Glass cloth, prepreg and printed circuit board
Through water cleaning with low sodium ion content and high-temperature heating deoiling treatment, the problems of reduced strength of glass cloth and increased dielectric loss tangent are solved, and the efficient insulation and heat resistance of the printed circuit board are achieved.
Patent Information
- Application Number
- CN202380025469.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-08
- Filing Date
- 2023-03-07
- Publication Date
- 2024-10-22
AI Technical Summary
The existing technology has deficiencies in improving the dielectric properties and heat resistance of printed circuit board glass cloth. In particular, the method of reducing the strength of the glass cloth and increasing the dielectric loss tangent has not been fully solved, and the fracture and heat resistance caused by high-temperature heating treatment have not been fully solved. Wrinkle problems are inevitable.
By using water with a sodium ion content of less than 20 ppm to clean the glass cloth, and performing a heating and deoiling process above 700°C, the devitrification phenomenon of quartz glass is suppressed, the strength of the glass cloth is maintained, and the dielectric loss tangent is reduced.
It achieves the stabilization of the unit area weight of the glass cloth at high temperatures, reduces the dielectric loss tangent, reduces the breakage and wrinkles of the glass cloth, and improves the insulation and heat resistance of the printed circuit board.
Smart Images

Figure BDA0005026892700000371 
Figure BDA0005026892700000381 
Figure BDA0005026892700000391
Abstract
Description
Technical Field
[0001] The invention relates to glass cloth, prepreg and printed circuit board. Background Art
[0002] At present, the high performance of information terminals such as smart phones and the high-speed communication represented by 5G communication are developing. Along with this background, especially for high-speed communication printed circuit boards, it is not only expected to improve the heat resistance required all the time, but also expected to further improve the dielectric properties of its insulating materials (for example, low dielectric loss tangent). Similarly, for the prepreg used in the insulating material of the printed circuit board, and the glass filaments and glass cloth contained in the prepreg, there is also a background of expecting to improve dielectric properties.
[0003] In order to achieve low dielectric properties of insulating materials, it is known to use a prepreg made by impregnating glass cloth with a low dielectric resin (hereinafter referred to as "matrix resin") to form an insulating material (Patent Documents 1 and 2). Patent Documents 1 and 2 describe that polyphenylene ethers terminally modified with vinyl or methacryloyloxy groups are advantageous for low dielectric properties and heat resistance, and that the modified polyphenylene ethers are used as matrix resins.
[0004] In addition, in order to improve the dielectric properties of the prepreg, a method of using low dielectric glass to form a prepreg is also known (Patent Document 3). In Patent Document 3, glass filaments with a silicon dioxide (SiO2) composition of 98% by mass to 100% by mass are used. In addition, Patent Document 3 describes a method of using low dielectric glass cloth to form a prepreg, wherein the low dielectric glass cloth is surface treated with a silane coupling agent having an unsaturated double bond group, and has a ignition loss value of 0.12% by mass to 0.40% by mass.
[0005] Here, there are also reports that the silanol groups on the surface of the glass cloth are the cause of the decrease in dielectric properties (Patent Documents 4 and 5). Patent Documents 4 and 5 describe a method of reducing the silanol groups on the surface of the glass cloth by treating the surface of the glass cloth with polysilazane in order to improve the dielectric properties. In addition, Patent Documents 6 and 7 describe reducing the dielectric loss tangent of the quartz glass cloth by performing a heat treatment.
[0006] However, in order to suppress the fuzzing of the glass yarn and prevent water absorption, a sizing agent mainly composed of starch is usually applied to the surface of the glass yarn. In addition, before or after the weaving of the glass yarn or during the weaving process, the glass yarn or glass cloth is washed to reduce the sizing agent (for desizing).
[0007] It should be noted that Patent Documents 8 and 9 report that thermal deoiling can be performed at a relatively low temperature by using a sizing agent for quartz glass fibers containing ammonium nitrate or a sizing agent for quartz glass fibers obtained by nitric esterification of at least a portion of starch.
[0008] In addition, due to the high density of printed circuit boards, the through holes and / or the inner layer wires and through holes become narrower, so that the insulation resistance decreases, and the printed circuit boards are required to have higher reliability than before. One of the reasons for the decrease in insulation resistance of printed circuit boards can be considered to be the influence of copper migration (electrocorrosion). Electrocorrosion is the following phenomenon: in a high humidity environment where voltage is applied, copper as a conductor dissolves and precipitates from the anode, and is connected to the cathode through the insulating material. Electrocorrosion is divided into: dendrites generated in the surface resist and / or adhesive layer, and CAF (Conductive Anodic Filaments) generated at the interface of the inner layer glass fiber and the resin. It is known that the ionic components in the interface of the glass fiber and the resin are one of the reasons for the generation of CAF. Patent document 10 records that the amount of alkali metals and / or alkaline earth metals extracted from the glass cloth composed of E glass is less than 20 ppm, thereby improving the CAF resistance of the printed circuit board. Patent Document 11 describes that after treating the surface of glass cloth with a surface treatment agent containing a coupling agent as the main component, water vapor is sprayed to reduce the amount of calcium ions attached to the surface of the glass cloth and improve CAF resistance. Patent Document 12 describes that a warp paste containing polyvinyl alcohol and / or a polyvinyl alcohol derivative containing an alkali metal compound content of 0.5 wt % or less is used as the main component to improve CAF resistance.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: International Publication No. 2019 / 065940
[0012] Patent Document 2: International Publication No. 2019 / 065941
[0013] Patent Document 3: Japanese Patent Application Publication No. 2018-127747
[0014] Patent Document 4: Japanese Patent Application Publication No. 2020-194888
[0015] Patent Document 5: Japanese Patent Application Publication No. 2021-88488
[0016] Patent Document 6: Japanese Patent Application Publication No. 2021-63320
[0017] Patent Document 7: Japanese Patent Application Publication No. 2021-195689
[0018] Patent Document 8: Japanese Patent Application Publication No. 2016-108162
[0019] Patent Document 9: Japanese Patent Application Publication No. 2016-113322
[0020] Patent Document 10: Japanese Patent Application Publication No. 2001-73253
[0021] Patent Document 11: Japanese Patent Application Publication No. 2005-42245
[0022] Patent Document 12: Japanese Patent Application Laid-Open No. 7-279055 Summary of the invention
[0023] Problem that the invention aims to solve
[0024] However, from the perspective of achieving further improvement in dielectric properties, there is still room for research in Patent Documents 1 and 2. For example, Patent Documents 1 and 2 do not consider the use of low dielectric glass as described in Patent Document 3. In addition, Patent Document 3 describes that glass having a SiO2 composition of 98% by mass to 100% by mass has problems from a practical point of view, and therefore, it is expected to provide another method that uses such glass yarn to appropriately provide glass cloth and further prepreg.
[0025] In the method of reducing the silanol groups present on the surface of glass cloth as disclosed in Patent Documents 4 and 5, the dielectric loss tangent of the quartz glass cloth at 10 GHz was improved by 1.0×10 -3 ~1.0×10 -4, it can be considered that the improvement effect is small. It can be considered that there are also reasons other than the presence of hydroxyl groups on the glass surface that increase the dielectric loss tangent of the glass cloth, and there is still room for improvement. In addition, in the method of reducing the dielectric loss tangent by heating the quartz glass cloth at high temperature as pointed out in Patent Document 6, there is a problem of worrying about the strength of the glass cloth being reduced due to excessive heating treatment. In addition, the glass cloth used for printed circuit boards is usually subjected to surface treatment processing such as silane coupling agents, but the surface treatment processing is not performed in Patent Document 6, and the glass cloth used as a printed circuit board is not practical, so there is still room for improvement. In addition, Patent Document 7 reports a method for restoring the tensile strength of the glass cloth after high-temperature heating treatment by removing the strain layer of quartz glass by etching. However, due to the high-temperature heating treatment, the strength is greatly reduced, so there is a technical problem that the glass cloth is prone to "fracture (tear)" in the strain layer removal process. In addition, the strain layer may not be fully removed in the woven intersection of the glass cloth and / or the twisted part of the glass fiber, which are not easily penetrated by the etching solution. Therefore, there are also technical problems such as uneven tensile strength of glass cloth and / or filament diameter of glass fiber, and wrinkles and tears are easily generated when glass cloth is transported. Furthermore, since the glass is dissolved by etching, there may be a technical problem of excessive reduction in the weight per unit area of glass cloth. The amount of matrix resin in the prepreg, which is called resin content, needs to be accurately controlled, but the etching process in which the weight per unit area of the glass cloth itself varies makes it difficult to control the resin content of the prepreg. Therefore, a processing method that can suppress the variation of the weight per unit area of the glass cloth and uniformly improve the tensile strength of the glass cloth is very necessary.
[0026] As the strength of the glass cloth decreases, the tension control range during the transportation of the glass cloth becomes extremely low and narrow, and "wrinkles" and / or "damage" caused by contact with parts during transportation may occur on the glass cloth. In order to suppress the decrease in the strength of the glass cloth, Patent Documents 8 and 9 describe methods of heating and degreasing the glass cloth at a relatively low temperature. However, there is such a background: in order to further improve the dielectric properties of the glass cloth, it is very necessary to develop a method that can not only suppress the decrease in the strength of the glass cloth but also reduce the dielectric loss tangent of the glass cloth. Therefore, there is also a background that is very necessary for a processing method that can reduce the appearance defects such as breakage and wrinkles of the glass cloth.
[0027] Patent documents 10, 11 and 12 describe methods for reducing alkali metals and / or alkaline earth metals on the glass surface. In the prior art including Patent documents 10, 11 and 12, although reports on alkali metals and / or alkaline earth metals and CAF resistance are reported, sufficient research has not been conducted from the perspective of maintaining the strength of glass cloth. Patent documents 8 and 9 describe that the recrystallization phenomenon known as devitrification of quartz glass fiber due to the presence of alkali metals will significantly reduce the strength of glass, but do not describe how the devitrification phenomenon is suppressed. For glass cloth for printed circuit boards for high-speed communications, it is very necessary to develop technology from the perspective of reducing the dielectric loss tangent of the glass cloth and being able to suppress the decrease in the strength of the glass cloth.
[0028] To this end, the object of the present invention is to provide a low dielectric glass cloth that can suppress the change of unit area weight and has excellent dielectric properties (such as low dielectric loss tangent), less wrinkles and / or damage, and less tearing, and to provide a prepreg containing the glass cloth. In addition, the object of the present invention is to provide a printed circuit board, an integrated circuit and an electronic device that can also achieve an increase in yield by using the prepreg. Furthermore, the object of the present invention is to provide a method for manufacturing a glass cloth for appropriately obtaining the above-mentioned glass cloth.
