in the resin composition is small and the resin composition is solvent-free, the generation of voids caused by the volatilization of the solvent can be suppressed, and then the handling property and operability can also be excellent.

[0198] By effectively utilizing the above-mentioned excellent properties, the resin composition is preferably used as a resin composition for manufacturing an inductor. For example, the above-mentioned resin composition is preferably used as a resin composition for filling holes in a substrate provided with a circuit substrate. In addition, for example, the above-mentioned resin composition is also preferably used to form a cured product layer on a circuit substrate. In order to facilitate application in these uses, the resin composition can be used in the form of a paste or in the form of a resin sheet containing a layer of the resin composition.

[0199] <Method for producing resin composition according to first embodiment>

[0200] The resin composition involved in the first embodiment of the present invention can be manufactured by, for example, a manufacturing method comprising mixing the above-mentioned components. A part or all of the above-mentioned components can be mixed simultaneously, or they can be mixed in sequence. In the process of mixing the components, the temperature can be appropriately adjusted, and therefore, heating and / or cooling can be performed temporarily or all the time. In addition, in the process of mixing the components, stirring or vibration can be performed. Moreover, degassing can be performed under low pressure conditions such as vacuum. The resin composition involved in the first embodiment of the present invention can be manufactured by the manufacturing method of the resin composition involved in the second embodiment described later.

[0201] <Overview of the method for producing a resin composition according to the second embodiment>

[0202] The method for producing a resin composition according to the second embodiment of the present invention includes mixing the following components:

[0203] (a) nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less;

[0204] (b) magnetic powder having an average particle size of 2 μm or less; and

[0205] (D) Thermosetting resin.

[0206] In the following description, "(a) nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less" is sometimes referred to as "(a) nanocrystalline magnetic raw material powder". In addition, "(b) magnetic powder having an average particle size of 2 μm or less" is sometimes referred to as "(b) small particle size magnetic raw material powder".

[0207] The resin composition manufactured by the manufacturing method involved in the second embodiment of the present invention can exert the same effect as the resin composition involved in the first embodiment. Therefore, the resin composition manufactured by the manufacturing method involved in the second embodiment of the present invention can be cured by thermally curing (D) thermosetting resin to provide a cured product. The cured product thus obtained can have high relative permeability and low magnetic loss in a low frequency band (e.g., 10MHz). In addition, the resin composition can generally have excellent coating properties.

[0208] From the range of the average particle size, it can be seen that the (A) nanocrystalline magnetic raw material powder described in the first embodiment may be included in the (a) nanocrystalline magnetic raw material powder, and the (B) small-particle-size magnetic raw material powder described in the first embodiment may be included in the (B) small-particle-size magnetic raw material powder. Therefore, the inventors speculate that the mechanism for obtaining the effect involved in this embodiment includes the combined effect of the (A) nanocrystalline magnetic powder and the (B) small-particle-size magnetic powder described in the first embodiment. However, the technical scope of the present invention is not limited to the mechanism described here.

[0209] <(a) Nanocrystalline Magnetic Raw Material Powder According to Second Embodiment>

[0210] The manufacturing method involved in the second embodiment of the present invention includes mixing (a) nanocrystalline magnetic raw material powder as (a) component with (b) small particle size magnetic raw material powder and (D) thermosetting resin. (a) Nanocrystalline magnetic raw material powder is nanocrystalline magnetic powder having an average particle size within a specific range. The range of nanocrystalline magnetic powder is as described in the first embodiment.

[0211] (a) The nanocrystalline magnetic raw material powder is usually provided for mixing in the form of particles. (a) The nanocrystalline magnetic raw material powder may contain crystal grains in at least a portion of the particles, preferably contain crystal grains in the surface layer of the particles, more preferably contain crystal grains in the entire particle, and particularly preferably consist only of crystal grains.

[0212] (a) The nanocrystalline magnetic raw material powder has an average particle size D in the range of 5.5 μm or more and 20 μm or less. 50 More specifically, (a) the average particle size D of the nanocrystalline magnetic raw material powder 50 The average particle size D is usually 5.5 μm or more, preferably 5.7 μm or more, more preferably 5.9 μm or more, and is usually 20 μm or less, preferably 18 μm or less, more preferably 16 μm or less. 50 A manufacturing method of mixing (a) nanocrystalline magnetic raw material powder, (b) small-particle-size magnetic raw material powder and (D) thermosetting resin can improve both relative magnetic permeability and magnetic loss in a low-frequency band and can manufacture a resin composition with excellent coating properties.

[0213] (a) Average particle size D of nanocrystalline magnetic raw material powder 50 The median particle size is based on volume. (a) The average particle size D of the nanocrystalline magnetic raw material powder 50 The particle size distribution of the nanocrystalline magnetic raw material powder can be measured by a laser diffraction / scattering method based on Mie scattering theory. Specifically, a laser diffraction / scattering particle size distribution measuring device can be used to prepare (a) a particle size distribution of the nanocrystalline magnetic raw material powder on a volume basis, and the median particle size is taken as the average particle size D 50 The measurement is performed. The measurement sample can preferably be a sample obtained by dispersing magnetic powder in water using ultrasound. As a laser diffraction scattering particle size distribution measuring device, "MT3000II" manufactured by MicrotracBEL; "LA-960" manufactured by Horiba; "SALD-2200" manufactured by Shimadzu Corporation, etc. can be used.

[0214] Generally, the volume-based particle size distribution of the (a) nanocrystalline magnetic raw material powder follows a normal distribution. Therefore, the (a) nanocrystalline magnetic raw material powder may have an average particle size D smaller than that of the (a) nanocrystalline magnetic raw material powder. 50 10% particle size D 10 and greater than the average particle size D of the (a) nanocrystalline magnetic raw material powder 50 90% particle size D 90 Here, 10% particle size D 10 It refers to the particle size when the cumulative volume accumulated from the smaller particle size side is 10% in the volume-based particle size distribution. 90 It refers to the particle size when the cumulative volume accumulated from the smaller particle size side is 90% in the volume-based particle size distribution. (a) 10% particle size D of nanocrystalline magnetic raw material powder 10 and 90% particle size D 90 The particle size distribution can be measured based on the volumetric particle size distribution measured by the above-mentioned laser diffraction / scattering method.

[0215] (a) 10% particle size D of nanocrystalline magnetic raw material powder 10 The average particle size D is preferably larger than 2.0 μm, more preferably 2.4 μm or larger, and particularly preferably 2.8 μm or larger. 50 For example, it may be 10 μm or less, 8 μm or less, 6 μm or less, etc. In (a) the 10% particle size D of the nanocrystalline magnetic raw material powder 10 When the content is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in a low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0216] (a) 90% particle size D of nanocrystalline magnetic raw material powder 90The average particle size D is preferably 60 μm or less, more preferably 50 μm or less, and particularly preferably 40 μm or less. 50 For example, it may be 6 μm or more, 8 μm or more, 10 μm or more, etc. In (a) the 90% particle size D of the nanocrystalline magnetic raw material powder 90 When the content is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in a low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0217] (a) 10% particle size D of nanocrystalline magnetic raw material powder 10 With 90% particle size D 90 Difference D 90 -D 10 It is preferably 1 μm or more, more preferably 3 μm or more, and particularly preferably 5 μm or more, and is preferably 40 μm or less, more preferably 35 μm or less, and particularly preferably 30 μm or less. 90 -D 10 When the content is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in a low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0218] (a) 10% particle size D of nanocrystalline magnetic raw material powder 10 With 90% particle size D 90 Ratio D 90 / D 10 It is preferably 1.1 or more, more preferably 2 or more, and particularly preferably 3 or more, and is preferably 10 or less, more preferably 8 or less, and particularly preferably 6 or less. 90 / D 10 When the content is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in a low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0219] The (a) nanocrystalline magnetic raw material powder may be particles of a magnetic material having a relative magnetic permeability greater than 1. As the magnetic material contained in the (a) nanocrystalline magnetic raw material powder, the magnetic material described as the magnetic material of the (A) nanocrystalline magnetic powder is preferably used.

[0220] The (a) nanocrystalline magnetic raw material powder preferably contains the above-mentioned magnetic material, and preferably contains only the above-mentioned magnetic material. The (a) nanocrystalline magnetic raw material powder may be used alone or in combination of two or more.

[0221] (a) Nanocrystalline magnetic raw material powder can be produced, for example, by an atomization method. As a specific example of the method for producing (a) nanocrystalline magnetic raw material powder, there can be cited: the method described in Japanese Patent Gazette No. 2021-141267 and Japanese Patent Gazette No. 2021-158343. In addition, commercially available (a) nanocrystalline magnetic raw material powder can be used. As commercially available magnetic powders containing (a) nanocrystalline magnetic raw material powder, for example: "KUAMET NC1-38um", "ATFINE-NC1PF10FA" manufactured by Epson Atmix, etc. can be cited. When obtaining (a) nanocrystalline magnetic raw material powder from the market, the commercially available magnetic powder can be classified and used as needed. For example, it can be classified into a powder having an average particle size D not within the above range. 50 The commercially available magnetic powder is classified and the average particle size D is appropriately adjusted. 50 The value to use.

[0222] The (a) nanocrystalline magnetic raw material powder is preferably spherical. The aspect ratio of the particles of the (a) nanocrystalline magnetic raw material powder may be in the same range as the aspect ratio of the (A) nanocrystalline magnetic powder.

[0223] The amount (volume %) of the (a) nanocrystalline magnetic raw material powder used in the manufacturing method according to the second embodiment of the present invention is preferably 30% by volume or more, more preferably 40% by volume or more, particularly preferably 50% by volume or more, preferably 80% by volume or less, more preferably 75% by volume or less, and particularly preferably 70% by volume or less, relative to 100% by volume of the non-volatile components of the manufactured resin composition. When the amount (volume %) of the (a) nanocrystalline magnetic raw material powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition having particularly excellent coating properties can be manufactured.

[0224] Relative to 100% by volume of the non-volatile components of the resin composition, the amount (volume %) of (a) nanocrystalline magnetic raw material powder is represented by "V(a)", and the amount (volume %) of (b) small-particle-size magnetic raw material powder is represented by "V(b)". In this case, the volume ratio of (a) nanocrystalline magnetic raw material powder to (b) small-particle-size magnetic raw material powder ((a) nanocrystalline magnetic raw material powder / (b) small-particle-size magnetic raw material powder) can be represented by "V(a) / V(b)". The volume ratio V(a) / V(b) is preferably 1.0 or more, more preferably 1.5 or more, further preferably 2.0 or more, and particularly preferably 2.5 or more, and is preferably 20 or less, more preferably 16 or less, further preferably 12 or less, and particularly preferably 8 or less. When the volume ratio V(a) / V(b) is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0225] In addition, the total amount (volume %) of (a) nanocrystalline magnetic raw material powder and (b) small-particle magnetic raw material powder relative to 100% by volume of the non-volatile components of the resin composition can be expressed as "V(a) + V(b)". The total amount (volume %) V(a) + V(b) is preferably 40% by volume or more, more preferably 50% by volume or more, particularly preferably 60% by volume or more, preferably 90% by volume or less, more preferably 86% by volume or less, particularly preferably 82% by volume or less. When the total amount (volume %) V(a) + V(b) of (a) nanocrystalline magnetic raw material powder and (b) small-particle magnetic raw material powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition with particularly excellent coating properties can be manufactured.

[0226] The total amount (volume %) of all magnetic powders mixed for manufacturing the resin composition relative to 100 volume % of the non-volatile components of the resin composition is preferably 40 volume % or more, more preferably 50 volume % or more, particularly preferably 60 volume % or more, preferably 95 volume % or less, more preferably 90 volume % or less, particularly preferably 85 volume % or less. When the total amount (volume %) of the magnetic powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition with particularly excellent coating properties can be manufactured.

[0227] The total amount (volume %) of (a) nanocrystalline magnetic raw material powder and (b) small-particle-size magnetic raw material powder relative to the total amount of all magnetic powders mixed for manufacturing the resin composition of 100 volume %, is preferably 80 volume % or more, more preferably 85 volume % or more, particularly preferably 90 volume % or more, for example, it can be 100 volume % or less, 98 volume % or less, 95 volume % or less, etc. When the total amount (volume %) of (a) nanocrystalline magnetic raw material powder and (b) small-particle-size magnetic raw material powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition with particularly excellent coating properties can be manufactured.