[0029] Solutions for solving problems
[0030] The inventors of the present invention believe that it is very meaningful to clarify the relationship between the strength of glass cloth and metal ions (including alkali metal ions and / or alkaline earth metal ions) from the perspective of industrial production of glass cloth. In addition, the inventors of the present invention have come up with the idea that by maintaining the strength of quartz glass cloth, sufficient tension can be applied to the glass cloth, which can be used to suppress the occurrence of wrinkles and / or damage during transportation.
[0031] Based on this idea, the inventors of the present invention conducted in-depth research to solve the above technical problems, and as a result, they focused on the amount of sodium ions attached to the glass cloth before the heating deoiling process. And it was found that by washing the glass cloth with water with a sodium ion content of 20 ppm or less, the strength reduction of the glass cloth caused by the devitrification phenomenon of the quartz glass cloth can be suppressed even at a high temperature of 700°C or above, thereby completing the present invention. By suppressing the reduction in the strength of the glass cloth caused by the devitrification phenomenon of the quartz glass, it is easy to control the tension during the transportation of the glass cloth, and it is possible to obtain a glass cloth that can suppress the change in the unit area weight of the glass cloth and has fewer wrinkles and / or damages, and further fewer tears. A part of the method of the present invention is shown below. [1]
[0033] A glass cloth is a glass cloth woven from glass yarns containing a plurality of filaments.
[0034] The bulk dielectric loss tangent of the glass in the glass filament is less than 0.0010,
[0035] The tensile strength of the warp yarn per unit thickness of the glass cloth represented by the following formula (A) is in the range of 0.50 to 6.0, and the coefficient of variation of the tensile strength in the warp yarn direction of the glass cloth is in the range of 15% or less.
[0036] The dielectric loss tangent of the glass cloth at 10 GHz is in a range of greater than 0 and less than 0.0010;
[0037] Formula (A): tensile strength of the glass cloth in the warp direction (N / 25 mm) / thickness of the glass cloth (μm)···(A). [2]
[0039] A glass cloth is a glass cloth woven from glass yarns containing a plurality of filaments.
[0040] The bulk dielectric loss tangent of the glass in the glass filament is less than 0.0010,
[0041] The tensile strength of the warp yarn per unit thickness of the glass cloth represented by the following formula (A) is in the range of 0.50 to 6.0.
[0042] The coefficient of variation of the filament diameter of the glass fibers constituting the glass cloth is within a range of 10% or less,
[0043] The dielectric loss tangent of the glass cloth at 10 GHz is in a range of greater than 0 and less than 0.0010;
[0044] Formula (A): tensile strength of the glass cloth in the warp direction (N / 25 mm) / thickness of the glass cloth (μm)···(A). [3]
[0046] The glass cloth according to item 1 or 2, wherein a dielectric loss tangent of the glass cloth at 10 GHz is in a range of greater than 0 and not more than 0.0055. [4]
[0048] The glass cloth according to any one of items 1 to 3, wherein the silicon (Si) content in the glass filaments is 95.0 to 100% by mass in terms of silicon dioxide (SiO 2 ). [5]
[0050] The glass cloth according to any one of items 1 to 4, wherein the silicon (Si) content in the glass filaments is 99.0 to 100% by mass in terms of silicon dioxide (SiO 2 ). [6]
[0052] The glass cloth according to any one of items 1 to 5, wherein the glass filaments are treated with a surface treatment agent containing a silane coupling agent. [7]
[0054] The glass cloth according to item 6, wherein the surface treatment agent contains the silane coupling agent represented by the following formula (1).
[0055] X(R) 3-n S Y n ···(1)
[0056] (In formula (1), X is an organic functional group having at least one of an amino group and an unsaturated double bond group, the unsaturated double bond group has free radical reactivity, Y is each independently an alkoxy group, n is an integer of 1 to 3, and R is each independently a group selected from the group consisting of a methyl group, an ethyl group, and a phenyl group) [8]
[0058] The glass cloth according to item 7, wherein X in the formula (1) is an organic functional group that does not form a salt with an ionic compound. [9]
[0060] The glass cloth according to item 7 or 8, wherein X in the formula (1) does not contain an amine or an ammonium cation.
[10]
[0062] The glass cloth according to any one of items 7 to 9, wherein X in the formula (1) is an organic functional group having one or more methacryloxy groups or acryloxy groups.
[11]
[0064] The glass cloth according to any one of items 1 to 10, wherein the glass cloth has a loss on ignition of 0.01% by mass or more and less than 0.18% by mass.
[12]
[0066] The glass cloth according to any one of items 1 to 11, wherein a dielectric loss tangent of the glass cloth at 10 GHz is within a range of 0.00050 or less.
[13]
[0068] The glass cloth according to any one of Items 1 to 12, wherein the glass cloth has a thickness of 60 μm or less.
[14]
[0070] The glass cloth according to any one of items 1 to 13, wherein the weight per unit area (g / m 2 ) had a coefficient of variation of less than 3%.
[15]
[0072] The glass cloth according to any one of items 1 to 4, wherein the weight per unit area (g / m 2 ) had a coefficient of variation of less than 1.5%.
[16]
[0074] The glass cloth according to any one of Items 1 to 15, wherein the number of voids after 5 minutes of impregnation with castor oil is 180 or less.
[17]
[0076] The glass cloth according to any one of items 1 to 16, which is used for a printed circuit board.
[18]
[0078] A prepreg comprising the glass cloth according to any one of items 1 to 17, a thermosetting resin and an inorganic filler.
[19]
[0080] A printed circuit board comprising the prepreg according to item 18.
[20]
[0082] An integrated circuit comprising the printed circuit board described in item 19. [twenty one]
[0084] An electronic device comprising the printed circuit board described in item 19. [twenty two]
[0086] A method for producing glass cloth comprises the step of washing the glass cloth with water having a sodium ion content of 20 ppm or less. [twenty three]
[0088] The method for producing a glass cloth according to Item 22, further comprising a step of heating and deoiling the glass cloth after the step of washing the glass cloth. [twenty four]
[0090] The method for producing glass cloth according to Item 23, wherein the step of performing heating deoiling includes a step of performing heating deoiling at 700° C. or higher.
[25]
[0092] The method for producing a glass cloth according to any one of Items 22 to 24, wherein the step of washing the glass cloth includes a step of immersing the glass cloth in water having a sodium ion content of 20 ppm or less.
[26]
[0094] The method for producing a glass cloth according to any one of items 22 to 25, wherein the step of washing the glass cloth includes washing the glass cloth with ultrasonic waves while immersing the glass cloth in water having a sodium ion content of 20 ppm or less.
[27]
[0096] The method for producing a glass cloth according to any one of items 22 to 26, wherein the step of washing the glass cloth includes a step of washing the glass cloth with water having a sodium ion content of 20 ppm or less using a sprayer.
[28]
[0098] The method for producing a glass cloth according to any one of items 22 to 27, wherein the step of washing the glass cloth includes a step of washing the glass cloth with water having a sodium ion content of 20 ppm or less while conveying the glass cloth.
[29]
[0100] The method for producing a glass cloth according to any one of items 22 to 28, comprising the steps of washing the glass cloth with water having a sodium ion content of 20 ppm or less while conveying the glass cloth and heating the glass cloth at a temperature of 700° C. or higher.
[30]
[0102] The method for producing a glass cloth according to any one of items 22 to 29, wherein the content of silicon (Si) in the glass yarns constituting the glass cloth is 95.0 to 100% by mass in terms of silicon dioxide (SiO 2 ).
[0103] Effects of the Invention
[0104] According to the present invention, it is possible to provide: a low dielectric glass cloth having excellent dielectric properties (e.g., low dielectric loss tangent) and less appearance defects while being able to suppress the change in weight per unit area, and a prepreg containing the glass cloth. In addition, the present invention can also provide a printed circuit board, an integrated circuit, and an electronic device that can also achieve improved productivity by using the prepreg. Furthermore, according to the present invention, it is also possible to provide a method for manufacturing a glass cloth for appropriately obtaining the above-mentioned glass cloth. DETAILED DESCRIPTION
[0105] Hereinafter, an embodiment of the present invention (hereinafter referred to as "the present embodiment") is described, but the present invention is not limited thereto and can be variously modified within the scope of the subject matter thereof. In the present embodiment, the numerical range recorded using "~" represents a numerical range that includes the numerical values before and after "~" as the lower limit and the upper limit. In addition, in the present embodiment, in the numerical range recorded in a stepwise manner, the upper limit or lower limit recorded in a certain numerical range can be replaced by the upper limit or lower limit of other numerical ranges recorded in a stepwise manner. Moreover, in the present embodiment, the upper limit or lower limit recorded in a certain numerical range can also be replaced by the value shown in the embodiment. Moreover, in the present embodiment, the term "process" not only refers to an independent process, but also is included in the term as long as the function of the process can be achieved even if it cannot be clearly distinguished from other processes.
[0106] [Glass cloth]
[0107] 〔Overall composition〕
[0108] The glass cloth of this embodiment is a glass cloth formed by weaving glass yarns.
[0109] The bulk dielectric loss tangent of the glass in the glass filament is less than 0.0010.
[0110] The tensile strength of the warp yarn per unit thickness of the glass cloth represented by the following formula (A) is in the range of 0.50 to 6.0.
[0111] The coefficient of variation (CV: Coefficient of Variation) of the tensile strength in the warp direction of the glass cloth is within the range of 15% or less.
[0112] The dielectric loss tangent of the glass cloth at 10 GHz is in the range of greater than 0 and less than 0.0010;
[0113] Formula (A): tensile strength of glass cloth in the warp direction (N / 25 mm) / thickness of glass cloth (μm)...(A).
[0114] Thus, it is possible to provide a glass cloth and a prepreg which can suppress the variation in weight per unit area, have excellent dielectric properties (for example, low dielectric loss tangent) and have few appearance defects.
[0115] In addition, as described in Examples, it can be confirmed that the variation in the weight per unit area of the glass cloth can be suppressed by the coefficient of variation of the weight per unit area of the glass cloth being equal to or less than a predetermined value.
[0116] It should be noted that the concept of “being able to suppress the variation of the weight per unit area” in this specification also includes that the weight per unit area does not vary.
[0117] The glass cloth of this embodiment can be woven by glass yarns (for example, glass yarns composed of multiple glass filaments) as warp yarns and weft yarns. The weaving structure of the glass cloth can be, for example, plain weave, basket weave, satin weave, twill weave, etc. Among them, the plain weave structure is preferred.