[0228] The amount (mass %) of the (a) nanocrystalline magnetic raw material powder used in the manufacturing method according to the second embodiment of the present invention is preferably 50% by mass or more, more preferably 60% by mass or more, particularly preferably 70% by mass or more, preferably 90% by mass or less, more preferably 86% by mass or less, and particularly preferably 82% by mass or less, relative to 100% by mass of the non-volatile components of the manufactured resin composition. When the amount (mass %) of the (a) nanocrystalline magnetic raw material powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition having particularly excellent coating properties can be manufactured.

[0229] Relative to 100% by mass of the non-volatile components of the resin composition, the amount (mass %) of (a) nanocrystalline magnetic raw material powder is represented by "M(a)", and the amount (mass %) of (b) small-particle-size magnetic raw material powder is represented by "M(b)". In this case, the mass ratio of (a) nanocrystalline magnetic raw material powder to (b) small-particle-size magnetic raw material powder ((a) nanocrystalline magnetic raw material powder / (b) small-particle-size magnetic raw material powder) can be represented by "M(a) / M(b)". The mass ratio M(a) / M(b) is preferably greater than 1, more preferably greater than 2, and further preferably greater than 3, and is preferably less than 20, more preferably less than 15, and further preferably less than 10. When the mass ratio M(a) / M(b) is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low-frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0230] In addition, the total amount (mass %) of (a) nanocrystalline magnetic raw material powder and (b) small-particle magnetic raw material powder relative to 100 mass % of the non-volatile components of the resin composition can be expressed as "M(a) + M(b)". The total amount (mass %) M(a) + M(b) is preferably 60 mass % or more, more preferably 70 mass % or more, particularly preferably 80 mass % or more, preferably 98 mass % or less, more preferably 97 mass % or less, particularly preferably 96 mass % or less. When the total amount (mass %) M(a) + M(b) of (a) nanocrystalline magnetic raw material powder and (b) small-particle magnetic raw material powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition with particularly excellent coating properties can be manufactured.

[0231] The total amount (mass %) of all magnetic powders mixed for manufacturing the resin composition relative to 100 mass % of the non-volatile components of the resin composition is preferably 80 mass % or more, more preferably 85 mass % or more, particularly preferably 90 mass % or more, preferably 99 mass % or less, more preferably 98 mass % or less, particularly preferably 97 mass % or less. When the total amount (mass %) of the magnetic powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition with particularly excellent coating properties can be manufactured.

[0232] The total amount (mass %) of (a) nanocrystalline magnetic raw material powder and (b) small-particle-size magnetic raw material powder relative to the total amount of all magnetic powders mixed for manufacturing the resin composition of 100 mass % is preferably 80 mass % or more, more preferably 85 mass % or more, particularly preferably 89.8 mass % or more, for example, it can be 100 mass % or less, 98 mass % or less, 95 mass % or less, etc. When the total amount (mass %) of (a) nanocrystalline magnetic raw material powder and (b) small-particle-size magnetic raw material powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition with particularly excellent coating properties can be manufactured.

[0233] <(b) Small-diameter magnetic raw material powder according to the second embodiment>

[0234] The resin composition according to the second embodiment of the present invention comprises (b) a small-particle magnetic raw material powder as the component (b) mixed with (a) a nanocrystalline magnetic raw material powder and (D) a thermosetting resin. The (b) small-particle magnetic raw material powder is usually mixed in a particle state.

[0235] (b) The small-particle magnetic raw material powder has an average particle size D of 2 μm or less. 50 Specifically, (b) the average particle size D of the small-particle magnetic raw material powder 50 It is usually 2 μm or less, preferably 1.5 μm or less, and more preferably 1 μm or less. The lower limit may be, for example, 0.01 μm or more, 0.1 μm or more, etc. By including the average particle size D in such a range 50 The method for producing a resin composition comprising mixing (b) a small-particle-size magnetic raw material powder with (a) a nanocrystalline magnetic raw material powder and (D) a thermosetting resin can improve both relative magnetic permeability and magnetic loss in a low-frequency band and can produce a resin composition having excellent coating properties. 50 The median particle size based on volume can be expressed by comparing (a) the average particle size D of the nanocrystalline magnetic raw material powder with 50 The same method was used to determine.

[0236] Generally, the volume-based particle size distribution of the (b) small-particle-size magnetic raw material powder follows a normal distribution. Therefore, the (b) small-particle-size magnetic raw material powder may have an average particle size D smaller than that of the (b) small-particle-size magnetic raw material powder. 50 10% particle size D 10 and an average particle size D greater than that of the (b) small particle size magnetic raw material powder 50 90% particle size D 90 (b) 10% particle size D of small particle size magnetic raw material powder 10 and 90% particle size D 90 (a) The 10% particle size D of the nanocrystalline magnetic raw material powder can be 10and 90% particle size D 90 The same method was used to determine.

[0237] (b) 10% particle size D of small particle size magnetic raw material powder 10 The average particle size D is preferably 0.01 μm or more, more preferably 0.02 μm or more, and particularly preferably 0.03 μm or more. 50 For example, it may be 1 μm or less, 0.7 μm or less, 0.5 μm or less, etc. In (b) the 10% particle size D of the small particle size magnetic raw material powder 10 When the content is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in a low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0238] (b) 90% particle size D of small particle size magnetic raw material powder 90 The average particle size D is preferably less than 5.5 μm, more preferably 4 μm or less, and particularly preferably 2 μm or less. 50 For example, it may be 0.5 μm or more, 0.8 μm or more, 1 μm or more, etc. In (b) the 90% particle size D of the small particle size magnetic raw material powder 90 When the content is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in a low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0239] (b) 10% particle size D of small particle size magnetic raw material powder 10 With 90% particle size D 90 Difference D 90 -D 10 It is preferably 0.1 μm or more, more preferably 0.3 μm or more, and particularly preferably 0.5 μm or more, and is preferably 5 μm or less, more preferably 4 μm or less, and particularly preferably 3 μm or less. 90 -D 10 When the content is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in a low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0240] (b) 10% particle size D of small particle size magnetic raw material powder 10 With 90% particle size D 90 Ratio D 90 / D 10 It is preferably 1.1 or more, more preferably 1.5 or more, and particularly preferably 2 or more, and is preferably 50 or less, more preferably 40 or less, and particularly preferably 30 or less. 90 / D 10 When the content is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in a low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0241] (b) The small-particle-size magnetic raw material powder may be nanocrystalline magnetic powder, amorphous magnetic powder, crystalline magnetic powder other than nanocrystalline magnetic powder, or a combination thereof.

[0242] The (b) small-diameter magnetic raw material powder may be particles of a magnetic material having a relative magnetic permeability greater than 1. The magnetic material contained in the (b) small-diameter magnetic raw material powder is preferably the magnetic material described as the magnetic material of the (B) small-diameter magnetic powder.

[0243] The (b) small-particle-size magnetic raw material powder preferably contains the above-mentioned magnetic material, and preferably contains only the above-mentioned magnetic material. The (b) small-particle-size magnetic raw material powder may be used alone or in combination of two or more.

[0244] As (b) small-particle-size magnetic raw material powder, commercially available magnetic powder can be used. Specific examples of commercially available magnetic powder include the same examples as (B) small-particle-size magnetic powder. When (b) small-particle-size magnetic raw material powder is obtained from the market, the commercially available magnetic powder can be classified and used as needed. For example, the average particle size D outside the above range can be 50 The commercially available magnetic powder is classified and the average particle size D is appropriately adjusted. 50 The value to use.

[0245] The (b) small-diameter magnetic raw material powder is preferably spherical. The aspect ratio of the particles of the (b) small-diameter magnetic raw material powder may be in the same range as the aspect ratio of the (B) small-diameter magnetic powder.

[0246] The amount (volume %) of the (b) small-particle-size magnetic raw material powder used in the production method according to the second embodiment of the present invention is preferably 5% by volume or more, more preferably 6% by volume or more, and particularly preferably 7% by volume or more, and preferably 50% by volume or less, more preferably 40% by volume or less, and particularly preferably 30% by volume or less, relative to 100% by volume of the non-volatile components of the resin composition to be produced. When the amount (volume %) of the (b) small-particle-size magnetic raw material powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0247] The amount (mass %) of the (b) small-particle-size magnetic raw material powder used in the production method according to the second embodiment of the present invention is preferably 5% by mass or more, more preferably 6% by mass or more, particularly preferably 7% by mass or more, and preferably 50% by mass or less, more preferably 40% by mass or less, particularly preferably 30% by mass or less, relative to 100% by mass of the non-volatile components of the resin composition to be produced. When the amount (mass %) of the (b) small-particle-size magnetic raw material powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0248] <(c) Intermediate Magnetic Raw Material Powder According to Second Embodiment>

[0249] The manufacturing method involved in the second embodiment of the present invention may include: combining (a) nanocrystalline magnetic raw material powder, (b) small particle size magnetic raw material powder and (D) thermosetting resin, and further mixing (c) magnetic powder as an optional component. The (c) magnetic powder as the (c) component means a magnetic powder having an average particle size greater than 2μm and less than 20μm, and smaller than the average particle size of the (a) nanocrystalline magnetic raw material powder. The (c) magnetic powder is sometimes referred to as "(c) intermediate magnetic raw material powder". The (c) intermediate magnetic raw material powder does not contain (a) nanocrystalline magnetic raw material powder and (b) small particle size magnetic raw material powder. After sorting, the (c) intermediate magnetic raw material powder contains the following (c1) and (c2) magnetic powders.

[0250] (c1) nanocrystalline magnetic powder having an average particle size greater than 2 μm and less than 5.5 μm;

[0251] (c2) Magnetic powder, which is a magnetic powder other than nanocrystalline magnetic powder, having an average particle size larger than 2 μm and smaller than the average particle size of (a) the nanocrystalline magnetic raw material powder.

[0252] As can be seen from the range of the average particle size, the intermediate magnetic raw material powder (c) may include the intermediate magnetic powder (C) described in the first embodiment. Therefore, the intermediate magnetic raw material powder (c) can generally suppress the increase in magnetic loss and improve the relative magnetic permeability, similar to the intermediate magnetic powder (C).

[0253] Specifically, (c) the average particle size D of the intermediate magnetic raw material powder 50 It is usually larger than 2 μm, preferably larger than 2.5 μm, more preferably larger than 3 μm, and usually smaller than the average particle size of (a) the nanocrystalline magnetic raw material powder, preferably smaller than 5.5 μm, more preferably smaller than 5 μm. 50In the case of the intermediate magnetic raw material powder (c), both the relative magnetic permeability and the magnetic loss can be effectively improved in the low frequency band, and a resin composition with particularly excellent coating properties can be produced. 50 The median particle size based on volume can be expressed by comparing (a) the average particle size D of the nanocrystalline magnetic raw material powder with 50 The same method was used to determine.

[0254] Generally, the volume-based particle size distribution of the (c) intermediate magnetic raw material powder follows a normal distribution. Therefore, the (c) intermediate magnetic raw material powder may have an average particle size D smaller than that of the (c) intermediate magnetic raw material powder. 50 10% particle size D 10 and greater than the average particle size D of the intermediate magnetic raw material powder (c). 50 90% particle size D 90 (c) 10% particle size D of the intermediate magnetic raw material powder 10 and 90% particle size D 90 (a) The 10% particle size D of the nanocrystalline magnetic raw material powder can be 10 and 90% particle size D 90 The same method was used to determine.

[0255] (c) 10% particle size D of intermediate magnetic raw material powder 10 The average particle size D is preferably 1 μm or more, more preferably 1.3 μm or more, and particularly preferably 1.5 μm or more. 50 For example, it may be 5 μm or less, 4 μm or less, 3 μm or less, etc. In (c) the 10% particle size D of the intermediate magnetic raw material powder 10 When the content is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in a low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0256] (c) 90% particle size D of the intermediate magnetic raw material powder 90 The average particle size D is preferably less than 10 μm, more preferably 9 μm or less, and particularly preferably 8 μm or less. 50 For example, it may be 3 μm or more, 4 μm or more, 5 μm or more, etc. In (c) the 90% particle size D of the intermediate magnetic raw material powder 90 When the content is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in a low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0257] (c) 10% particle size D of intermediate magnetic raw material powder 10 With 90% particle size D 90 Difference D 90 -D 10It is preferably 0.1 μm or more, more preferably 1 μm or more, and particularly preferably 2 μm or more, and is preferably 9 μm or less, more preferably 7 μm or less, and particularly preferably 5 μm or less. 90 -D 10 When the content is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in a low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0258] (c) 10% particle size D of intermediate magnetic raw material powder 10 With 90% particle size D 90 Ratio D 90 / D 10 It is preferably 1.1 or more, more preferably 1.5 or more, and particularly preferably 2 or more, and is preferably 10 or less, more preferably 8 or less, and particularly preferably 6 or less. 90 / D 10 When the content is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in a low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0259] The (c) intermediate magnetic raw material powder may be nanocrystalline magnetic powder, amorphous magnetic powder, crystalline magnetic powder other than nanocrystalline magnetic powder, or a combination thereof. The (c) intermediate magnetic raw material powder may be particles of a magnetic material having a relative magnetic permeability greater than 1. As the magnetic material contained in the (c) intermediate magnetic raw material powder, it is preferred to use the magnetic material described as the magnetic material of the (C) intermediate magnetic powder.

[0260] The intermediate magnetic raw material powder (c) preferably contains the above-mentioned magnetic material, and preferably contains only the above-mentioned magnetic material. The intermediate magnetic raw material powder (c) may be used alone or in combination of two or more.

[0261] As the intermediate magnetic raw material powder (c), commercially available magnetic powder can be used. Specific examples of commercially available magnetic powder include the same examples as those for the intermediate magnetic powder (C). When the intermediate magnetic raw material powder (c) is obtained from the market, the commercially available magnetic powder can be classified and used as needed. For example, the average particle size D outside the above range can be 50 The commercially available magnetic powder is classified and the average particle size D is appropriately adjusted. 50 The value to use.

[0262] The (c) intermediate magnetic raw material powder is preferably spherical. The range of the aspect ratio of the particles of the (c) intermediate magnetic raw material powder may be the same as the range of the aspect ratio of the (C) intermediate magnetic powder.

[0263] The amount (volume %) of the intermediate magnetic raw material powder (c) used in the production method according to the second embodiment of the present invention may be 0% by volume or more than 0% by volume, preferably 1% by volume or more, more preferably 3% by volume or more, particularly preferably 5% by volume or more, preferably 34% by volume or less, more preferably 30% by volume or less, particularly preferably 20% by volume or less, relative to 100% by volume of the non-volatile components of the resin composition to be produced. When the amount (volume %) of the intermediate magnetic raw material powder (c) is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in the low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0264] The amount (volume %) of the (c) intermediate magnetic raw material powder relative to 100 volume % of the non-volatile components of the resin composition is represented by "V(c)". In this case, the volume ratio of the (a) nanocrystalline magnetic raw material powder to the (c) intermediate magnetic raw material powder ((c) intermediate magnetic raw material powder / (a) nanocrystalline magnetic raw material powder) can be represented by "V(c) / V(a)". The volume ratio V(c) / V(a) can be 0 or greater than 0, and is preferably greater than 0.01, more preferably greater than 0.05, and particularly preferably greater than 0.1, and is preferably less than 0.8, more preferably less than 0.6, and particularly preferably less than 0.4. When the volume ratio V(c) / V(a) is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition with particularly excellent coating properties can be produced.

[0265] In addition, the volume ratio of the (b) small particle size magnetic raw material powder to the (c) intermediate magnetic raw material powder contained in the resin composition ((c) intermediate magnetic raw material powder / (b) small particle size magnetic raw material powder) can be represented by "V(c) / V(b)". This volume ratio V(c) / V(b) may be 0 or greater than 0, and is preferably 0.01 or greater, more preferably 0.1 or greater, and particularly preferably 0.2 or greater, and is preferably 9 or less, more preferably 7 or less, and particularly preferably 5 or less. When the volume ratio V(c) / V(b) is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0266] The total amount (volume %) of (a) nanocrystalline magnetic raw material powder, (b) small-particle-size magnetic raw material powder and (c) intermediate magnetic raw material powder relative to 100% by volume of the non-volatile component of the resin composition is preferably 40% by volume or more, more preferably 50% by volume or more, particularly preferably 60% by volume or more, and preferably 95% by volume or less, more preferably 90% by volume or less, particularly preferably 85% by volume or less. When the total amount (volume %) of (a) nanocrystalline magnetic raw material powder, (b) small-particle-size magnetic raw material powder and (c) intermediate magnetic raw material powder is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0267] Relative to 100% by volume of the total amount of all magnetic powders mixed for the manufacture of the resin composition, the total amount (volume %) of (a) nanocrystalline magnetic raw material powder, (b) small-particle magnetic raw material powder and (c) intermediate magnetic raw material powder is preferably 90% by volume or more, more preferably 94% by volume or more, particularly preferably 98% by volume or more, and usually less than 100% by volume. A large value indicates that there are few giant magnetic powders with an average particle size greater than 20 μm. When the total amount (volume %) of (a) nanocrystalline magnetic raw material powder, (b) small-particle magnetic raw material powder and (c) intermediate magnetic raw material powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0268] The amount (mass %) of the intermediate magnetic raw material powder (c) used in the production method according to the second embodiment of the present invention may be 0 mass % or more than 0 mass %, preferably 1 mass % or more, more preferably 3 mass % or more, particularly preferably 5 mass % or more, preferably 45 mass % or less, more preferably 30 mass % or less, particularly preferably 15 mass % or less, relative to 100 mass % of the non-volatile components of the produced resin composition. When the amount (mass %) of the intermediate magnetic raw material powder (c) is within the above range, both the relative magnetic permeability and the magnetic loss can be effectively improved in the low frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0269] The amount (mass %) of the (c) intermediate magnetic raw material powder relative to 100 mass % of the non-volatile components of the resin composition is represented by "M(c)". In this case, the mass ratio of the (a) nanocrystalline magnetic raw material powder to the (c) intermediate magnetic raw material powder ((c) intermediate magnetic raw material powder / (a) nanocrystalline magnetic raw material powder) can be represented by "M(c) / M(a)". The mass ratio M(c) / M(a) can be 0 or greater than 0, and is preferably greater than 0.01, more preferably greater than 0.05, and particularly preferably greater than 0.1, and is preferably less than 0.8, more preferably less than 0.6, and particularly preferably less than 0.4. When the mass ratio M(c) / M(a) is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low frequency band, and a resin composition with particularly excellent coating properties can be manufactured.

[0270] In addition, the mass ratio of the (b) small-particle-size magnetic raw material powder to the (c) intermediate-particle-size magnetic raw material powder contained in the resin composition ((c) intermediate-particle-size magnetic raw material powder / (b) small-particle-size magnetic raw material powder) can be represented by "M(c) / M(b)". The mass ratio M(c) / M(b) may be 0 or greater than 0, and is preferably 0.01 or greater, more preferably 0.1 or greater, and particularly preferably 0.2 or greater, and is preferably 9 or less, more preferably 7 or less, and particularly preferably 5 or less. When the mass ratio M(c) / M(b) is within the above range, both relative magnetic permeability and magnetic loss can be effectively improved in the low-frequency band, and a resin composition having particularly excellent coating properties can be produced.

[0271] The total amount (mass%) of (a) nanocrystalline magnetic raw material powder, (b) small-particle-size magnetic raw material powder and (c) intermediate magnetic raw material powder relative to 100% by mass of the non-volatile components of the resin composition is preferably 80% by mass or more, more preferably 85% by mass or more, particularly preferably 90% by mass or more, preferably 99% by mass or less, more preferably 98% by mass or less, particularly preferably 97% by mass or less. When the total amount (mass%) of (a) nanocrystalline magnetic raw material powder, (b) small-particle-size magnetic raw material powder and (c) intermediate magnetic raw material powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0272] Relative to 100% by mass of the total amount of all magnetic powders mixed for the manufacture of the resin composition, the total amount (mass %) of (a) nanocrystalline magnetic raw material powder, (b) small-particle magnetic raw material powder and (c) intermediate magnetic raw material powder is preferably 90% by mass or more, more preferably 94% by mass or more, particularly preferably 98% by mass or more, and usually less than 100% by mass. A large value indicates that there are few giant magnetic powders with an average particle size greater than 20 μm. When the total amount (mass %) of (a) nanocrystalline magnetic raw material powder, (b) small-particle magnetic raw material powder and (c) intermediate magnetic raw material powder is within the above range, both relative permeability and magnetic loss can be effectively improved in the low frequency band, and the coating property of the resin composition can be made better.

[0273] <(D) Thermosetting resin according to the second embodiment>

[0274] The manufacturing method involved in the second embodiment of the present invention includes mixing a (D) thermosetting resin as the (D) component with (a) nanocrystalline magnetic raw material powder and (b) small particle size magnetic raw material powder. As the (D) thermosetting resin involved in the second embodiment, the same resin as the (D) thermosetting resin involved in the first embodiment can be used. The range of the amount of the (D) thermosetting resin used in the manufacturing method involved in the second embodiment can be the same as the range described in the first embodiment. Therefore, in the manufacturing method involved in the second embodiment, for example, the range of the amount of liquid epoxy resin, the amount of epoxy resin and the amount of (D) thermosetting resin can be the same as the range described in the first embodiment, and the same effect as described in the first embodiment can be obtained.

[0275] <(E) Curing Accelerator According to Second Embodiment>

[0276] In the manufacturing method involved in the second embodiment of the present invention, in combination with the above-mentioned components, (E) a curing accelerator may be further mixed as an optional component. Regarding the (E) curing accelerator as the (E) component involved in the second embodiment, the same curing accelerator as the (E) curing accelerator involved in the first embodiment may be used. The range of the amount of the (E) curing accelerator used in the manufacturing method involved in the second embodiment may be the same as the range described in the first embodiment. According to the (E) curing accelerator, the same effect as described in the first embodiment can be obtained.

[0277] <(F) Dispersant According to Second Embodiment>

[0278] In the manufacturing method involved in the second embodiment of the present invention, in combination with the above-mentioned components, a (F) dispersant may be further mixed as an optional component. Regarding the (F) dispersant as the (F) component involved in the second embodiment, the same dispersant as the (F) dispersant involved in the first embodiment can be used. The range of the amount of the (F) dispersant used in the manufacturing method involved in the second embodiment may be the same as the range described in the first embodiment. According to the (F) dispersant, the same effect as described in the first embodiment can be obtained.

[0279] <(G) Optional Additives According to the Second Embodiment>

[0280] In the production method according to the second embodiment of the present invention, (G) an optional additive may be further mixed in combination with the above-mentioned components. As the (G) optional additive according to the second embodiment, the same additive as the (G) optional additive according to the first embodiment can be used.

[0281] <(H) Solvent According to Second Embodiment>

[0282] In the resin composition involved in the second embodiment of the present invention, in addition to the non-volatile components such as the above-mentioned (a) to (c) components and (D) to (G) components, an optional (H) solvent may be further included as a volatile component. As the (H) solvent involved in the second embodiment, the same solvent as the (H) solvent involved in the first embodiment can be used. In addition, the range of the amount of the (H) solvent used in the manufacturing method involved in the second embodiment can be the same as the range described in the first embodiment.

[0283] <Operation of the Manufacturing Method According to the Second Embodiment>

[0284] The manufacturing method according to the second embodiment of the present invention comprises mixing the above-mentioned (a) nanocrystalline magnetic raw material powder, (b) small-particle-size magnetic raw material powder and (D) thermosetting resin. In addition, as required, part or all of the optional components such as (c) intermediate magnetic raw material powder, (E) curing accelerator, (F) dispersant, (G) optional additives and (H) solvent can be mixed in combination with (a) nanocrystalline magnetic raw material powder, (b) small-particle-size magnetic raw material powder and (D) thermosetting resin.

[0285] The above-mentioned components may be mixed partially or all at the same time, or may be mixed sequentially. During the mixing of the components, the temperature may be appropriately set. Therefore, heating and / or cooling may be performed temporarily or continuously. In addition, during the mixing of the components, stirring or shaking may be performed. Furthermore, degassing may be performed under low pressure conditions such as vacuum.

[0286] <Resin composition produced by the production method according to the second embodiment>

[0287] The resin composition manufactured by the manufacturing method involved in the second embodiment of the present invention may include the above-mentioned components mixed. Therefore, the resin composition includes (a) nanocrystalline magnetic raw material powder, (b) small-particle magnetic raw material powder and (D) thermosetting resin, and may further include (c) intermediate magnetic raw material powder, (E) curing accelerator, (F) dispersant, (G) optional additives and (H) solvent as needed. In addition, the resin composition may include the above-mentioned components in the amount of their mixing. Therefore, the range of the amount of (a) nanocrystalline magnetic raw material powder, (b) small-particle magnetic raw material powder, (c) intermediate magnetic raw material powder, (D) thermosetting resin, (E) curing accelerator, (F) dispersant, (G) optional additives and (H) solvent contained in the resin composition may be as described above. In addition, the resin composition involved in the first embodiment can be manufactured by the manufacturing method involved in the second embodiment of the present invention.