[0118] The insertion density of the warp and weft yarns constituting the glass cloth of this embodiment is preferably 10 to 120 yarns / inch (= 10 to 120 yarns / 25 mm), and more preferably 40 to 100 yarns / inch. If the insertion density is within the above range, the effect of the present invention is easily obtained. The insertion density of the warp and weft yarns may be different.
[0119] The weight per unit area (mass of the glass cloth) of the present embodiment is preferably 8 to 250 g / m 2 , more preferably 8 to 100 g / m 2 , more preferably 8 to 80 g / m 2 , particularly preferably 8 to 50 g / m 2 When the weight per unit area of the glass cloth is within the above range, the effects of the present invention can be easily obtained.
[0120] The coefficient of variation (CV: Coefficient of Variation) of the unit area weight of the glass cloth of this embodiment is preferably 3% or less, more preferably 1.5% or less, further preferably 1.3% or less, further preferably 1% or less, and particularly preferably 0.9% or less. If the coefficient of variation of the unit area weight of the glass cloth is within the above range, the tensile strength of the glass cloth will vary less, and it is easy to obtain a glass cloth with excellent appearance. In addition, it is also greatly advantageous in that the resin content of the prepreg can be easily controlled. The lower limit of the coefficient of variation is theoretically 0.
[0121] In the present embodiment, the tensile strength in the warp direction of the glass cloth per unit thickness is preferably in the range of 0.50 or more, more preferably in the range of 0.52 or more, further preferably in the range of 0.54 or more, further preferably in the range of 0.56 or more, and particularly preferably in the range of 0.58 or more. When the tensile strength in the warp direction of the glass cloth per unit thickness is less than 0.50, the tension applied during transportation of the glass cloth cannot be sufficiently applied, and thus wrinkles and / or damage caused by accidental contact with equipment, etc. are easily generated. The tensile strength in the warp direction of the glass cloth per unit thickness may be 6.0 or less, 5.0 or less, 4.0 or less, 3.5 or less, or 3.0 or less.
[0122] The coefficient of variation of the tensile strength in the warp direction of the glass cloth of this embodiment is preferably less than 15%, more preferably less than 10%, further preferably less than 7%, further preferably less than 5%, and particularly preferably less than 3%. When the coefficient of variation of the tensile strength is greater than 15%, wrinkles and the like are easily generated on the glass cloth when the glass cloth is transported.
[0123] Another aspect of the glass cloth of the present embodiment is a glass cloth obtained by weaving glass yarns including a plurality of filaments.
[0124] The bulk dielectric loss tangent of the glass in the glass filament is less than 0.0010.
[0125] The tensile strength of the warp yarn per unit thickness of the glass cloth represented by the following formula (A) is in the range of 0.50 to 6.0.
[0126] The coefficient of variation of the filament diameter of the glass fibers constituting the glass cloth is within the range of 10% or less.
[0127] The dielectric loss tangent of the glass cloth at 10 GHz is in the range of greater than 0 and less than 0.0010;
[0128] Formula (A): tensile strength of glass cloth in the warp direction (N / 25 mm) / thickness of glass cloth (μm)...(A).
[0129] Thus, it is possible to provide a glass cloth and a prepreg which can suppress the variation in weight per unit area, have excellent dielectric properties and have few appearance defects.
[0130] The coefficient of variation of the filament diameter is preferably less than 10%, more preferably less than 7%, further preferably less than 5%, further preferably less than 4%, and particularly preferably less than 3%. When the coefficient of variation of the filament diameter of the glass fiber is greater than 10%, wrinkles are easily generated on the glass cloth when the glass cloth is transported.
[0131] The coefficient of variation of the tensile strength in the warp direction and the coefficient of variation of the filament diameter can be obtained by the following formulae, respectively.
[0132] (Standard deviation of tensile strength in warp direction / average tensile strength in warp direction)×100
[0133] (Standard deviation of filament diameter / average filament diameter)×100
[0134] The average tensile strength is the average value of the tensile strengths in the warp direction of the glass cloth at 5 locations, and the average filament diameter is the average value of the filament diameters at 10 locations. The values of the tensile strength obtained at a plurality of locations and the values of the filament diameter obtained at a plurality of locations can be used to calculate the standard deviation of the tensile strength and the standard deviation of the filament diameter, respectively.
[0135] The tensile strength of the glass cloth with a small coefficient of variation in the warp direction or the unevenness of the filament diameter is relatively low, so it becomes a glass cloth with high uniformity and less appearance defects. The lower limit of the coefficient of variation is theoretically 0. The coefficient of variation can be controlled by adjusting the amount of sodium ions attached to the surface of the glass cloth before the heating and degreasing treatment (using high-purity cleaning water to clean the surface of the glass cloth to adjust the amount of sodium ions). For example, the above coefficient of variation can be controlled by controlling the immersion time (seconds) of the grey cloth in the cleaning water containing sodium ions. By ensuring that the immersion time (seconds) is the specified time, it is easy to fully obtain the cleaning effect brought by the cleaning solution, so it is easy to exert the effect of this embodiment.
[0136] The thickness of the glass cloth of this embodiment is preferably 60 μm or less, more preferably 55 μm or less, and further preferably 50 μm or less. If the thickness of the glass cloth is within the above range, the effect of the present invention is easily obtained. The thickness of the glass cloth may be greater than 0, 5 μm or more, or 5 μm or more.
[0137] 〔Glass Fiber〕
[0138] The glass filaments constituting the glass cloth of the present embodiment can be obtained by using low dielectric glass as a raw material. Specifically, regarding the glass filaments, the Si content in the glass filaments is in the range of 95.0 to 100% by mass in terms of SiO2. By using such glass filaments, for example, the dielectric properties of the obtained glass cloth can be improved. From the viewpoint of improving the dielectric properties of the obtained glass cloth, the Si content is preferably in the range of 99.0 to 100% by mass, more preferably in the range of 99.5 to 100% by mass, and further preferably in the range of 99.9 to 100% by mass.
[0139] When glass containing 99.0 mass % or more in terms of SiO2 is in the form of a bulk body having a certain thickness, its dielectric loss tangent (bulk dielectric loss tangent) generally shows the relationship represented by the following formula (2).
[0140] Bulk dielectric loss tangent ≤1.2×10 -3 ···(2)
[0141] The average filament diameter of the glass filaments constituting the glass yarn is preferably 2.5 to 9.0 μm, more preferably 2.5 to 7.5 μm, further preferably 3.5 to 7.0 μm, further preferably 3.5 to 6.0 μm, and particularly preferably 3.5 to 5.0 μm. When the filament diameter is less than the above value, the breaking strength of the filament becomes low, so the obtained glass cloth is prone to produce fuzz. In addition, when the filament diameter exceeds the above value, the mass of the glass cloth becomes large, so it is difficult to transport or process. In addition, if the average filament diameter of the glass filaments is within the above range, the effect of the present invention is easily obtained.
[0142] 〔Silane coupling agent〕
[0143] The glass yarn (including glass filaments) constituting the glass cloth is preferably surface treated with a silane coupling agent. That is, in one embodiment, the surface treatment agent for the glass yarn includes a silane coupling agent. As the silane coupling agent, for example, a silane coupling agent represented by the following formula (1) is preferably used.
[0144] X(R) 3-n S Y n ···(1)
[0145] {In formula (1), X is an organic functional group including at least one of an unsaturated double bond group having free radical reactivity and an amino group, wherein the unsaturated double bond group is a carbon-carbon double bond having free radical reactivity, etc., Y is each independently an alkoxy group, n is an integer of 1 to 3, and R is a group selected from the group consisting of methyl, ethyl and phenyl}
[0146] This embodiment focuses on the reasons why the dielectric loss tangent of conventional glass cloth increases:
[0147] (i) a very small amount of thermally oxidized degraded product of the sizing agent remaining in a state of being physically attached to the surface of the glass yarn, and
[0148] (ii) Residues of the surface treatment agent or modified products thereof which do not form a chemical bond with the glass surface but are physically attached and cannot be removed by washing with water.
[0149] From the viewpoint of suppressing the generation of (i) thermal oxidation degradation products and / or (ii) residues or modified products, X in the general formula (1) is preferably an organic functional group that does not form a salt with an ionic compound. In addition, from the viewpoint of reactivity with the matrix resin, X in the general formula (1) is more preferably an organic functional group having one or more methacryloyloxy groups or acryloyloxy groups. It should be noted that from the viewpoint of easily showing the effects of the present invention, X in the general formula (1) preferably does not contain amines such as primary amines, secondary amines, tertiary amines, or ammonium cations such as quaternary ammonium cations.
[0150] Regarding Y in the above formula (1), the alkoxy group is preferably an alkoxy group having 1 to 5 carbon atoms (1, 2, 3, 4 or 5 carbon atoms) in order to achieve stable treatment of the glass cloth.
[0151] As the surface treatment agent, the silane coupling agent represented by formula (1) may be used alone or two or more silane coupling agents having different X in formula (1) may be used in combination. In addition, as the silane coupling agent represented by formula (1), for example, a single component such as vinyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, acryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 5-hexenyltrimethoxysilane, or a mixture thereof may be used.
[0152] The molecular weight of the silane coupling agent is preferably 100 to 600, more preferably 150 to 500, and further preferably 200 to 450. Among them, it is particularly preferred to use two or more silane coupling agents with different molecular weights. By treating the surface of the glass filament with two or more silane coupling agents with different molecular weights, the density of the treatment agent on the glass surface increases, and there is a tendency for the reactivity with the matrix resin to be further improved.
[0153] From the viewpoint of not easily hindering the reactivity with the resin, the silane coupling agent is preferably nonionic. Among the nonionic silane coupling agents, a silane coupling agent having at least one group selected from the group consisting of a vinyl group, a methacryloxy group, and an acryloxy group is preferred, and a silane coupling agent having at least one methacryloxy group or an acryloxy group is particularly preferred. By not hindering the reactivity with the resin, the heat resistance and reliability of the printed circuit board can be improved.
[0154] In one embodiment, in formula (1), X is an organic functional group having at least one of the unsaturated double bond group and the amino group. Therefore, not only the embodiment in which X has both the unsaturated double bond group and the amino group, but also the embodiment in which X has the unsaturated double bond group but does not have the amino group, and the embodiment in which X does not have the unsaturated double bond group but has the amino group are all included in the scope of formula (1). However, X in formula (1) is preferably the unsaturated double bond group, and preferably does not contain the amino group.