[0288] The resin composition manufactured by the manufacturing method involved in the second embodiment of the present invention can be cured by heat. Therefore, by thermally curing the resin composition, a cured product of the resin composition can be obtained. Usually, among the components contained in the resin composition, volatile components such as (H) solvents can volatilize due to the heat during thermal curing, but non-volatile components such as (a) to (c) components and (D) to (G) components will not volatilize due to the heat during thermal curing. Therefore, the cured product of the resin composition can include the non-volatile components of the resin composition or its reaction product.

[0289] According to the resin composition manufactured by the manufacturing method involved in the second embodiment of the present invention, a cured product with improved relative magnetic permeability and magnetic loss can be obtained. In detail, the cured product of the resin composition can have high relative magnetic permeability and low magnetic loss in a low frequency band (e.g., 10MHz). In one example, the range of the relative magnetic permeability of the cured product of the resin composition manufactured by the manufacturing method involved in the second embodiment of the present invention may be in the same range as the relative magnetic permeability of the cured product of the resin composition involved in the first embodiment. In addition, in one example, the range of the loss factor of the cured product of the resin composition manufactured by the manufacturing method involved in the second embodiment of the present invention may be in the same range as the loss factor of the cured product of the resin composition involved in the first embodiment. Relative magnetic permeability and loss factor can be measured by the same method as described in the first embodiment.

[0290] The resin composition produced by the production method according to the second embodiment of the present invention can have excellent coating properties, similar to the resin composition according to the first embodiment.

[0291] The properties of the resin composition produced by the production method according to the second embodiment of the present invention are not particularly limited, but are preferably in a paste state having fluidity, similar to the resin composition according to the first embodiment.

[0292] The resin composition manufactured by the manufacturing method according to the second embodiment of the present invention can obtain the same advantages as the resin composition according to the first embodiment. In addition, the resin composition manufactured by the manufacturing method according to the second embodiment of the present invention can be used for the same purposes as the resin composition according to the first embodiment.

[0293] <Resin sheet according to third embodiment>

[0294] The resin sheet according to the third embodiment of the present invention comprises: a support and a resin composition layer formed on the support. The resin composition layer comprises a resin composition, preferably only a resin composition. As the above-mentioned resin composition, one or a combination of the resin composition according to the first embodiment and the resin composition manufactured by the manufacturing method according to the second embodiment can be used.

[0295] From the viewpoint of thinning, the thickness of the resin composition layer is preferably 250 μm or less, more preferably 200 μm or less. The lower limit of the thickness of the resin composition layer is not particularly limited, and may be, for example, 5 μm or more, 10 μm or more, or the like.

[0296] Examples of the support include films of plastic materials, metal foils, and release papers, and films of plastic materials and metal foils are preferred.

[0297] When a film of a plastic material is used as a support, examples of the plastic material include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), acrylic polymers such as polycarbonate (PC) and polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among them, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0298] When a metal foil is used as a support, examples of the metal foil include copper foil and aluminum foil, preferably copper foil. The copper foil may be a foil made of a single metal such as copper or an alloy of copper and other metals (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.).

[0299] The surface of the support to be in contact with the resin composition layer may be subjected to a surface treatment such as a matte treatment or a corona treatment.

[0300] In addition, as the support, a support with a release layer having a release layer on the surface bonded to the resin composition layer can be used. As a release agent for the release layer of the support with a release layer, for example, there can be mentioned: one or more release agents selected from alkyd release agents, polyolefin release agents, urethane release agents and silicone release agents. The support with a release layer can use commercially available products, for example, there can be mentioned: "PET501010", "SK-1", "AL-5", "AL-7" manufactured by LINTEC, which is a PET film having a release layer with a silicone release agent or an alkyd resin release agent as a main component; "Lumirror T60" manufactured by Toray Industries; "Purex" manufactured by Teijin; "Unipeel" manufactured by UNITIKA, etc.

[0301] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, the thickness of the entire support with a release layer is preferably in the above range.

[0302] In the resin sheet, a protective film selected according to the support can be provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface on the opposite side to the support). The thickness of the protective film is not particularly limited, and is, for example, 1 μm to 40 μm. By laminating the protective film, dust can be prevented from adhering to the surface of the resin composition layer and from causing damage to the surface of the resin composition layer.

[0303] The resin sheet can be manufactured, for example, by a manufacturing method including a step of applying a resin composition on a support. The resin sheet manufacturing method can be manufactured by a manufacturing method including the following steps: a step of manufacturing a resin composition by the manufacturing method described in the first embodiment or the second embodiment; and a step of applying the resin composition on a support. The application of the resin composition can be performed, for example, using a coating device such as a die coater. By applying the resin composition, a resin composition layer can be formed on the support, so that a resin sheet can be obtained.

[0304] As needed, an organic solvent can be mixed in the resin composition and then applied to the support. As an organic solvent, for example, the (H) solvent described in the first embodiment can be used. When an organic solvent is used, it can be dried after coating as needed. Drying can be implemented by heating, blowing hot air, etc. There is no particular limitation on the drying conditions, and the content of the organic solvent in the resin composition layer is generally 10% by mass or less, preferably 5% by mass or less. Although it varies depending on the components contained in the resin composition, for example, by drying at 50°C to 150°C for 3 minutes to 10 minutes, a resin composition layer can be formed.

[0305] The resin sheet can be stored by being wound up in a roll shape. When the resin sheet has a protective film, it is usually used by peeling off the protective film.

[0306] <Circuit Board According to Fourth Embodiment>

[0307] The circuit board according to the fourth embodiment of the present invention includes a cured product of a resin composition. As the resin composition, one of the resin composition according to the first embodiment and the resin composition produced by the production method according to the second embodiment or a combination thereof can be used.

[0308] There is no restriction on the specific structure of the circuit substrate, and it only needs to include a cured product of a resin composition. The circuit substrate involved in the first example includes: a substrate having a hole and a cured product of a resin composition filled in the hole. In addition, the circuit substrate involved in the second example includes: a cured product layer formed by a cured product of a resin composition. Hereinafter, the circuit substrates involved in these first and second examples are described.

[0309] (Circuit board according to the first example)

[0310] The circuit board involved in the first example includes: a substrate having holes formed therein and a cured product of a resin composition filled in the holes. The circuit board can be manufactured, for example, by a manufacturing method including the following steps:

[0311] (1) a step of filling the holes of the substrate with a resin composition; and

[0312] (2) A step of thermally curing the resin composition to obtain a cured product.

[0313] In addition, the method for manufacturing the circuit board according to the first example may further include the following steps:

[0314] (3) a step of grinding the surface of the cured product or the resin composition;

[0315] (4) a step of roughening the solidified product; and

[0316] (5) A step of forming a conductive layer on the roughened surface of the cured product.

[0317] Usually, the above steps (1) to (5) are carried out in the order of step (1), step (2), step (3), step (4) and step (5), but step (2) may be carried out after step (3). In the method for manufacturing a circuit substrate according to the first example, a paste-like resin composition is preferably used to form a cured product. In the following description, an example of a substrate having a through hole (a hole penetrating the substrate in the thickness direction) is shown for description.

[0318] -Process (1)-

[0319] Step (1) generally includes the step of preparing a substrate having a through hole. The substrate can be purchased from the market. Alternatively, the substrate can be prepared by manufacturing using an appropriate material. An example of a method for manufacturing a substrate is described below.

[0320] Figure 1 1 is a cross-sectional view schematically showing a core substrate 10 prepared in the method for manufacturing a circuit substrate according to the first example of the fourth embodiment of the present invention. Figure 1 As shown in the example, the process of preparing the substrate may include the process of preparing the core substrate 10. The core substrate 10 usually includes a supporting substrate 11. As the supporting substrate 11, for example, insulating substrates such as glass epoxy substrates, metal substrates, polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates can be cited. In addition, a metal layer can be provided on the supporting substrate 11. The metal layer can be provided on a single surface of the supporting substrate 11, or on both surfaces. Here, an example is shown in which a first metal layer 12 and a second metal layer 13 are provided on both surfaces of the supporting substrate 11. As the first metal layer 12 and the second metal layer 13, layers formed using metals such as copper can be cited. The first metal layer 12 and the second metal layer 13 can be, for example, copper foil with a carrier copper foil, or can be a metal layer formed from the material of the conductor layer described later.

[0321] Figure 2 1 is a cross-sectional view schematically showing a core substrate 10 having a through hole 14 formed therein in the method for manufacturing a circuit substrate according to the first example of the fourth embodiment of the present invention. Figure 2 As shown in the example, the process of preparing the substrate may include the process of forming a through hole 14 on the core substrate 10. The through hole 14 can be formed, for example, by drilling, laser irradiation, plasma irradiation, etc. In general, the through hole 14 can be formed by forming a through hole on the core substrate 10. If a specific example is given, the formation of the through hole 14 can be implemented using a commercially available drill device. As a commercially available drill device, for example, "ND-1S211" manufactured by Hitachi Via Machinery Co., Ltd. can be cited.

[0322] Figure 3 1 is a cross-sectional view schematically showing a core substrate 10 having a plating layer 20 formed in a through hole 14 in a method for manufacturing a circuit substrate according to a first example of a fourth embodiment of the present invention. Figure 3As shown, the process of preparing the substrate may include a process of forming an electroplating layer 20 after the core substrate 10 is subjected to a roughening treatment as required. As the above-mentioned roughening treatment, any of dry and wet roughening treatments may be performed. Examples of dry roughening treatments include plasma treatment and the like. In addition, examples of wet roughening treatments include methods of sequentially performing swelling treatments based on a swelling solution, roughening treatments based on an oxidant, and neutralization treatments based on a neutralizing solution. The electroplating layer 20 may be formed using an electroplating method. The step of forming the electroplating layer 20 using an electroplating method may be the same as the formation of the conductor layer in the later-described step (5). Here, an example in which the electroplating layer 20 is formed in the through hole 14, on the surface of the first metal layer 12, and on the surface of the second metal layer 13 is shown for illustration.

[0323] Figure 4 1 is a cross-sectional view schematically showing a state where the through hole 14 of the core substrate 10 is filled with the resin composition 30a in the method for manufacturing a circuit substrate according to the first example of the fourth embodiment of the present invention. Figure 4 As shown, regarding step (1), after preparing the core substrate 10 having the through hole 14 formed therein as described above, the step includes filling the through hole 14 of the core substrate 10 with a resin composition 30a. The filling can be performed, for example, by a printing method. As a printing method, for example, there can be cited: a method of printing the resin composition 30a into the through hole 14 via a squeegee, a method of printing the resin composition 30a via a cartridge, a method of printing the resin composition 30a by mask printing, a roller coating method, an inkjet method, and the like. Usually, excess resin composition 30a protrudes or adheres outside the through hole 14. Therefore, the resin composition 30a is not only arranged in the through hole 14, but also can be arranged outside the through hole 14.

[0324] -Process (2)-

[0325] Figure 5 Schematic cross-sectional view for explaining step (2) of the method for manufacturing a circuit substrate according to the first example of the fourth embodiment of the present invention. Figure 5 As shown, step (2) includes curing the resin composition 30 a to form the cured product 30 after filling the through hole 14 with the resin composition 30 a .

[0326] The curing of the resin composition 30a is usually performed by thermal curing. The thermal curing conditions of the resin composition 30a can be appropriately set within the range of the curing of the resin composition 30a. The curing temperature is preferably 120°C or more, more preferably 130°C or more, and more preferably 150°C or more, preferably 245°C or less, more preferably 220°C or less, and more preferably 200°C or less. The curing time is preferably 5 minutes or more, more preferably 10 minutes or more, and more preferably 15 minutes or more, preferably 120 minutes or less, more preferably 110 minutes or less, and more preferably 100 minutes or less.

[0327] The degree of curing of the cured product 30 obtained in step (2) is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. The degree of curing can be measured using, for example, a differential scanning calorimeter.

[0328] Regarding the manufacturing method of the circuit board involved in the first example, after the resin composition 30a is filled into the through hole 14 and before the resin composition 30a is cured, a step of heating the resin composition 30a at a temperature lower than the curing temperature (preheating step) may be included. For example, before the resin composition 30a is cured, the resin composition 30a may be preheated at a temperature of 50°C or more and less than 120°C (preferably 60°C or more and 110°C or less, more preferably 70°C or more and 100°C or less) for 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes).

[0329] -Process (3)-

[0330] Figure 6 Schematic cross-sectional view for explaining step (3) of the method for manufacturing a circuit substrate according to the first example of the fourth embodiment of the present invention. Figure 6 As shown, step (3) includes grinding the excess solidified material 30 protruding from or attached to the core substrate 10. The excess solidified material 30 is removed by grinding, so that the surface of the solidified material 30 can be flattened. The surface (ground surface) 31 of the solidified material 30 flattened by grinding can usually form the same plane as the surface 21 around the ground surface 31 (for example, the surface of the core substrate 10, the surface of the electroplating layer 20).

[0331] As a grinding method, a method that can remove the excess solidified material 30 protruding from or attached to the core substrate 10 can be adopted. As such a grinding method, for example, polishing grinding, belt grinding, ceramic grinding, etc. can be cited. As a commercially available polishing grinding device, for example, "NT-700IM" manufactured by Ishii Hyoki Co., Ltd. can be cited.

[0332] From the viewpoint of improving the adhesion with the conductor layer, the arithmetic mean roughness (Ra) of the polished surface (after thermal curing of the cured layer) 31 of the cured product 30 is preferably 300 nm or more, more preferably 350 nm or more, and further preferably 400 nm or more. The upper limit is preferably 1000 nm or less, more preferably 900 nm or less, and further preferably 800 nm or less. The surface roughness (Ra) can be measured, for example, using a non-contact surface roughness meter.

[0333] In the case where step (3) is performed after step (2), the method for manufacturing a circuit substrate may include a step of heat treating the cured product 30 after step (2) and before step (3) in order to further improve the degree of cure of the cured product 30. The temperature in the above-mentioned heat treatment may be in accordance with the above-mentioned curing temperature. The specific heat treatment temperature is preferably 120°C or more, more preferably 130°C or more, and more preferably 150°C or more, preferably 245°C or less, more preferably 220°C or less, and more preferably 200°C or less. The heat treatment time is preferably 5 minutes or more, more preferably 10 minutes or more, and more preferably 15 minutes or more, and preferably 90 minutes or less, more preferably 70 minutes or less, and more preferably 60 minutes or less.

[0334] In addition, when step (3) is performed before step (2), the method for producing a circuit board may include a step of preheating the resin composition layer at a temperature lower than the curing temperature of the resin composition before step (3). The temperature in the preheating is preferably 100° C. or higher, more preferably 110° C. or higher, and further preferably 120° C. or higher, preferably 245° C. or lower, more preferably 220° C. or lower, and further preferably 200° C. or lower. The heat treatment time is preferably 5 minutes or longer, more preferably 10 minutes or longer, and further preferably 15 minutes or longer, and preferably 90 minutes or shorter, more preferably 70 minutes or shorter, and further preferably 60 minutes or shorter.

[0335] -Process (4)-

[0336] Step (4) includes roughening the surface of the solidified article 30 (decontamination treatment). The surface of the solidified article 30 is roughened by the roughening treatment. When the surface of the solidified article 30 is ground, it usually includes roughening the ground surface 31 thereof (decontamination treatment). There are no particular limitations on the steps and conditions of the roughening step, and for example, the steps and conditions used in the method for manufacturing a multilayer printed wiring board can be used. As a roughening step, for example, the surface of the solidified article 30 can be roughened by sequentially performing a swelling treatment based on a swelling liquid, a roughening treatment based on an oxidant, and a neutralization treatment based on a neutralizing liquid.

[0337] As the swelling liquid that can be used in the roughening process, for example, there can be mentioned: an alkaline solution, a surfactant solution, etc., preferably an alkaline solution, and as for the alkaline solution as the swelling liquid, a sodium hydroxide solution and a potassium hydroxide solution are more preferred. As commercially available swelling liquids, for example, there can be mentioned: "Swelling Dip Securiganth P", "Swelling Dip Securiganth SBU" manufactured by Atotech Japan, etc. The swelling treatment based on the swelling liquid can be carried out, for example, by immersing the solidified material 30 in a swelling liquid at 30°C to 90°C for 1 minute to 20 minutes. From the viewpoint of suppressing the swelling of the resin constituting the solidified material 30 to an appropriate level, it is preferred to immerse the solidified material 30 in a swelling liquid at 40°C to 80°C for 5 minutes to 15 minutes.

[0338] As an oxidant that can be used for roughening treatment based on an oxidant, for example, an alkaline permanganate solution obtained by dissolving potassium permanganate or sodium permanganate in an aqueous solution of sodium hydroxide can be cited. The roughening treatment based on an oxidant such as an alkaline permanganate solution is preferably performed by immersing the cured product 30 in an oxidant solution heated to 60° C. to 80° C. for 10 minutes to 30 minutes. In addition, the concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. As a commercially available oxidant, for example, alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securiganth P" manufactured by Atotech Japan can be cited.

[0339] As a neutralizing solution that can be used for the neutralization treatment, an acidic aqueous solution is preferred. As a commercially available product of the neutralizing solution, for example, there can be cited: "Reduction Solution Securiganth P" manufactured by Atotech Japan. The neutralization treatment based on the neutralizing solution can be performed by immersing the treated surface that has been roughened by the oxidizing solution in the neutralizing solution at 30°C to 80°C for 5 minutes to 30 minutes. In view of operability, etc., it is preferred to immerse the cured product 30 that has been roughened by the oxidizing solution in the neutralizing solution at 40°C to 70°C for 5 minutes to 20 minutes.

[0340] From the viewpoint of improving the adhesion with the conductor layer, the arithmetic mean roughness (Ra) of the surface of the cured product 30 after the roughening treatment is preferably 300 nm or more, more preferably 350 nm or more, and further preferably 400 nm or more. The upper limit is preferably 1500 nm or less, more preferably 1200 nm or less, and further preferably 1000 nm or less. The surface roughness (Ra) can be measured, for example, using a non-contact surface roughness meter.

[0341] -Process (5)-

[0342] Figure 7 Schematic cross-sectional view for explaining step (5) of the method for manufacturing a circuit substrate according to the first example of the fourth embodiment of the present invention. Figure 7 As shown in FIG. 1 , step (5) includes forming a conductor layer 40 on the polished surface 31 of the cured product 30. Here, an example is shown in which the conductor layer 40 is formed not only on the polished surface 31 of the cured product 30 but also on the surrounding surface 21 (e.g., the surface of the core substrate 10, the surface of the electroplating layer 20). Figure 7 , an example is shown in which the conductor layer 40 is formed on both sides of the core substrate 10 , but the conductor layer 40 may be formed only on one side of the core substrate 10 .

[0343] Figure 8 Schematic cross-sectional view for explaining step (5) of the method for manufacturing a circuit substrate according to the first example of the fourth embodiment of the present invention. Figure 8 As shown, step (5) may include the following step: after forming the conductor layer 40, the conductor layer 40, the first metal layer 12, the second metal layer 13 and a portion of the plating layer 20 are removed by etching or the like to form a pattern conductor layer 41.

[0344] The method for forming the conductor layer 40 includes, for example, electroplating, sputtering, and evaporation, among which electroplating is preferred. In a suitable embodiment, electroplating is performed on the surface of the cured product 30 (and the electroplated layer 20) by an appropriate method such as a semi-additive method and a full-additive method to form a pattern conductor layer 41 having a desired wiring pattern. Examples of the material of the conductor layer 40 include single metals such as gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium; and alloys of two or more metals selected from gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium. Among them, from the viewpoints of versatility, cost, ease of patterning, etc., it is preferred to use chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy, more preferably to use chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or a nickel-chromium alloy, and even more preferably to use copper.

[0345] Here, an example of a method for forming a pattern conductor layer 41 on the polished surface 31 of the cured product 30 is described in detail. A plating seed layer is formed on the polished surface 31 of the cured product 30 by electroless plating. Next, an electrolytic plating layer is formed on the formed plating seed layer by electrolytic plating. Thereafter, as required, the unnecessary plating seed layer is removed by etching or the like, and a pattern conductor layer 41 having a desired wiring pattern can be formed. After the pattern conductor layer 41 is formed, an annealing treatment can be performed as required in order to improve the adhesion strength of the pattern conductor layer 41. The annealing treatment can be performed, for example, by heating at 150°C to 200°C for 20 minutes to 90 minutes.

[0346] From the viewpoint of thinning, the thickness of the pattern conductor layer 41 is preferably 70 μm or less, more preferably 60 μm or less, further preferably 50 μm or less, further preferably 40 μm or less, particularly preferably 30 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. The lower limit is preferably 1 μm or more, more preferably 3 μm or more, and further preferably 5 μm or more.

[0347] By the above method, the circuit board 1 including the cured product 30 of the resin composition 30a can be manufactured.

[0348] (Circuit board according to the second example)

[0349] The circuit substrate involved in the second example includes: a cured product layer containing a cured product of a resin composition. The cured product layer preferably only contains a cured product of the resin composition. The cured product layer is preferably formed using a resin sheet. The circuit substrate can be manufactured, for example, by a manufacturing method including the following steps:

[0350] (i) forming a cured product layer on the inner substrate;

[0351] (ii) a step of performing a hole-forming process on the cured layer;

[0352] (iii) a step of roughening the surface of the cured product layer; and

[0353] (iv) A step of forming a conductive layer on the surface of the cured product layer.

[0354] -Process (i)-

[0355] Step (i) includes forming a cured product layer on the inner substrate. Preferably, step (i) includes laminating a resin sheet on the inner substrate in a manner such that the resin composition layer is bonded to the inner substrate to form a cured product layer. For example, laminating a resin sheet on the inner substrate in a manner such that the resin composition layer is bonded to the inner substrate, and thermally curing the resin composition layer to form a cured product layer.

[0356] Fig. 9: is a schematic cross-sectional view for explaining step (i) in the method for manufacturing a circuit substrate according to the second example of the fourth embodiment of the present invention. Fig. 9 As shown, a resin sheet 310 is prepared, which includes a support 330 and a resin composition layer 320a provided on the support 330. Then, the resin sheet 310 and the inner substrate 200 are laminated so that the resin composition layer 320a is bonded to the inner substrate 200.

[0357] An insulating substrate can be used as the inner substrate 200. Examples of the inner substrate 200 include insulating substrates such as glass epoxy substrates, metal substrates, polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates. The inner substrate 200 can be an inner circuit substrate having wiring and the like built into its thickness.

[0358] The inner substrate 200 shown in this example includes: a first conductor layer 420 provided on the first main surface 200a and an external terminal 240 provided on the second main surface 200b. The first conductor layer 420 may include a plurality of wirings. Fig. 9 In the example shown, only the coil-shaped conductive structure 400 constituting the inductor element is shown (see Fig.12 The external terminal 240 may be a terminal for electrically connecting to an external device (not shown) or the like. The external terminal 240 may be configured as a part of a conductor layer provided on the second main surface 200b.

[0359] Examples of the conductive material that can constitute the first conductive layer 420 and the external terminal 240 include the same materials as those for the conductive layer described in the first example.

[0360] The first conductor layer 420 and the external terminal 240 may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers composed of different types of metals or alloys are stacked. In addition, the thickness of the first conductor layer 420 and the external terminal 240 may be the same as that of the second conductor layer 440 described later.

[0361] There is no particular restriction on the line width (L) / line spacing (S) ratio of the first conductor layer 420 and the external terminal 240. From the viewpoint of reducing surface irregularities to obtain a cured layer with excellent smoothness, it is usually 900 / 900 μm or less, preferably 700 / 700 μm or less, more preferably 500 / 500 μm or less, further preferably 300 / 300 μm or less, and further preferably 200 / 200 μm or less. There is no particular restriction on the lower limit of the line width / line spacing ratio. From the viewpoint of making the resin composition layer well embedded in the wiring space, it is preferably 1 / 1 μm or more.

[0362] The inner substrate 200 may have a plurality of through holes 220 penetrating the inner substrate 200 from the first main surface 200a to the second main surface 200b. Through-hole wiring 220a is provided in the through hole 220. The through-hole wiring 220a electrically connects the first conductor layer 420 and the external terminal 240.