[0155] From the viewpoint of reducing the dielectric loss tangent of the glass cloth, the ignition loss value of the glass cloth of the present embodiment is preferably 0.01 mass % or more and less than 0.180 mass %, preferably 0.01 mass % or more and less than 0.174 mass %, more preferably 0.01 mass % or more and less than 0.150 mass %, and further preferably 0.01 mass % or more and less than 0.130 mass %. When the ignition loss value is 0.180 mass % or more, there are a large number of residues of the surface treatment agent or its modified product on the surface of the glass cloth that do not form a chemical bond with the glass surface but are physically attached and cannot be reduced by washing with water, and as a result, the dielectric loss tangent of the glass cloth is easily increased. In addition, when the ignition loss value is less than 0.010 mass %, the bonding between the resin and the glass cloth is easily insufficient, so when a printed circuit board is made, it is easy to lack heat resistance and insulation reliability.
[0156] 〔Bulk dielectric loss tangent〕
[0157] In this specification, the bulk dielectric loss tangent refers to the dielectric loss tangent measured at 10 GHz for the raw material of the glass cloth using a split cylindrical resonator. The raw material of the glass cloth, for example, can be a glass raw material such as a glass type, glass filaments, and glass yarns as described later. The bulk dielectric loss tangent of the glass raw material constituting the glass cloth can be measured by the same method as the dielectric loss tangent measurement of the glass cloth, using a glass plate with a thickness of 300 μm or less having the same type and composition as the glass raw material.
[0158] From the viewpoint of further improving the effect of the present invention, for the weaving of the glass cloth of the present embodiment, the bulk dielectric loss tangent of the glass constituting the glass yarn is preferably 2.5×10 -3 Below, more preferably 2.0×10 -3 Below, more preferably 1.7×10 -3 Below, more preferably 1.5×10 -3 Below, more preferably 1.2×10 -3 Below, particularly preferably 1.0×10 -3 Below, the most preferred is 8.0×10 -4 The bulk dielectric loss tangent is greater than 0.
[0159] Regarding the dielectric loss tangent, bulk dielectric loss tangent and their difference of the glass cloth, although we do not wish to be limited by theory, it is believed that they can be adjusted within the above numerical ranges, for example, by the following method:
[0160] The surface treatment agent is selected in such a manner as to suppress the residue and generation of the following (i) or (ii);
[0161] Optimize the conditions of heating degreasing (heating desizing) process, residual slurry reduction process, fixing process, cleaning process, drying process, fine cleaning process, fine drying process, etc. in the glass cloth manufacturing process;
[0162] In the fine cleaning process, the surface treated glass cloth is cleaned with an organic solvent; etc.
[0163] (i) Generation of thermal oxidation degradation products of the sizing agent physically attached to the surface of the glass yarn
[0164] (ii) Generation of surface treatment agent residues or modified products thereof that are physically attached to the glass surface without forming a chemical bond and cannot be reduced by washing with water
[0165] [Measurement method of dielectric loss tangent of glass cloth]
[0166] The dielectric properties of the glass cloth of the present embodiment can be measured using a resonance method. As a preferred measuring instrument using the resonance method, a split cylindrical resonator can be cited. Compared with the previous measuring method of evaluating the dielectric properties by making a printed circuit board as a measurement sample, the resonance method can be measured simply and accurately. The reason for this is not limited to theory, because the resonance method is suitable for evaluating low-loss materials in the high-frequency region. As evaluation methods for dielectric properties other than the resonance method, for example, a concentrated constant method or a reflection transmission method are known. On the other hand, in the concentrated constant method, since it is necessary to use two electrodes to clamp the measurement sample to form a capacitor, the operation is cumbersome. In addition, in the reflection transmission method, when evaluating low-loss materials, the influence of the matching characteristics of the port is easily manifested, and therefore, it is easy to become difficult to evaluate the dielectric loss tangent of the sample with high accuracy.
[0167] When measuring the dielectric properties of the glass cloth of the present embodiment which can be applied to printed circuit boards, especially printed circuit boards for high-speed communications, the measurable range of the measuring instrument is preferably a suitable range for both the frequency dielectric constant (Dk) and the dielectric loss tangent (Df). For example, Dk is preferably 1.1 to 50 Fm -1 The range is more preferably 1.5 to 10 Fm -1 The range is more preferably 2.0 to 5 Fm -1 In addition, Df can be greater than 0, preferably 1.0×10 -6 ~1.0×10 -1 The range is more preferably 1.0×10 -5 ~5.0×10 -1 The range is more preferably 5.0×10 -5 ~1.0×10 -2 range.
[0168] The measurable frequency of the measuring instrument is preferably 10 GHz or higher. If the frequency is 10 GHz or higher, it is possible to evaluate the characteristics in the frequency band region assumed when the glass cloth is actually used as a printed wiring board for high-speed communication.
[0169] The measurement area is preferably 10 mm 2 More than 15 mm is more preferred 2 More than, more preferably 20mm 2 By measuring the dielectric properties of the glass cloth over a larger area, the reliability of the inspection result of the glass cloth can be improved.
[0170] The thickness of the sample that can be measured is preferably 3 to 300 μm, more preferably 5 to 200 μm, and even more preferably 7 to 150 μm. This can improve the reliability of the test results of the glass cloth.
[0171] Based on the bulk dielectric loss tangent, the dielectric loss tangent of the glass cloth can be estimated to a certain extent, and vice versa. On the other hand, the dielectric loss tangent of the glass cloth sometimes differs from the bulk dielectric loss tangent. Although we do not want to be limited by theory, the reasons for this difference include: (1) the generation of thermal oxides and / or degraded products of the sizing agent that are physically attached to the surface of the glass filaments; (2) the residue and generation of unnecessary components that are physically attached to the surface of the glass filaments without forming chemical bonds. Therefore, by selecting the type of sizing agent, optimizing various conditions in the manufacturing process of the glass cloth, etc., the dielectric loss tangent of the glass cloth can be controlled within the above range.
[0172] The dielectric loss tangent of the glass cloth of the present embodiment at 10 GHz measured by the above-mentioned resonance method is 0.0010 or less. If it is such a glass cloth, a prepreg that can achieve improved dielectric properties can be provided. The dielectric loss tangent of the glass cloth at 10 GHz is preferably 0.0009 or less, more preferably 0.0008 or less, further preferably 0.00055 or less, further preferably 0.00053 or less, further preferably 0.00050 or less, further preferably 0.00045 or less, further preferably 0.00040 or less, and particularly preferably 0.00035 or less. If it is such a glass cloth, a prepreg that can further achieve improved dielectric properties can be provided. In addition, the lower limit is greater than 0.
[0173] 〔Permeability of glass cloth〕
[0174] The glass cloth of the present embodiment preferably has a void number of 180 or less after 5 minutes when castor oil is infiltrated. Thus, the glass cloth has good impregnation with the resin, and thus it is easy to improve the insulation and heat resistance of the printed circuit board. The void number after 5 minutes is more preferably in the range of 160 or less, further preferably in the range of 140 or less, further preferably in the range of 120 or less, and particularly preferably in the range of 100 or less. The fewer the void number after 5 minutes, the better the impregnation, and the stronger the adhesion between the glass cloth and the resin. Therefore, it is easy to provide a printed circuit board with good insulation reliability and heat resistance. In order to control the void number after 5 minutes when castor oil is infiltrated to less than 180, it is effective to treat the glass cloth with a silane coupling agent shown in the above formula (1), or to use a fiber opening method such as dry ice blasting or bending.
[0175] [Method for producing glass cloth]
[0176] The method for producing glass cloth of the present embodiment includes the step of washing the glass cloth with water having a sodium ion content of 20 ppm or less. In addition, the method for producing glass cloth of the present embodiment may include the step of heating and degreasing the glass cloth and the step of treating the glass cloth with a surface treatment agent.
[0177] [Heating and degreasing method of glass cloth]
[0178] In the heating degreasing method of the glass of the present embodiment, the glass cloth composed of glass fibers having a Si content of 95.0 to 100% by mass in terms of SiO2 is heated and degreased at a temperature above 700°C, thereby reducing the dielectric loss tangent of the glass cloth. From the viewpoint of being able to appropriately obtain the effect of the present embodiment, the temperature of the heating degreasing is preferably in the range of 700 to 1500°C, more preferably in the range of 800 to 1300°C, and further preferably in the range of 900 to 1100°C. When the heating degreasing temperature is lower than 700°C, it is not possible to fully remove the residue of the paste attached to the glass cloth, and therefore it is difficult to reduce the dielectric loss tangent of the glass cloth. On the other hand, when the heating degreasing temperature exceeds 1500°C, it becomes difficult to suppress the devitrification phenomenon of the glass and it is difficult to prevent the strength of the glass cloth from decreasing. The heating time can be appropriately selected, for example, 3 to 120 seconds.
[0179] As for the means for heating the glass cloth, as long as the heating can be performed in a manner that the heating and degreasing temperature is 700°C or higher, known heating methods, heating media, heating mechanisms, heating devices and heating components can be used, for example, (1) heating the glass cloth in a heating furnace; (2) bringing the glass cloth into contact with a heating unit; (3) bringing the glass cloth into contact with high-temperature steam; etc. By heating the glass cloth in a manner that the heating and degreasing temperature is 700°C or higher, organic matter attached to the surface of the glass cloth can be effectively removed or the time for removing the organic matter can be shortened. The heating of the glass cloth can be performed sequentially or continuously in a closed system or an open system, or a closed system and an open system can be combined.
[0180] In the case of a closed system, from the viewpoint of performing appropriate heating by a heating means, it is preferred to place the glass cloth in a heating furnace, and / or from the viewpoint of storage space and heating range, it is preferred to heat the glass cloth while storing it in a wound state. In addition, from the viewpoint of improving the removal efficiency of organic matter or shortening the removal time of organic matter, it is also preferred to heat the glass cloth while conveying it in a heating furnace.
[0181] In the case of an open system, it is preferred to heat the glass cloth while conveying it from the viewpoint of the heated area. The glass cloth can be conveyed, for example, by using an unwinding mechanism and a winding mechanism.
[0182] 〔Heating furnace〕
[0183] The heating means of the heating furnace is not limited to a specific means, and any means can be considered as long as the heating can be performed so that the deoiling temperature is 700° C. or higher, and various means such as electric heaters and burners can be considered. In addition, a combination of multiple means can be used for heating, but it is preferable to use a gas-fired single radiant tube burner or an electric heater.
[0184] From the viewpoint of heating efficiency, the heating furnace preferably has means for discharging the gas generated in the heating furnace and / or air circulation means. The gas discharging means may be, for example, a nozzle, a gas pipe, a small hole, an exhaust valve, etc. The air circulation means may be, for example, a fan, an air conditioning device, etc.
[0185] In addition, in order to effectively remove organic matter attached to the surface of the glass cloth, a continuous method in which the glass cloth is heated while being continuously passed through a heating furnace is preferred over an intermittent method in which the glass fiber fabric is wound on a winding core and heated at a predetermined atmospheric temperature. Furthermore, a method in which the glass cloth can be continuously cleaned using reverse osmosis (RO) water is most preferred.
[0186] [Contact parts for heating glass cloth]
[0187] As a method of heating the glass cloth, the above-mentioned heating furnace can be used, but from the viewpoint of low running cost, the glass cloth may be heated by bringing a member heated to a predetermined temperature into contact with the glass cloth.
[0188] The shape of the contact member is not particularly limited, as long as it can heat the glass cloth so that the heating and degreasing temperature thereof is 700°C or higher. From the perspective of the ease of conveying the glass cloth, a roller is preferably used as a member capable of heating the glass cloth in a roller shape, which can be used in a high temperature region, has less temperature unevenness in the width direction, and is heated by induction heating. When the glass cloth is heated by the contact member, it is considered that the temperature of the contact member is approximately equal to the surface temperature of the glass cloth.
[0189] Furthermore, in order to remove carbides adhering to the heating roller as the glass cloth is continuously heated, the heating roller method is preferably a method including a mechanism such as a scraper to remove adhering foreign matter.
[0190] [Method of applying high temperature steam to glass cloth (steam application method)]
[0191] The steam applied to the glass cloth may contain, for example, volatile solvents, water vapor, gases other than water vapor, etc., but water vapor is preferred from the viewpoint of toxicity to the human body and the viewpoint of easily promoting the decomposition of the sizing agent used in the glass fiber. Regarding the temperature of the high-temperature steam, in order to make the surface temperature of the glass cloth higher than 650°C, a method of supplying high-temperature steam and heated air in any proportion may be used if necessary. The temperature of the high-temperature steam is above 400°C, preferably above 450°C, more preferably above 550°C, further preferably above 600°C, and particularly preferably above 650°C. There is no limitation on the steam application method, which may be spraying, shower diffusion, nozzle, etc. As an alternative, the gas discharged from the heating furnace is sometimes reused as high-temperature steam.
[0192] The inventors conducted intensive research and found that when the amount of sodium ions attached to the surface of the glass cloth exceeds a specified amount, the tensile strength of the glass cloth significantly decreases due to the devitrification of the quartz glass if the glass cloth is subjected to a heat deoiling treatment at 700°C or above. In addition, it was found that, in order to suppress the devitrification phenomenon, when the glass cloth is washed with water having a sodium ion content of 20 ppm or less before the heat deoiling treatment, the amount of sodium ions on the glass surface decreases, thereby suppressing the devitrification phenomenon of the quartz glass even if the heat deoiling treatment is performed at 700°C or above. By maintaining the strength of the glass cloth after heat deoiling, wrinkles and / or damage in the process of treating the glass cloth with a surface treatment agent can be suppressed.
[0193] From the viewpoint of being able to appropriately obtain the effects of the present embodiment, the sodium ion content of the water used for washing is preferably in the range of 18 ppm or less, more preferably in the range of 15 ppm or less, further preferably in the range of 12 ppm or less, further preferably in the range of 10 ppm or less, and particularly preferably in the range of 7 ppm or less. When the sodium ion content of the washing water exceeds 20 ppm, the devitrification phenomenon of the quartz glass during heating and deoiling at 700° C. or more cannot be suppressed, and the tensile strength of the glass cloth decreases. As the lower limit of the sodium ion content, it is preferably zero, but it may be greater than 0.
[0194] As for the means of cleaning the glass cloth with a sodium ion content of less than 20 ppm, as long as the sodium ions on the glass surface can be removed, it can be a known cleaning method. For example, methods such as using ultrasonic waves (such as methods using ultrasonic vibrators), spraying using a sprayer (such as spraying using a high-pressure sprayer), and water vapor spraying can be considered. From the perspective of being able to process cheaply, the following method is preferred: after the glass cloth is immersed in a water tank storing washing water (water with a sodium ion content of less than 20 ppm), the excess washing water is removed with a squeeze roller, and then the glass cloth is dried. At this time, as an immersion time, for example, it can be more than 2 seconds, more than 5 seconds, more than 10 seconds, more than 15 seconds, or less than 120 seconds, less than 90 seconds, less than 60 seconds, or less than 45 seconds.
[0195] The method for producing water with a sodium ion content of 20 ppm or less can be a known method. For example, methods such as filtration using an RO membrane and deionization using an ion exchange resin can be considered. In the range that does not hinder the effect of the present invention, "water with a sodium ion content of 20 ppm or less" may include other liquid components (liquids other than water; etc.).
[0196] 〔Glass cloth heating and deoiling device〕
[0197] As described above, the heating and degreasing device for glass cloth of the present embodiment can heat the glass cloth so that the heating and degreasing temperature is 700° C. or higher. More specifically, the heating and degreasing device for glass cloth is preferably a heating and degreasing device for glass cloth having the following configuration:
[0198] The device has an unwinding mechanism and a winding mechanism; and
[0199] The invention comprises a heating furnace capable of carrying out the steps of washing the glass cloth with water having a sodium ion content of 20 ppm or less to remove sodium ions on the glass surface while conveying the glass cloth, and heating the glass cloth so that the heating degreasing temperature is 700° C. or higher.
[0200] The unwinding mechanism and the winding mechanism may be, for example, at least one pair of rolls, a roll-to-roll system, etc. The heating furnace, the air circulation means, the contact member, and the steam application means are as described in the method for producing the glass cloth.
[0201] 〔Surface treatment method of glass cloth〕
[0202] The glass processing method of this embodiment can be applied to glass filaments, and can also be applied to glass cloth. In other words, the process of weaving glass filaments to obtain glass cloth can be set before the glass processing method of this embodiment, can also be set in the middle, and can also be set after. It should be noted that in the glass processing method of this embodiment, the main purpose of "reducing" is, for example, removing at least a part of the sizing agent or the surface treatment agent containing the silane coupling agent, and the residue that is not completely removed is allowed to be generated.
[0203] The step of attaching the surface treatment agent may include, for example, at least one of the following steps:
[0204] a coating step of attaching a silane coupling agent to the surface of the glass using a treatment liquid having a concentration of 0.1 to 0.5 mass %,
[0205] The fixing step is to fix the silane coupling agent on the surface of the glass by heating and drying.
[0206] This makes it easy to perform appropriate surface treatment on the glass.
[0207] As a method for applying the treatment liquid to the glass in the covering process, the following methods can be used: (a) a method of immersing or passing the glass in the treatment liquid stored in a bath (hereinafter referred to as the "immersion method"), (b) a method of applying the treatment liquid to the glass using a roller coater, a die coater or a gravure coater, etc. In the case of the immersion method, it is preferred to set the immersion time of the glass in the treatment liquid to be greater than 0.5 seconds and less than 1 minute. In addition, when the immersion method is adopted, a prescribed tension (for example, 100 to 250 N) can be applied to the glass while the glass is passed through the treatment liquid at a conveying speed of 10 to 50 m / min. In addition, after the treatment liquid is applied to the glass, the solvent contained in the treatment liquid can be heated and dried by methods such as hot air and electromagnetic waves.
[0208] The concentration of the treatment liquid is preferably 0.1 to 0.5 mass %, more preferably 0.1 to 0.45 mass %, and still more preferably 0.1 to 0.4 mass %. This makes it easier to more appropriately treat the surface of the glass.
[0209] In the fixing step, the heating and drying temperature is preferably 80° C. or higher, more preferably 90° C. or higher, to allow the silane coupling agent to react sufficiently with the glass. In addition, the heating and drying temperature is preferably 300° C. or lower, more preferably 180° C. or lower, to prevent degradation of the organic functional groups of the silane coupling agent.
[0210] The process of reducing the silane coupling agent may include, for example, at least one of the following processes: a cleaning process of cleaning the silane coupling agent that has not formed a chemical bond with the glass surface; a drying process of heating and drying the cleaned glass; and a fine cleaning process of reducing unnecessary components that have not been completely washed and have not formed a chemical bond with the glass surface. In this way, it is easy to control the ignition loss value. It should be noted that the process of reducing the silane coupling agent may include, for example, a fine drying process after the fine cleaning process.
[0211] Among them, the fine cleaning process can reduce the unnecessary components that are not washed out with water in the cleaning process and do not form chemical bonds with the glass surface. In this fine cleaning process, for example, an organic solvent can be used as a cleaning liquid. By having a fine cleaning process, even if a low-dielectric glass like the present embodiment is used, it is easy to control the difference between the dielectric loss tangent of the obtained glass cloth and the dielectric loss tangent of the bulk phase within the numerical range described above. As the organic solvent here, an organic solvent with high hydrophobicity is preferred, and an organic solvent with high affinity for residues and modified products of silane coupling agents with hydroxyl groups is also preferred. The cleaning method can adopt an immersion method, a spray spray, etc., and can also be heated or cooled as needed. In order to be able to inhibit the glass dissolved in the cleaning solution from adhering again, it is preferred to use an extrusion roller to reduce the residual solvent in the glass after cleaning.
[0212] Regarding the organic solvent that can be used as the cleaning liquid in the fine cleaning step, for example, the following solvents can be used alone or in combination. Examples of highly hydrophobic organic solvents include:
[0213] Saturated chain aliphatic hydrocarbons such as n-pentane, isopentane, n-hexane, isohexane, n-heptane, isoheptane, n-octane, isooctane, 2,2,4-trimethylpentane (isooctane), n-nonane, isononane, n-decane, isodecane, 2,2,4,6,6-pentamethylheptane (isododecane), etc.
[0214] Saturated cyclic aliphatic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, and ethylcyclohexane;
[0215] Aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, diethylbenzene, trimethylbenzene, triethylbenzene, etc.
[0216] Halogen-containing solvents such as chloroform, dichloromethane, and dichloroethane; etc.
[0217] Examples of organic solvents having high affinity with the residue or modified product of a silane coupling agent include:
[0218] Alcohols such as methanol, ethanol, butanol, etc.
[0219] Ketones such as acetone and methyl ethyl ketone;
[0220] Ethers such as methyl ethyl ether and diethyl ether;
[0221] Amides such as N,N-dimethylformamide and N,N-dimethylacetamide;
[0222] Dimethyl sulfoxide; etc.