[0363] The resin composition layer 320a and the inner substrate 200 can be bonded, for example, by heat-pressing the resin sheet 310 to the inner substrate 200 from the support 330 side. As a component for heat-pressing the resin sheet 310 to the inner substrate 200 (hereinafter, also referred to as a "heat-pressing component"), for example, a heated metal plate (stainless steel (SUS) end plate, etc.) or a metal roller (SUS roller, etc.) can be cited. It should be noted that it is preferred that the heat-pressing component is not pressed by directly contacting the resin sheet 310, but is pressed through a sheet made of an elastic material such as heat-resistant rubber, so that the resin sheet 310 fully follows the surface unevenness of the inner substrate 200.

[0364] The temperature during heat pressing is preferably in the range of 80°C to 160°C, more preferably in the range of 90°C to 140°C, and further preferably in the range of 100°C to 120°C. The pressure during heat pressing is preferably in the range of 0.098MPa to 1.77MPa, and more preferably in the range of 0.29MPa to 1.47MPa. The time during heat pressing is preferably in the range of 20 seconds to 400 seconds, and more preferably in the range of 30 seconds to 300 seconds. The bonding of the resin sheet to the inner substrate is preferably carried out under reduced pressure conditions of 26.7hPa or less.

[0365] The resin composition layer 320a of the resin sheet 310 and the inner substrate 200 can be bonded using a commercially available vacuum laminator. Examples of commercially available vacuum laminators include a vacuum pressure laminator manufactured by Meiki Manufacturing Co., Ltd. and a vacuum applicator manufactured by Nikko-Materials Co., Ltd.

[0366] After the resin sheet 310 and the inner substrate 200 are bonded, the laminated resin sheet 310 can be smoothed by pressing the heating and pressing member at normal pressure (atmospheric pressure), for example, from the support 330 side. The pressing conditions for the smoothing treatment can be set to the same conditions as the heating and pressing conditions for the above-mentioned lamination. The smoothing treatment can be performed using a commercially available laminator. It should be noted that the lamination and smoothing treatment can be performed continuously using the above-mentioned commercially available vacuum laminator.

[0367] Fig.10: is a schematic cross-sectional view for explaining step (i) in the method for manufacturing a circuit substrate according to the second example of the fourth embodiment of the present invention. After the resin sheet 310 is laminated on the inner substrate 200, the resin composition layer 320a is thermally cured to form a cured layer. In this example, Fig.10 As shown, the resin composition layer 320 a bonded to the inner substrate 200 is thermally cured to form the first cured material layer 320 .

[0368] The heat curing conditions of the resin composition layer 320a can be appropriately set within the range of curing of the resin composition. The curing temperature is preferably 120°C or more, more preferably 130°C or more, and more preferably 150°C or more, preferably 245°C or less, more preferably 220°C or less, and more preferably 200°C or less. The curing time is preferably 5 minutes or more, more preferably 10 minutes or more, and more preferably 15 minutes or more, preferably 120 minutes or less, more preferably 110 minutes or less, and more preferably 100 minutes or less.

[0369] The support body 330 may be removed after the thermal curing in step (i) and between step (ii), or may be peeled off after step (ii).

[0370] The arithmetic mean roughness (Ra) of the cured product layer before the roughening treatment is preferably 300 nm or more, more preferably 350 nm or more, and further preferably 400 nm or more from the viewpoint of improving the adhesion with the electroplating. The upper limit is preferably 1000 nm or less, more preferably 900 nm or less, and further preferably 800 nm or less. The surface roughness (Ra) can be measured, for example, using a non-contact surface roughness meter.

[0371] Step (i) may include coating the resin composition on the inner substrate 200 using a coating device such as a die coater instead of the resin sheet and thermally curing the resin composition to form a cured product layer.

[0372] -Step (ii)-

[0373] Fig.11 : is a schematic cross-sectional view for explaining step (ii) in the method for manufacturing a circuit substrate according to the second example of the fourth embodiment of the present invention. Fig.11 As shown in FIG. 1 , step (ii) includes: performing a hole-forming process on the first cured material layer 320 to form a via hole 360. The via hole 360 ​​can be a path for electrically connecting the first conductor layer 420 to the second conductor layer 440 described later. The via hole 360 ​​can be formed by, for example, using a drill, laser, plasma, etc. The size or shape of the hole can be appropriately determined according to the design of the printed wiring board.

[0374] -Process (iii)-

[0375] In step (iii), the surface of the cured product layer having the via hole formed therein is subjected to a roughening treatment. The roughening treatment in step (iii) can be performed by the same method as that described in step (4) of the first example.

[0376] The arithmetic mean roughness (Ra) after the roughening treatment of the cured layer is preferably 300 nm or more, more preferably 350 nm or more, and further preferably 400 nm or more from the viewpoint of improving the adhesion with the electroplating. The upper limit is preferably 1500 nm or less, more preferably 1200 nm or less, and further preferably 1000 nm or less. The surface roughness (Ra) can be measured, for example, using a non-contact surface roughness meter.

[0377] -Step (iv)-

[0378] Fig.12 : is a schematic cross-sectional view for explaining step (iv) in the method for manufacturing a circuit substrate according to the second example of the fourth embodiment of the present invention. Fig.12 As shown, in step (iv), the second conductor layer 440 is formed on the first cured material layer 320 .

[0379] Examples of the conductive material that can constitute the second conductive layer 440 include the same materials as those for the conductive layer described in the first example.

[0380] From the viewpoint of thinning, the thickness of the second conductor layer 440 is preferably 70 μm or less, more preferably 60 μm or less, further preferably 50 μm or less, further preferably 40 μm or less, particularly preferably 30 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. The lower limit is preferably 1 μm or more, more preferably 3 μm or more, and further preferably 5 μm or more.

[0381] The second conductor layer 440 can be formed by electroplating. The second conductor layer 440 is preferably formed by a wet plating method such as a semi-additive method or a full-additive method including an electroless plating step, a mask pattern forming step, an electrolytic plating step, and a rapid etching step. By forming the second conductor layer 440 by the wet plating method, the second conductor layer 440 including a desired wiring pattern can be easily formed. It should be noted that, through this process, the via-hole wiring 360a can be formed in the via 360 at the same time.

[0382] For example, as described below Figures 13-15As shown in one example, the first conductor layer 420 and the second conductor layer 440 can be provided in a spiral shape. In one example, one end on the central side of the spiral wiring portion of the second conductor layer 440 is electrically connected to one end on the central side of the spiral wiring portion of the first conductor layer 420 through the via-hole wiring 360a. The other end on the peripheral side of the spiral wiring portion of the second conductor layer 440 is electrically connected to the pad 420a of the first conductor layer 420 through the via-hole wiring 360a. Therefore, the other end on the peripheral side of the spiral wiring portion of the second conductor layer 440 is electrically connected to the external terminal 240 via the via-hole wiring 360a, the pad 420a, and the through-hole wiring 220a.

[0383] The coil-shaped conductive structure 400 is composed of a spiral wiring portion as a part of the first conductor layer 420 , a spiral wiring portion as a part of the second conductor layer 440 , and an intra-via wiring 360 a that electrically connects the spiral wiring portion of the first conductor layer 420 and the spiral wiring portion of the second conductor layer 440 .

[0384] After step (iv), a step of forming a cured product layer on the conductor layer may be further performed. Fig.14 As shown in the example of FIG, the second cured material layer 340 is formed on the first cured material layer 320 formed with the second conductor layer 440 and the via-hole wiring 360a. The second cured material layer 340 can be formed by the same process as the process already described. By the above method, the circuit substrate 100 including the first cured material layer 320 and the second cured material layer 340 formed by the cured material of the resin composition can be manufactured.

[0385] <Sensor substrate according to fifth embodiment>

[0386] The sensor substrate according to the fifth embodiment of the present invention includes the circuit substrate according to the fourth embodiment. When such a sensor substrate includes the circuit substrate according to the first example, at least a portion of the surrounding area of ​​the cured product of the resin composition may have a sensor pattern formed of a conductor. In this case, the sensor substrate may include, for example, a sensor element composed of "a sensor pattern formed by at least a portion of the first metal layer 12, the second metal layer 13, the electroplated layer 20, and the pattern conductor layer 41" and "a core formed of the cured product 30 surrounded by the sensor pattern". Such a sensor substrate may be applied to, for example, the sensor substrate described in Japanese Patent Application Laid-Open No. 2016-197624.

[0387] In the case of the circuit substrate according to the second example, the sensor substrate may include a cured material layer and a conductive structure at least a portion of which is embedded in the cured material layer. Furthermore, the sensor substrate may include a sensor element, the sensor element being composed of the conductive structure and a portion of the cured material layer extending in the thickness direction of the cured material layer and surrounded by the conductive structure.

[0388] Fig.13 This is a schematic plan view of the circuit substrate 100 included in the sensor substrate as viewed from one side in the thickness direction of the circuit substrate 100 . Fig.14 It means in Fig.13 The schematic diagram of the cut end surface of the circuit substrate 100 cut at the position indicated by the II-II dot-dash line is shown. Fig.15 It is a schematic plan view for explaining the structure of the first conductor layer 420 of the circuit substrate 100 included in the sensor substrate.

[0389] like Fig.13 and Fig.14 As shown as an example in FIG. 1 , the circuit substrate 100 may be a substrate having a plurality of cured material layers (a first cured material layer 320, a second cured material layer 340) and a plurality of conductor layers (a first conductor layer 420, a second conductor layer 440). Therefore, in the example shown here, the circuit substrate 100 may be a built-up wiring board having a build-up cured material layer and a build-up conductor layer. In addition, the circuit substrate 100 includes an inner layer substrate 200.

[0390] like Fig.14 As shown in FIG. 1 , the first cured material layer 320 and the second cured material layer 340 constitute the magnetic part 300 which can be regarded as a single cured material layer. Therefore, the coil-shaped conductive structure 400 is provided in a manner that at least a portion is buried in the magnetic part 300. That is, in the circuit substrate 100 shown in this example, the inductor element is constituted by the coil-shaped conductive structure 400 and the core portion, which is a portion of the magnetic part 300 extending in the thickness direction of the magnetic part 300 and surrounded by the coil-shaped conductive structure 400.

[0391] like Fig.15 As shown as an example in FIG. 1 , the first conductor layer 420 includes: a spiral wiring portion for constituting the coil-shaped conductive structure 400 and a rectangular pad 420a electrically connected to the through-hole wiring 220a. In the example shown here, the spiral wiring portion includes: a straight portion, a bent portion bent at a right angle, and a detour portion detour at the pad 420a. In addition, the spiral wiring portion of the first conductor layer 420 has a shape that is roughly rectangular in overall outline and is wound in a counterclockwise direction from the center side to the outside thereof.

[0392] Similarly, the second conductor layer 440 is provided on the first cured material layer 320. The second conductor layer 440 includes a spiral wiring portion for constituting the coil-shaped conductive structure 400. Fig.13 or Fig.14 In the embodiment, the spiral wiring portion includes a straight line portion and a curved portion curved at a right angle. Fig.13 or Fig.14 In FIG. 4 , the spiral wiring portion of the second conductor layer 440 has a generally rectangular outline and is wound in a clockwise direction from the center toward the outside.

[0393] The sensor substrate can be used as a wiring board for mounting electronic components such as semiconductor chips, or as a (multi-layer) printed wiring board using the wiring board as an inner substrate. In addition, it can be used as a chip sensor component obtained by singulating the wiring board, or as a printed wiring board with the chip sensor component mounted on the surface.

[0394] In addition, various forms of semiconductor devices can be manufactured using the wiring board. The semiconductor device including the wiring board can be suitably used in electrical products (e.g., computers, mobile phones, digital cameras, and televisions) and transportation vehicles (e.g., motorcycles, cars, trains, ships, and airplanes).

[0395] Example

[0396] The present invention is specifically described below by way of examples. The present invention is not limited to these examples. It should be noted that, below, unless otherwise expressly stated, "%" and "parts" indicating amounts refer to "mass %" and "mass parts". The temperature condition when no particular temperature is specified is room temperature (23°C). The pressure condition when no particular pressure is specified is normal pressure (1 atm).

[0397] <(a) Nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less>

[0398] · "KUAMET NC1-38um" manufactured by Epson Atmix, nanocrystalline magnetic powder composed of Fe-Si-Nb-B alloy, 10% particle size (D 10 )5.8μm, average particle size (D 50 )15.1μm, 90% particle size (D 90)34.7μm, the volume proportion of particles with a particle size of less than 2μm in the magnetic powder is 0.0vol%, the volume proportion of particles with a particle size greater than 2μm and less than 5.5μm in the magnetic powder is 8.6vol%, the volume proportion of particles with a particle size greater than 5.5μm and less than 20μm in the magnetic powder is 56.4Vol%, and the volume proportion of particles with a particle size greater than 20μm in the magnetic powder is 35.0vol%.

[0399] · Epson Atmix's "ATFINE-NC1 PF10FA" is a nanocrystalline magnetic powder made of Fe-Si-Nb-B alloy, with a particle size of 10% (D 10 )3.0μm, average particle size (D 50 )6.0μm, 90% particle size (D 90 )10.7μm, the volume proportion of particles with a particle size of less than 2μm in the magnetic powder is 2.5vol%, the volume proportion of particles with a particle size greater than 2μm and less than 5.5μm in the magnetic powder is 40.2vol%, the volume proportion of particles with a particle size greater than 5.5μm and less than 20μm in the magnetic powder is 57.3vol%, and the volume proportion of particles with a particle size greater than 20μm in the magnetic powder is 0.0vol%.

[0400] <(a') Nanocrystalline magnetic powder having an average particle size exceeding 20 μm>

[0401] · "KUAMET NC1-53um" manufactured by Epson Atmix, nanocrystal composed of Fe-Si-Nb-B alloy, 10% particle size (D 10 )9.8μm, average particle size (D 50 )27.3μm, 90% particle size (D 90 )59.7μm, the volume proportion of particles with a particle size of less than 2μm in the magnetic powder is 0.0vol%, the volume proportion of particles with a particle size greater than 2μm and less than 5.5μm in the magnetic powder is 2.5vol%, the volume proportion of particles with a particle size greater than 5.5μm and less than 20μm in the magnetic powder is 35.4vol%, and the volume proportion of particles with a particle size greater than 20μm in the magnetic powder is 62.1vol%.

[0402] <(b) Magnetic powder having an average particle size of 2 μm or less>

[0403] "M001" manufactured by Powdertech, Fe-Mn ferrite powder (crystalline magnetic powder other than nanocrystalline magnetic powder), 10% particle size (D 10 )0.05μm, average particle size (D 50 )0.12μm, 90% particle size (D 90)1.1μm, the volume proportion of particles with a particle size of less than 2μm in the magnetic powder is 97.0vol%, the volume proportion of particles with a particle size greater than 2μm and less than 5.5μm in the magnetic powder is 3.0vol%, the volume proportion of particles with a particle size greater than 5.5μm and less than 20μm in the magnetic powder is 0.0vol%, and the volume proportion of particles with a particle size greater than 20μm in the magnetic powder is 0.0vol%.

[0404] · "CVD iron powder (0.7 μm)" manufactured by JFE MINERAL, Fe-Si-Cr alloy powder (crystalline magnetic powder other than nanocrystalline magnetic powder), 10% particle size (D 10 )0.46μm, average particle size (D 50 )0.75μm, 90% particle size (D 90 )1.12μm, the volume proportion of particles with a particle size of less than 2μm in the magnetic powder is 100.0vol%, the volume proportion of particles with a particle size greater than 2μm and less than 5.5μm in the magnetic powder is 0.0vol%, the volume proportion of particles with a particle size greater than 5.5μm and less than 20μm in the magnetic powder is 0.0vol%, and the volume proportion of particles with a particle size greater than 20μm in the magnetic powder is 0.0vol%.

[0405] <(c) Magnetic powder having an average particle size of more than 2 μm and less than 20 μm and smaller than that of component (a)>

[0406] · “ATFINE-NC1 PF5FA” manufactured by Epson Atmix, Fe-Si-Nb-B alloy powder (nanocrystalline magnetic powder with an average particle size of less than 5.5 μm), 10% particle size (D 10 )2.3μm, average particle size (D 50 )4.3μm, 90% particle size (D 90 )7.1μm, the volume proportion of particles with a particle size of less than 2μm in the magnetic powder is 6.9vol%, the volume proportion of particles with a particle size greater than 2μm and less than 5.5μm in the magnetic powder is 77.1vol%, the volume proportion of particles with a particle size greater than 5.5μm and less than 20μm in the magnetic powder is 16.0vol%, and the volume proportion of particles with a particle size greater than 20μm in the magnetic powder is 0.0vol%.

[0407] · “ATFINE-NC1 PF3FA” manufactured by Epson Atmix, Fe-Si-Nb-B alloy powder (nanocrystalline magnetic powder with an average particle size of less than 5.5 μm), 10% particle size (D 10 )2.0μm, average particle size (D 50 )3.5μm, 90% particle size (D 90)5.8μm, the volume proportion of particles with a particle size of less than 2μm in the magnetic powder is 10.4vol%, the volume proportion of particles with a particle size greater than 2μm and less than 5.5μm in the magnetic powder is 73.6vol%, the volume proportion of particles with a particle size greater than 5.5μm and less than 20μm in the magnetic powder is 16.0vol%, and the volume proportion of particles with a particle size greater than 20μm in the magnetic powder is 0.0vol%.

[0408] · Epson Atmix's "AW2-08PF3F", Fe-Si-Cr alloy powder (amorphous powder), 10% particle size (D 10 )1.7μm, average particle size (D 50 )3.1μm, 90% particle size (D 90 )5.2μm, the volume proportion of particles with a particle size of less than 2μm in the magnetic powder is 13.9vol%, the volume proportion of particles with a particle size greater than 2μm and less than 5.5μm in the magnetic powder is 72.1vol%, the volume proportion of particles with a particle size greater than 5.5μm and less than 20μm in the magnetic powder is 14.0vol%, and the volume proportion of particles with a particle size greater than 20μm in the magnetic powder is 0.0vol%.

[0409] <Example 1>

[0410] 103.5 parts by mass of (a) nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less ("KUAMET NC1-38um" manufactured by Epson Atmix Co., Ltd., an average particle size (D 50 ) 15.1 μm), 24.6 parts by mass of (b) magnetic powder having an average particle size of 2 μm or less ("M001" manufactured by Powdertech), an average particle size (D 50 ) 0.12 μm), 11.8 parts by mass of (c) a magnetic powder having an average particle size greater than 2 μm and less than 20 μm and smaller than the average particle size of the component (a) ("AW2-08PF3F" manufactured by Epson Atmix), an average particle size (D 50)3.1μm), 0.9 mass parts of (D) epoxy resin ("ZX-1059" manufactured by Nippon Steel Chemical Materials Co., Ltd., a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin), 0.9 mass parts of (D) epoxy resin ("630" manufactured by Mitsubishi Chemical Corporation, a glycidyl ether type aromatic epoxy resin), 0.2 mass parts of (E) curing accelerator ("2MZA-PW" manufactured by Shikoku Chemical Co., Ltd., an imidazole-based curing accelerator), 0.5 mass parts of (F) dispersant ("SC-1015F" manufactured by NOF Corporation, a polyoxyalkylene-based dispersant) and 3.8 mass parts of (H) solvent ("Butyl carbitol acetate" manufactured by Tokyo Chemical Industry Co., Ltd., a solvent) were mixed and uniformly dispersed using a high-speed rotating mixer to prepare a resin composition.

[0411] <Example 2>

[0412] The amount of (a) nanocrystalline magnetic powder ("KUAMET NC1-38um" manufactured by Epson Atmix) having an average particle size of 5.5 μm or more and 20 μm or less was changed from 103.5 parts by mass to 120.8 parts by mass. In addition, the amount of (b) magnetic powder ("M001" manufactured by Powdertech) having an average particle size of 2 μm or less was changed from 24.6 parts by mass to 21.3 parts by mass. Moreover, 11.8 parts by mass of (c) magnetic powder ("AW2-08PF3F" manufactured by Epson Atmix) having an average particle size greater than 2 μm and less than 20 μm and smaller than the average particle size of the component (a) was not used. Except for the above matters, the resin composition was prepared in the same manner as in Example 1.

[0413] <Example 3>

[0414] The amount of (a) nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less ("KUAMET NC1-38um" manufactured by Epson Atmix) was changed from 103.5 parts by mass to 120.8 parts by mass. In addition, the amount of (b) magnetic powder having an average particle size of 2 μm or less was changed from 24.6 parts by mass of "M001" manufactured by Powdertech to 14.4 parts by mass of "CVD iron powder (0.7 μm)" manufactured by JFE MINERAL (average particle size (D 50 )0.75 μm). In addition, the amount of (c) magnetic powder ("AW2-08PF3F" manufactured by Epson Atmix) having an average particle size greater than 2 μm and less than the average particle size of component (a) was changed from 11.8 parts by mass to 14.4 parts by mass. Except for the above matters, the same operation as in Example 1 was carried out to prepare a resin composition.

[0415] <Example 4>

[0416] 56.0 parts by mass of (a) nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less (“ATFINE-NC1 PF10FA” manufactured by Epson Atmix Co., Ltd.), an average particle size (D 50 ) 6.0μm), 18.2 parts by mass of (b) magnetic powder having an average particle size of less than 2μm ("CVD iron powder (0.7μm)" manufactured by JFE MINERAL), 0.8 parts by mass of (D) epoxy resin ("ZX-1059" manufactured by Nippon Steel Chemical Materials Co., Ltd.), 0.8 parts by mass of (D) epoxy resin ("630" manufactured by Mitsubishi Chemical Corporation, glycidyl ether type aromatic epoxy resin), 0.2 parts by mass of (E) curing accelerator ("2MZA-PW" manufactured by Shikoku Chemical Co., Ltd., imidazole-based curing accelerator), 0.4 parts by mass of (F) dispersant ("SC-1015F" manufactured by NOF Corporation, polyoxyalkylene-based dispersant) and 3.1 parts by mass of (H) solvent ("Butyl carbitol acetate" manufactured by Tokyo Chemical Industry Co., Ltd., solvent) were mixed and uniformly dispersed using a high-speed rotary mixer to prepare a resin composition.

[0417] <Example 5>

[0418] 53.1 parts by mass of (a) nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less ("KUAMET NC1-38um" manufactured by Epson Atmix), 6.3 parts by mass of (b) magnetic powder having an average particle size of 2 μm or less ("CVD iron powder (0.7 μm)" manufactured by JFE MINERAL), 6.7 parts by mass of (c) magnetic powder having an average particle size of greater than 2 μm and less than 20 μm and smaller than the average particle size of the component (a) ("ATFINE-NC1PF5FA" manufactured by Epson Atmix), and an average particle size (D 50)4.3μm, nanocrystalline magnetic powder with an average particle size of less than 5.5μm), 0.8 mass parts of (D) epoxy resin ("ZX-1059" manufactured by Nippon Steel Chemical Materials Co., Ltd.), 0.8 mass parts of (D) epoxy resin ("630" manufactured by Mitsubishi Chemical Corporation, glycidyl ether type aromatic epoxy resin), 0.1 mass parts of (E) curing accelerator ("2MZA-PW" manufactured by Shikoku Chemical Co., Ltd., imidazole-based curing accelerator), 0.4 mass parts of (F) dispersant ("SC-1015F" manufactured by NOF Corporation, polyoxyalkylene-based dispersant) and 2.0 mass parts of (H) solvent ("Butyl carbitol acetate" manufactured by Tokyo Chemical Industry Co., Ltd., solvent) were mixed and uniformly dispersed using a high-speed rotating mixer to prepare a resin composition.

[0419] <Example 6>

[0420] 49.1 parts by mass of (a) nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less ("KUAMET NC1-38um" manufactured by Epson Atmix), 10.1 parts by mass of (b) magnetic powder having an average particle size of 2 μm or less ("CVD iron powder (0.7 μm)" manufactured by JFE MINERAL), and 6.3 parts by mass of (c) spherical magnetic powder having an average particle size greater than 2 μm and less than 20 μm and smaller than the average particle size of the component (a) (Epson The resin composition was prepared by mixing 0.8 parts by mass of (D) epoxy resin (“AW2-08PF3F” manufactured by Atmix Co., Ltd.), 0.8 parts by mass of (D) epoxy resin (“ZX-1059” manufactured by Nippon Steel Chemical Materials Co., Ltd.), 0.8 parts by mass of (D) epoxy resin (“630” manufactured by Mitsubishi Chemical Corporation, glycidyl ether type aromatic epoxy resin), 0.1 parts by mass of (E) curing accelerator (“2MZA-PW” manufactured by Shikoku Chemical Co., Ltd., imidazole-based curing accelerator), 0.4 parts by mass of (F) dispersant (“SC-1015F” manufactured by NOF Corporation, polyoxyalkylene-based dispersant) and 1.8 parts by mass of (H) solvent (“Butyl carbitol acetate” manufactured by Tokyo Chemical Industry Co., Ltd., solvent), and uniformly dispersing the mixture using a high-speed rotary mixer.