[0223] Among them, aromatic hydrocarbons, alcohols or ketones are preferred, and methanol is more preferred, from the viewpoint of easily and efficiently reducing the silane coupling agent physically attached to the glass. Therefore, as the cleaning liquid in the fine cleaning step, a cleaning liquid having methanol as the main component (methanol is 50% by mass or more or 60% by mass relative to 100% by mass of the cleaning liquid) is preferably used.
[0224] In the fine drying process, the cleaning liquid used in the above-mentioned fine cleaning process can be reduced. From the viewpoint of the ease of reducing the cleaning liquid by drying, the boiling point of the cleaning liquid used in the above-mentioned fine cleaning process is preferably below 120°C. Drying can be performed by heating drying or air drying. It should be noted that when an organic solvent is used as the cleaning liquid, from the viewpoint of safety, it is preferably heated and dried by hot air drying using low-pressure steam or heat medium oil as a heat source. The drying temperature is preferably above the boiling point of the cleaning liquid, and from the viewpoint of suppressing the deterioration of the silane coupling agent, it is preferably below 180°C.
[0225] As a fiber-opening method in the fiber-opening process of glass cloth, for example, a method of fiber-opening the glass cloth using spray water (high-pressure water fiber-opening), an oscillating washing machine, ultrasonic water or a liquid squeezer can be used. During the fiber-opening process, by reducing the tension applied to the glass cloth, there is a tendency to further reduce the air permeability. It should be noted that in order to suppress the decrease in the tensile strength of the glass cloth caused by the fiber-opening process, it is preferred to implement measures such as low friction with the contact parts when weaving the glass fibers, optimization of the sizing agent, and high adhesion quantification. From the viewpoint of reducing the number of voids after 5 minutes when impregnated with castor oil, it is effective to increase the processing pressure in the fiber-opening process. As a fiber-opening method for glass cloth composed of glass fibers with high glass hardness, dry ice blasting is preferred.
[0226] Dry ice blasting is a method of spraying (blowing) dry ice particles with a particle size of 5 to 300 μm from a height of 5 to 1000 mm at an air pressure of 0.05 to 1 MPa. More preferably, dry ice particles with a particle size of 5 to 300 μm are sprayed from a height of 5 to 600 mm at an air pressure of 0.1 to 0.5 MPa. By staying within this range, quality problems such as glass fiber breakage are less likely to occur, so the effect of improving impregnation can be expected.
[0227] The above steps do not necessarily have to be performed through different steps, and multiple steps can also be concentrated into one step. For example, when the cleaning step is performed after the weaving step, the cleaning step can also be used as the fiber opening step by using a high-pressure water sprayer in the cleaning step. In most cases, the composition of the glass cloth does not usually change before and after the fiber opening. In addition, in addition to the above steps, the manufacturing method of the glass cloth can also have any steps. For example, after the fiber opening step, there can be a longitudinal cutting process. In addition, if possible, the order of the above steps can be changed.
[0228] According to the surface treatment method of the glass cloth of the present embodiment described above, unnecessary components that are considered to increase the dielectric loss tangent can be appropriately reduced, and on the basis of this, the silane coupling agent can be easily applied to the surface of each glass filament constituting the glass yarn.
[0229] [Wrinkles and / or damage on glass cloth]
[0230] As appearance defects of glass cloth, wrinkles generated when the glass cloth is transported and / or collision damage caused by accidental contact with equipment are known. The wrinkles and / or damage on the glass cloth will become defective parts when making prepreg, so it is preferred not to generate wrinkles and / or damage. As a method to suppress wrinkles and / or damage, it is effective to control the tension during the transportation of the glass cloth. By sufficiently applying tension to the glass cloth, the vibration of the glass cloth can be suppressed, so wrinkles and / or damage can be less likely to occur. However, when the tensile strength of the glass cloth in the warp direction per unit thickness is too low, it is impossible to apply sufficient tension to the glass cloth, so it is difficult to suppress wrinkles and / or damage. The range of the tensile strength in the warp direction per unit thickness is as described above. When the tensile strength in the warp direction per unit thickness of the glass cloth is less than 0.50, the glass cloth is prone to breakage during the transportation process, so sufficient tension cannot be applied. In particular, after the glass cloth is immersed in the surface treatment liquid and the liquid is squeezed out, it is dried to fix the surface treatment agent on the glass cloth. However, if sufficient tension is not applied, wrinkles may occur at the liquid squeezed portion of the glass cloth and / or the glass cloth may be damaged by collision due to accidental contact with the heating furnace. In addition, the glass cloth may be broken at the liquid squeezed portion.
[0231] [Tear of glass cloth]
[0232] When the strength of the glass cloth is significantly reduced, the glass cloth is likely to break (tear). Such a significant reduction in the strength of the glass cloth is likely to occur when the glass cloth is subjected to a high-temperature heat treatment (for example, 700 to 1500° C.).
[0233] In addition, when the uniformity of the tensile strength in the warp direction of the glass cloth and / or the uniformity of the filament diameter are low, the glass cloth is easily torn when it is transported. In this case, the above-mentioned wrinkles and / or damages are also likely to occur. Therefore, the coefficient of variation of the tensile strength in the warp direction of the glass cloth of this embodiment is within the range of 15% or less and / or the coefficient of variation of the filament diameter of the glass fiber constituting the glass cloth is within the range of 10% or less. The glass cloth having the coefficient of variation within the above range will be a glass cloth with high uniformity and less appearance defects.
[0234] Here, it is assumed that the ratio (coefficient of variation of tensile strength in the warp direction / coefficient of variation of filament diameter) when the glass cloth is subjected to high temperature heat treatment (e.g., 700 to 1500°C) is in the range of 1.3 to 1.4. At this time, in the glass cloth of the present embodiment, the ratio (coefficient of variation of tensile strength in the warp direction / coefficient of variation of filament diameter) is preferably greater than 0 and less than 5.0 (excluding the range of 1.3 to 1.4). This method is a method of glass cloth with less appearance defects.
[0235] In addition, it is assumed that the ratio (coefficient of variation of filament diameter / coefficient of variation of tensile strength in the warp direction) when the glass cloth is subjected to high temperature heat treatment (e.g., 700 to 1500° C.) is in the range of 0.7 to 0.8. At this time, in the glass cloth of the present embodiment, the ratio (coefficient of variation of filament diameter / coefficient of variation of tensile strength in the warp direction) is preferably greater than 0 and less than 4.5 (excluding the range of 0.7 to 0.8). This method is also a method of glass cloth with less appearance defects.
[0236] [Prepreg]
[0237] The prepreg of the present embodiment includes the glass cloth and a matrix resin impregnated into the glass cloth. Thus, a prepreg with fewer voids can be provided.
[0238] As the matrix resin, a thermosetting resin or a thermoplastic resin may be used, and if possible, both may be used in combination, or other resins may be further included.
[0239] Examples of the thermosetting resin include:
[0240] (a) an epoxy resin obtained by curing a compound having an epoxy group with a compound having at least one group selected from the group consisting of an amino group, a phenol group, an acid anhydride group, a hydrazide group, an isocyanate group, a cyanate group, and a hydroxyl group that reacts with the epoxy group;
[0241] (b) a radical polymerization type curable resin obtained by curing a compound having at least one group selected from the group consisting of an allyl group, a methacrylic group, and an acrylic group;
[0242] (c) a maleimide triazine resin obtained by curing a compound having a cyanate group with a compound having a maleimide group;
[0243] (d) a thermosetting polyimide resin obtained by curing a maleimide compound with an amine compound;
[0244] (e) Benzoxazine resins, which are obtained by cross-linking and curing a compound having a benzoxazine ring by heating and polymerization; etc.
[0245] It should be noted that, when obtaining (a) epoxy resin, the compounds can be reacted without a catalyst, or a catalyst having a reaction catalytic ability such as an imidazole compound, a tertiary amine compound, a urea compound, or a phosphorus compound can be added to react the compounds. In addition, when obtaining (b) free radical polymerization type curing resin, a thermal decomposition catalyst or a photodecomposition catalyst can be used as a reaction initiator.
[0246] Examples of thermoplastic resins include polyphenylene ether, modified polyphenylene ether, polyphenylene sulfide, polysulfone, polyethersulfone, polyarylate, aromatic polyamide, polyetheretherketone, thermoplastic polyimide, insoluble polyimide, polyamideimide, and fluororesin. As insulating materials for printed circuit boards for high-speed communications, polyphenylene ether or modified polyphenylene ether having sufficient free radical reactivity is preferred.
[0247] When the matrix resin used in the printed wiring board for high-speed communication has a vinyl group or a methacrylic group, the hydrophobicity is high, and the silane coupling agent having a functional group participating in a radical reaction such as a methacrylic group has good compatibility with the matrix resin.
[0248] As mentioned above, a thermosetting resin and a thermoplastic resin can be used in combination. In addition, the prepreg may further contain an inorganic filler. The inorganic filler is preferably used in combination with a thermosetting resin, and examples thereof include: aluminum hydroxide, zirconium oxide, calcium carbonate, aluminum oxide, mica, aluminum carbonate, magnesium silicate, aluminum silicate, silicon dioxide, talc, short glass fibers, aluminum borate, and silicon carbide. The inorganic filler may be used alone or in combination of two or more.
[0249] [Printed Circuit Board]
[0250] The printed wiring board of the present embodiment includes the above-mentioned prepreg, thereby providing a printed wiring board having excellent insulation reliability.
[0251] [Integrated Circuits and Electronic Equipment]
[0252] In addition, an integrated circuit and an electronic device including the printed wiring board are also one aspect of the present embodiment. An integrated circuit and an electronic device obtained by using the printed wiring board of the present embodiment are excellent in various characteristics.
[0253] Example
[0254] Next, the present invention will be described using examples and comparative examples.
[0255] [Method for measuring the thickness of glass cloth]
[0256] The thickness of the glass cloth is determined according to 7.10 of JIS R 3420. Specifically, a micrometer is used to rotate the mandrel steadily and gently contact the measuring surface of the sample in parallel. Then, the scale is read after the ratchet sounds three times. It should be noted that 7.10 of JIS R 3420 stipulates the general test method for cloth products such as glass cloth.
[0257] [Method for measuring weight per unit area (mass of cloth)]
[0258] Cut the cloth into a specified size and divide its mass by the sample area to obtain the mass. 2 The weight of each glass cloth was measured 20 times using the obtained values. The average weight per unit area (g / m 2 ) and coefficient of variation.
[0259] Coefficient of variation of unit area weight of glass cloth (%)
[0260] =(Standard deviation of the weight per unit area of glass cloth / average value of the weight per unit area of glass cloth)×100
[0261] 〔Measurement method of converted thickness〕
[0262] Since glass cloth is a discontinuous planar body with air between glass fibers, the converted thickness is calculated by dividing the weight per unit area of each glass cloth (mass of cloth) by the density of glass. Specifically, the converted thickness is calculated by the following formula. The value of this converted thickness is used for the measurement by the resonance method.
[0263] Conversion thickness (μm) = unit area weight (g / m 2 )÷density(g / cm 3 )
[0264] 〔Measurement method of dielectric loss tangent〕
[0265] The dielectric loss tangent of each glass cloth is calculated according to IEC 62562. Specifically, the glass cloth samples sampled according to the size required for measurement using a split cylindrical resonator are stored in a constant temperature and humidity oven at 23°C and 50% RH for more than 8 hours. Then, the dielectric properties of the stored samples are measured using a split cylindrical resonator (manufactured by EM Labs) and an impedance analyzer (manufactured by Agilent Technologies). Each sample is measured 5 times, and the average value is calculated. In addition, the above-mentioned converted thickness is used as the thickness of each sample for measurement. Similarly, a glass plate with a thickness of less than 300μm and the same composition as each glass cloth is prepared, and the bulk dielectric loss tangent is also measured based on the thickness value obtained by measuring the thickness of the glass plate. It should be noted that IEC 62562 mainly stipulates the method for measuring the dielectric properties of fine ceramic materials used in microwave circuits in the microwave band.
[0266] [Method for determining the ignition loss of glass cloth]
[0267] The ignition loss value of the glass cloth was determined according to JIS R3420.
[0268] 〔Tensile strength and coefficient of variation of glass cloth〕
[0269] According to JIS R3420, the tensile test of the glass cloth in the warp direction was performed 5 times, and the average value was taken as the tensile strength in the warp direction. In addition, the coefficient of variation of the tensile strength in the warp direction was calculated using the following formula.
[0270] Coefficient of variation of tensile strength in warp direction (%) =
[0271] (Standard deviation of tensile strength in warp direction / average tensile strength in warp direction)×100
[0272] [Tensile strength in the warp direction per unit thickness of glass cloth]
[0273] The tensile strength in the warp direction per unit thickness of the glass cloth was determined from the following formula (A) using the thickness of the glass cloth and the tensile strength in the warp direction.
[0274] Tensile strength of glass cloth in the warp direction (N / 25mm) / thickness of glass cloth (μm)···(A)
[0275] 〔Coefficient of variation of filament diameter〕
[0276] The warp yarns of the glass cloth were extracted, and the diameter of the filaments constituting the arbitrary glass fibers was measured every 1 cm for 10 cm. The average value was taken as the average filament diameter. The coefficient of variation of the filament diameter was calculated from the obtained measurement results using the following formula.
[0277] Coefficient of variation of filament diameter (%) = (standard deviation of filament diameter / average filament diameter) × 100
[0278] [Determination of the amount of sodium ions contained in water used for washing before degreasing]
[0279] The amount of sodium ions contained in the water used to wash the glass cloth before heating and degreasing was measured using an ion chromatograph.
[0280] <Pretreatment conditions>
[0281] Adjust the sample by diluting with water as appropriate.
[0282] <Cation ion chromatography conditions>
[0283] Installation: Tosoh, IC-2010
[0284] Separation column: Tosoh, TSKgel-Super IC-Cation / P (4.6mm×150mm)
[0285] Separation solution: 2.5mM HNO3+0.5mM L-histidine
[0286] Flow rate: 1.0mL / min
[0287] Detection: Conductivity
[0288] Column temperature: 40°C
[0289] Injection volume: 30μL
[0290] [Measurement / Evaluation Method of Resin Impregnation]
[0291] The glass cloth is sampled in a size of 50 mm × 50 mm. At this time, the sampling is performed in a manner that does not bend or touch the measurement site. The number of voids when the sampled glass cloth is immersed in castor oil (manufactured by Hayashi Junyao Industry Co., Ltd., product number: 03001535) at a liquid temperature of 25°C for a specified time is counted. A high-precision camera (frame size: 5120 × 5120 pixels) is set at a position perpendicular to the glass cloth, and an LED lamp (manufactured by CCS Co., Ltd., PowerFlash-bar type lighting) as a light source is irradiated from both sides in a manner that the glass cloth is sandwiched from the side position 15 cm away from the glass cloth. Then, the number of voids of 160 μm or more existing between the glass filaments within a 32 mm × 32 mm viewing angle is counted, and the average value obtained by three measurements is taken as the number of voids.
[0292] That is, “the number of voids in the glass cloth after 5 minutes of being immersed in castor oil” is the number of voids observed when the glass cloth is immersed in castor oil for 5 minutes under the above conditions.
[0293] The voids correspond to the portions that are not impregnated with the matrix resin. Therefore, a small number of voids in the glass cloth means that the glass cloth is excellent in the impregnation property with the matrix resin.
[0294] [Manufacturing of Q1035 (grey cloth)]
[0295] Glass yarns with a SiO2 composition greater than 99.9% by mass were used, and a jet loom was used to weave the cloth with a weaving density of 66 warp yarns / 25 mm and 68 weft yarns / 25 mm. It should be noted that the weaving was performed in a manner such that the cloth width was 1300 mm. As the warp yarns, quartz glass yarns with an average filament diameter of 5.0 μm, 100 filaments, and a twist number of 1.0Z were used. In addition, as the weft yarns, quartz glass yarns with an average filament diameter of 5.0 μm, 100 filaments, and a twist number of 1.0Z were used.
[0296] [Manufacturing of Q1078 (grey cloth)]
[0297] Glass yarns with a SiO2 composition greater than 99.9% by mass were used, and a jet loom was used to weave the cloth with a weaving density of 54 warp yarns / 25 mm and 54 weft yarns / 25 mm. It should be noted that the weaving was performed in a manner such that the cloth width was 1300 mm. As the warp yarns, quartz glass yarns with an average filament diameter of 5.0 μm, 200 filaments, and a twist number of 1.0Z were used. In addition, as the weft yarns, quartz glass yarns with an average filament diameter of 5.0 μm, 200 filaments, and a twist number of 1.0Z were used.
[0298] [Manufacturing of Q1017 (grey cloth)]
[0299] Glass yarns with a SiO2 composition greater than 99.9% by mass were used, and a jet loom was used to weave the cloth with a weaving density of 95 warp yarns / 25mm and 95 weft yarns / 25mm. It should be noted that the weaving was performed in a manner such that the cloth width was 1300mm. As the warp yarns, quartz glass yarns with an average filament diameter of 4.0μm, 50 filaments, and a twist number of 1.0Z were used. In addition, as the weft yarns, quartz glass yarns with an average filament diameter of 4.0μm, 50 filaments, and a twist number of 1.0Z were used.
[0300] (Example 1)
[0301] The obtained Q1035 grey cloth is transported at a line speed of immersing in a water tank storing cleaning water 1 (sodium ion content = 2ppm) for 20 seconds, while cleaning the sodium ions attached to the glass surface (pre-degreasing cleaning process). Then, in a heating furnace set on the same line, it is heated at 800°C for 15 seconds to deoil. (Heating degreasing process). Next, a treatment liquid is prepared in which 0.3% by mass of 3-methacryloxypropyltrimethoxysilane (silane coupling agent A) Z6030 (manufactured by Dow Toray) is dispersed in pure water adjusted to pH = 3 with acetic acid. The cloth is immersed in the treatment liquid at a line tension of 200N and a line speed of 30m / min (surface treatment agent coating process), and after squeezing out the liquid, it is heated and dried at 130°C for 60 seconds to fix the silane coupling agent (fixing process). The dried cloth is irradiated in water at a frequency of 25kHz and an output power of 0.50W / cm 2 The excess silane coupling agent physically attached to the cloth was reduced by ultrasonic cleaning (cleaning step), and then dried at 130° C. for 1 minute (drying step), thereby obtaining a glass cloth.
[0302] (Example 2)
[0303] A glass cloth was obtained in the same manner as in Example 1 except that the glass cloth was washed with washing water 2 (sodium ion content = 10 ppm) and heated at 900° C. for 15 seconds for deoiling.
[0304] (Example 3)
[0305] A glass cloth was obtained in the same manner as in Example 1 except that the oil was removed by heating at 1000°C for 15 seconds.
[0306] (Example 4)
[0307] A glass cloth was obtained by the same method as in Example 3 except that a treatment liquid in which 0.15 mass % of 3-methacryloxypropyltrimethoxysilane (silane coupling agent A) Z6030 (manufactured by Dow Toray Co., Ltd.) and 0.40 mass % of 5-hexenyltrimethoxysilane (silane coupling agent B) Z6161 (manufactured by Dow Toray Co., Ltd.) were dispersed in pure water adjusted to pH = 3 with acetic acid was used.
[0308] (Example 5)
[0309] The glass cloth was obtained in the same manner as in Example 1 except that the deoiling was performed by heating at 1100° C. for 15 seconds, the line tension was changed to 130 N, and the silane coupling agent was fixed using a treatment liquid in which 0.50 mass % of 5-hexenyltrimethoxysilane (silane coupling agent B) Z6161 (manufactured by Dow Toray) was dispersed.
[0310] (Example 6)
[0311] The obtained Q1078 grey cloth is transported at a line speed of immersing in a water tank storing cleaning water 1 (sodium ion content = 2ppm) for 20 seconds, while cleaning the sodium ions attached to the glass surface (pre-degreasing cleaning process). Then, in a heating furnace set on the same line, it is heated at 800°C for 15 seconds to deoil. (Heating degreasing process). Next, a treatment liquid is prepared in which 0.3% by mass of 3-methacryloxypropyltrimethoxysilane (silane coupling agent A) Z6030 (manufactured by Dow Toray) is dispersed in pure water adjusted to pH = 3 with acetic acid. The cloth is immersed in the treatment liquid at a line tension of 260N and a line speed of 30m / min (surface treatment agent coating process), and after squeezing out the liquid, it is heated and dried at 130°C for 60 seconds to fix the silane coupling agent (fixing process). The dried cloth is irradiated in water at a frequency of 25kHz and an output power of 0.50W / cm 2 The excess silane coupling agent physically attached to the cloth was reduced by ultrasonic cleaning (cleaning step), and then dried at 130° C. for 1 minute (drying step), thereby obtaining a glass cloth.