[0421] <Comparative Example 1>

[0422] A resin composition was prepared in the same manner as in Example 1 except that 24.6 parts by mass of (b) magnetic powder having an average particle size of 2 μm or less (“M001” manufactured by Powdertech) was not used.

[0423] <Comparative Example 2>

[0424] 105.1 parts by mass of (a') nanocrystalline magnetic powder having an average particle size of more than 20 μm ("KUAMET NC1-53um" manufactured by Epson Atmix Co., Ltd., an average particle size (D 50 ) 27.3 μm), 13.1 parts by mass of (b) a magnetic powder having an average particle size greater than 2 μm and less than 20 μm and smaller than that of (A) ("M001" manufactured by Powdertech), and 13.1 parts by mass of (c) a spherical magnetic powder having an average particle size greater than 2 μm and less than 20 μm and smaller than that of the average particle size of the component (a) (Epson A resin composition was prepared by mixing 1.0 parts by mass of (D) epoxy resin (“AW2-08PF3F” manufactured by Atmix Co., Ltd.), 1.0 parts by mass of (D) epoxy resin (“ZX-1059” manufactured by Nippon Steel Chemical Materials Co., Ltd.), 1.0 parts by mass of (D) epoxy resin (“630” manufactured by Mitsubishi Chemical Corporation, a glycidyl ether type aromatic epoxy resin), 0.2 parts by mass of (E) curing accelerator (“2MZA-PW” manufactured by Shikoku Chemical Co., Ltd., an imidazole-based curing accelerator), 0.5 parts by mass of (F) dispersant (“SC-1015F” manufactured by NOF Corporation, a polyoxyalkylene-based dispersant), and 4.0 parts by mass of (H) solvent (“Butyl carbitol acetate” manufactured by Tokyo Chemical Industry Co., Ltd., a solvent), and uniformly dispersing the mixture using a high-speed rotary mixer.

[0425] <Comparative Example 3>

[0426] Instead of using 103.5 parts by mass of (a) nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less (“KUAMET NC1-38um” manufactured by Epson Atmix), 103.5 parts by mass of (c) magnetic powder having an average particle size of greater than 2 μm and less than 20 μm and smaller than the average particle size of the component (a) (“ATFINE-NC1 PF3FA” manufactured by Epson Atmix), an average particle size (D 50 )3.5μm, and nanocrystalline magnetic powder with an average particle size of less than 5.5μm), the same operation as in Example 1 was carried out to prepare a resin composition.

[0427] <Comparative Example 4>

[0428] A resin composition was prepared in the same manner as in Comparative Example 1, except that the amount of (c) magnetic powder ("AW2-08PF3F" manufactured by Epson Atmix) having an average particle size greater than 2 μm and less than the average particle size of component (a) was changed from 11.8 parts by mass to 23.0 parts by mass.

[0429] <Volume ratio of particles with a particle size of 5.5 μm or more and 20 μm or less, volume ratio of magnetic powder with a particle size of 2 μm or less, volume ratio of particles with a particle size of more than 2 μm and less than 5.5 μm, volume ratio of particles with a particle size of more than 20 μm, 10% particle size (D 10 ), average particle size (D 50 ) and 90% particle size (D 90 ) >

[0430] The magnetic powder was dispersed in pure water using ultrasound as the measurement sample, and the particle size distribution of the magnetic powder was prepared on a volume basis using a laser diffraction scattering particle size distribution measuring device ("LA-960" manufactured by Horiba, Ltd.). Based on the particle size distribution, the volume ratio of magnetic powder with a particle size of 5.5 μm or more and 20 μm or less, the volume ratio of magnetic powder with a particle size of 2 μm or less, the volume ratio of particles with a particle size of more than 2 μm and less than 5.5 μm, the volume ratio of particles with a particle size of more than 20 μm, the 10% particle size (D 10 )、50% particle size (average particle size) (D 50 ) and 90% particle size (D 90 ).

[0431] <Test Example 1: Evaluation of coating properties of resin composition>

[0432] The resin compositions prepared in the examples and comparative examples were evaluated for coating properties. As a support, a polyethylene terephthalate (PET) film ("PET501010" manufactured by LINTEC, thickness 50 μm) treated with a silicone release agent was prepared. Each resin composition was evenly applied on the release surface of the PET film using a scraper so that the thickness of the dried resin composition layer was 100 μm, thereby obtaining a resin sheet. The fluidity of the resin composition was confirmed, and the coating properties were evaluated according to the following evaluation criteria.

[0433] (Evaluation criteria for coating properties)

[0434] “○”: The resin composition is in a fluid paste state and has coating properties;

[0435] “×”: The resin composition has no fluidity and cannot be applied.

[0436] <Test Example 2: Measurement and Evaluation of Relative Magnetic Permeability>

[0437] In Examples and Comparative Examples other than Comparative Example 1, the relative magnetic permeability (μ') was measured by the following method.

[0438] The resin sheet obtained in Test Example 1 was heated at 190°C for 90 minutes to thermally cure the resin composition layer, and the support was peeled off to obtain a sheet-like cured product. The obtained cured product was cut into test pieces with a width of 5 mm and a length of 18 mm to obtain an evaluation sample. For the evaluation sample, a measuring device (manufactured by Agilent Technologies, "HP8362B") was used, and the measuring frequency was set to 10 MHz by a 3-turn coil method, and the relative magnetic permeability (μ') was measured at room temperature of 23°C. The relative magnetic permeability was evaluated according to the following evaluation criteria.

[0439] The resin composition obtained in Comparative Example 1 had poor coating properties, and therefore a resin sheet could not be produced by the same method as in other Examples and Comparative Examples. Therefore, in Comparative Example 1, the relative magnetic permeability (μ') was measured by the following method.

[0440] 3 wt% of a solvent ("Butyl Carbitol Acetate" manufactured by Tokyo Chemical Industry Co., Ltd., solvent) was added to the resin composition prepared in Comparative Example 1, and the mixture was evenly dispersed using a high-speed rotary mixer to obtain a varnish. As a support, a polyethylene terephthalate (PET) film ("PET501010" manufactured by LINTEC, thickness 50 μm) treated with a silicone-based release agent was prepared. The varnish was evenly applied on the release surface of the PET film using a scraper so that the thickness of the resin composition layer after drying was 100 μm, thereby obtaining a resin sheet. Using the resin sheet, a sheet-like cured product was prepared using the same method as in the embodiments and comparative examples other than Comparative Example 1, and the relative magnetic permeability (μ') was measured. The relative magnetic permeability was evaluated according to the following evaluation criteria.

[0441] (Evaluation criteria for relative magnetic permeability)

[0442] “○”: relative magnetic permeability is greater than 25;

[0443] “×”: Relative magnetic permeability is less than 25.

[0444] <Test Example 3: Measurement and Evaluation of Loss Coefficient (tanδ)>

[0445] The sheet-like cured product obtained in Test Example 2 was cut into test pieces with a width of 5 mm and a length of 18 mm to obtain an evaluation sample. For the evaluation sample, a measuring device (manufactured by Agilent Technologies, "HP8362B") was used, and the measuring frequency was set to 10 MHz by the 3-turn coil method, and the magnetic loss (μ") was obtained at room temperature 23°C. The loss coefficient tanδ is calculated by the formula "tanδ=μ" / μ'". The loss coefficient (tanδ) was evaluated according to the following evaluation criteria.

[0446] (Evaluation criteria for loss coefficient (tanδ))

[0447] “○”: loss coefficient (tanδ) is less than 0.1;

[0448] "×": The loss coefficient (tan δ) exceeds 0.1.

[0449] <Results>

[0450] The components and contents of the resin compositions of the embodiments and comparative examples, as well as the measurement results and evaluation results of the test examples are shown in the following table. In the following table, the content (mass % and volume %) of the total amount of components (a) to (c), components (A) to (C) and magnetic powder represents the value when the non-volatile component in the resin composition is set to 100%.

[0451] [Table 1]

[0452] [Table 1. Results of Example]

[0453]

[0454] [Table 2]

[0455] [Table 2. Results of Comparative Example]

[0456]

[0457] ※Due to poor coating, a resin sheet could not be produced by the same method as other examples and comparative examples in Comparative Example 1. For reference, a resin sheet was produced by a method different from other examples and comparative examples and evaluated.

[0458] Explanation of symbols

[0459] 1. Circuit board;

[0460] 10-core substrate;

[0461] 11 supporting substrate;

[0462] 12 1st metal layer;

[0463] 13 2nd metal layer;

[0464] 14 through holes;

[0465] 20 electroplating layer;

[0466] 21 The surface surrounding the grinding surface;

[0467] 30 solidified material;

[0468] 30a resin composition;

[0469] 31: a ground surface of the solidified material (ground surface);

[0470] 40 conductor layer;

[0471] 41 pattern conductor layer;

[0472] 100 circuit substrate;

[0473] 200 inner substrate;

[0474] 200a a first main surface;

[0475] 200b a second main surface;

[0476] 220 through hole;

[0477] 220a: wiring in through hole;

[0478] 240 external terminals;

[0479] 310 resin sheet;

[0480] 320 first cured material layer;

[0481] 320a resin composition layer;

[0482] 330 support body;

[0483] 360 vias;

[0484] 360a Routing in vias;

[0485] 400 Coil-shaped conductive structure;

[0486] 420 first conductor layer;

[0487] 420a pad;

[0488] 440: second conductor layer.

Claims

1. A resin composition comprising the following ingredients: (A) nanocrystalline magnetic powder having a particle size of 5.5 μm or more and 20 μm or less; (B) magnetic powder having a particle size of 2 μm or less; and (D) thermosetting resin, in, The amount of the component (A) is 23% by volume or more and 60% by volume or less relative to 100% by volume of the non-volatile component of the resin composition, The amount of the component (B) is 5% by volume or more and 30% by volume or less relative to 100% by volume of the nonvolatile component of the resin composition.

2. The resin composition according to claim 1, wherein The volume ratio of the component (A) to the component (B) (component (A) / component (B)) is 1 or more and 12 or less.

3. The resin composition according to claim 1, further comprising (C) magnetic powder, in, The (C) magnetic powder is a magnetic powder other than the above-mentioned (A) component and has a particle size of more than 2 μm and 20 μm or less.

4. The resin composition according to claim 1, wherein The component (D) contains an epoxy resin. The resin composition according to claim 1 , further comprising (E) a curing accelerator.

6. The method for producing the resin composition according to claim 1, comprising mixing the following components: (a) nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less; (b) magnetic powder having an average particle size of 2 μm or less; and (D) Thermosetting resin.

7. A method for producing a resin composition, comprising mixing the following ingredients: (a) nanocrystalline magnetic powder having an average particle size of 5.5 μm or more and 20 μm or less; (b) magnetic powder having an average particle size of 2 μm or less; and (D) Thermosetting resin.

8. The method for producing a resin composition according to claim 6 or 7, wherein: The amount of the component (a) is 30% by volume or more and 80% by volume or less relative to 100% by volume of the nonvolatile component of the resin composition.

9. The method for producing a resin composition according to claim 6 or 7, wherein: (a) 10% particle size D of component 10 Greater than 2μm.

10. The method for producing a resin composition according to claim 6 or 7, wherein: The amount of the component (b) is 5% by volume or more and 50% by volume or less relative to 100% by volume of the nonvolatile component of the resin composition.

11. The method for producing a resin composition according to claim 6 or 7, wherein: (b) 90% particle size D of the component 90 Less than 5.5μm.

12. The method for producing a resin composition according to claim 6 or 7, further comprising mixing (c) magnetic powder, in, (c) The magnetic powder has an average particle size of more than 2 μm and less than 20 μm, and smaller than the average particle size of the component (a).

13. The method for producing a resin composition according to claim 12, wherein: The amount of the (c) magnetic powder is 34% by volume or less relative to 100% by volume of the non-volatile component of the resin composition.

14. A cured product of the resin composition according to any one of claims 1 to 5.

15. A resin sheet comprising: a support and a resin composition layer formed on the support, in, The resin composition layer contains the resin composition according to any one of claims 1 to 5.

16. A method for producing a resin sheet, comprising the following steps: A step of producing a resin composition by the production method according to claim 6 or 7; and A step of applying the resin composition onto a support. 17 . A circuit board comprising a cured product of the resin composition according to claim 1 . 18 . The circuit board according to claim 17 , comprising: a substrate having through holes formed therein; and a cured product of the resin composition filled in the through holes.