[0312] (Example 7)
[0313] A glass cloth was obtained in the same manner as in Example 6 except that the glass cloth was washed with washing water 2 (sodium ion content = 10 ppm) and heated at 1000° C. for 15 seconds for deoiling.
[0314] (Example 8)
[0315] A glass cloth was obtained by the same method as in Example 7 except that a treatment liquid in which 0.15 mass % of 3-methacryloxypropyltrimethoxysilane (silane coupling agent A) Z6030 (manufactured by Dow Toray Co., Ltd.) and 0.3 mass % of 5-hexenyltrimethoxysilane (silane coupling agent B) Z6161 (manufactured by Dow Toray Co., Ltd.) were dispersed in pure water adjusted to pH = 3 with acetic acid to fix the silane coupling agent.
[0316] (Example 9)
[0317] A glass cloth was obtained in the same manner as in Example 6 except that the oil was removed by heating at 1100°C for 15 seconds.
[0318] (Example 10)
[0319] A glass cloth was obtained in the same manner as in Example 6 except that the oil was removed by heating at 1200° C. for 15 seconds and the line tension was changed to 150 N.
[0320] (Example 11)
[0321] The obtained Q1017 grey cloth was transported at a line speed while being immersed in a water tank storing cleaning water 1 (sodium ion content = 2 ppm) for 20 seconds, while the sodium ions attached to the glass surface were cleaned (pre-deoiling cleaning process). Then, in a heating furnace set on the same line, it was heated at 1000°C for 15 seconds to deoil. (Heating deoiling process). Next, a treatment liquid was prepared in which 0.15% by mass of 3-methacryloxypropyltrimethoxysilane (silane coupling agent A) Z6030 (manufactured by Dow Toray) and 0.3% by mass of 5-hexenyltrimethoxysilane (silane coupling agent B) Z6161 (manufactured by Dow Toray) were dispersed in pure water adjusted to pH = 3 with acetic acid. The cloth was immersed in the treatment liquid at a line tension of 150N and a line speed of 30m / min (surface treatment agent coating process), and after squeezing out the liquid, it was heated and dried at 130°C for 60 seconds to fix the silane coupling agent (fixing process). The dried cloth was irradiated in water at a frequency of 25kHz and an output power of 0.50W / cm 2 The excess silane coupling agent physically attached to the cloth was reduced by ultrasonic cleaning (cleaning step), and then dried at 130° C. for 1 minute (drying step), thereby obtaining a glass cloth.
[0322] (Example 12)
[0323] Glass cloth was obtained in the same manner as in Example 1 except that the glass cloth whose excess silane coupling agent had been reduced by ultrasonic cleaning was subjected to fiber opening treatment by uniformly spraying dry ice particles of 5 to 50 μm at an air pressure of 0.4 MPa onto the entire glass cloth.
[0324] (Example 13)
[0325] Glass cloth was obtained in the same manner as in Example 6 except that the glass cloth whose excess silane coupling agent had been reduced by ultrasonic cleaning was subjected to fiber opening treatment by uniformly spraying dry ice particles of 5 to 50 μm onto the entire glass cloth at an air pressure of 0.45 MPa.
[0326] (Comparative Example 1)
[0327] A glass cloth was obtained in the same manner as in Example 1 except that washing water 3 (sodium ion content = 24 ppm) was used in the pre-deoiling washing step and the line tension was changed to 60 N. Since the tension was low, the glass cloth was greatly vibrated during transportation, and wrinkles and collision damage caused by contact with the drying furnace were visually confirmed on the glass cloth during the step of fixing the treatment liquid.
[0328] (Comparative Example 2)
[0329] The glass cloth was obtained by heating and deoiling at 1000°C for 15 seconds and changing the line tension to 90 N. Due to the low tension, the glass cloth vibrated greatly during transportation, and wrinkles and collision damage caused by contact with the drying furnace were visually confirmed on the glass cloth during the fixing step of the treatment liquid.
[0330] (Comparative Example 3)
[0331] The glass cloth was processed in the same manner as in Comparative Example 2 except that the line tension was changed to 130 N. However, since the ratio of the tensile strength of the glass cloth to the line tension (tensile strength of the glass cloth (warp direction) / line tension) was low, the glass cloth broke during the step of fixing the silane coupling agent, and the glass cloth could not be obtained.
[0332] (Comparative Example 4)
[0333] A glass cloth was obtained in the same manner as in Example 7 except that washing water 3 (sodium ion content = 24 ppm) was used in the pre-deoiling washing step and the line tension was changed to 80 N. Since the tension was low, the glass cloth was greatly vibrated during transportation, and wrinkles and collision damage caused by contact with the drying furnace were visually confirmed on the glass cloth during the fixing step of the treatment liquid.
[0334] (Comparative Example 5)
[0335] Except that the line tension was changed to 150 N, processing of glass cloth was attempted in the same manner as in Comparative Example 4. However, since the ratio of the tensile strength of the glass cloth to the line tension (tensile strength of the glass cloth (warp direction) / line tension) was low, the glass cloth broke during the step of fixing the silane coupling agent, and glass cloth could not be obtained.
[0336] (Comparative Example 6)
[0337] The glass cloth was obtained by the same method as in Example 4 except that the degreasing was performed at 350°C for 10 hours, the line tension was set to 200 N, and the washing water was changed to 2. As a result, although wrinkles and damages were not observed in the obtained glass cloth, the dielectric loss tangent of the glass cloth was high because the temperature of the degreasing was low.
[0338] 〔Appearance inspection method of glass cloth〕
[0339] For the glass cloth of the above-mentioned embodiment and comparative example, a tension of 100N / 1300mm was applied on a roll-to-roll inspection table, and a visual inspection was performed on each meter of the product while irradiating with a halogen lamp to confirm whether there were wrinkles, damages, or tears on the glass cloth. The portion of the product with more than one defective appearance per 1m of the product was counted as the number of defective products, and the portion of the product without any defective appearance per 1m of the product was counted as the number of good products. The number of defective products per 2000m was counted. Based on the inspection results, the glass cloth of the embodiment and comparative example was graded according to the following indicators.
[0340] Wrinkles
[0341] A: The total number of product parts with wrinkles is less than 101m (= the incidence of defective quantity is less than 5%)
[0342] B: The total number of product parts with wrinkles is 101 or more and less than 200 m (= the occurrence rate of defective quantity is 5% or more and less than 10%)
[0343] C: The total length of the product where wrinkles are observed is 200 m or more (= the defective quantity occurrence rate is 10% or more)
[0344] damage
[0345] A: The total number of product parts with observable damage is less than 101m (= the incidence of defective quantity is less than 5%)
[0346] B: The total number of product parts with visible damage is 101 or more and less than 200m (= the occurrence rate of defective quantity is 5% or more and less than 10%)
[0347] C: The total number of product parts with visible damage is more than 200m (= the incidence rate of defective quantity is more than 10%)
[0348] Tear
[0349] A: The total length of the product with the fabric torn is less than 7m (the defective quantity incidence rate is less than 0.3%)
[0350] B: The total length of the product with fabric tearing is 7m or more and less than 12m (the defective quantity occurrence rate is 0.3% or more and less than 0.6%)
[0351] C: The total length of the product with torn fabric is more than 12 m (the defective quantity rate is more than 0.6%)
[0352] The manufacturing conditions and evaluation results of the examples and comparative examples are shown in the following table. It should be noted that the glass cloths of the examples can be used to produce prepregs, printed wiring boards, integrated circuits, and electronic devices by conventional methods.
[0353] [Method for producing laminated board]
[0354] 45 parts by mass of polyphenylene ether (Noryl SA9000 manufactured by SABIC), 10 parts by mass of triallyl isocyanurate, 45 parts by mass of toluene, and 0.6 parts by mass of 1,3-di(tert-butylisopropylbenzene) were added to a stainless steel container and stirred at room temperature for 1 hour to prepare a varnish. The glass cloth obtained in Examples 1, 6, 12, and 13 was impregnated with the prepared varnish and then dried at 115°C for 1 minute to obtain a prepreg. The obtained prepreg was overlapped, and copper foil with a thickness of 12 μm was overlapped on the upper and lower sides thereof, and heated at 200°C and 40 kg / cm 2 The heating and pressing were performed for 120 minutes, thereby obtaining a laminated plate having a thickness of 1 mm.
[0355] [Evaluation method of insulation reliability of laminated board]
[0356] A circuit pattern with through holes at intervals of 0.30 mm was made on the copper foil on both sides of the laminate obtained above to obtain an insulation reliability evaluation sample. A voltage of 50 V was applied to the obtained sample in an atmosphere of temperature 85°C and humidity 85% RH, and the change in resistance value was measured. At this time, the case where the resistance becomes less than 1 MΩ within 500 hours after the start of the test is considered as poor insulation. The same measurement was performed on 10 samples, and the number of samples that did not become poorly insulated among the 10 samples was calculated.
[0357] Table 1
[0358]
[0359] Table 2
[0360]
[0361] Table 3
[0362]
[0363] Table 4
[0364] Example 1 Example 6 Example 12 Embodiment 13 Number of gaps after 5 minutes 198 200 110 100 Insulation reliability of laminated substrates 3 3 9 9
Claims
1. A glass cloth, which is a glass cloth woven from glass yarns containing a plurality of filaments, The bulk dielectric loss tangent of the glass in the glass filament is less than 0.0010, The tensile strength of the warp yarn per unit thickness of the glass cloth represented by the following formula (A) is in the range of 0.50 to 6.0, and the coefficient of variation of the tensile strength in the warp yarn direction of the glass cloth is in the range of 15% or less. The dielectric loss tangent of the glass cloth at 10 GHz is in a range of greater than 0 and less than 0.0010; Formula (A): tensile strength of the glass cloth in the warp direction (N / 25 mm) / thickness of the glass cloth (μm)···(A).
2. A glass cloth, which is a glass cloth woven from glass yarns containing a plurality of filaments, The bulk dielectric loss tangent of the glass in the glass filament is less than 0.0010, The tensile strength of the warp yarn per unit thickness of the glass cloth represented by the following formula (A) is in the range of 0.50 to 6.
0. The coefficient of variation of the filament diameter of the glass fibers constituting the glass cloth is within a range of 10% or less, The dielectric loss tangent of the glass cloth at 10 GHz is in a range of greater than 0 and less than 0.0010; Formula (A): tensile strength of the glass cloth in the warp direction (N / 25 mm) / thickness of the glass cloth (μm)···(A).
3. The glass cloth according to claim 1 or 2, wherein: The dielectric loss tangent of the glass cloth at 10 GHz is in a range of greater than 0 and less than 0.0055.
4. The glass cloth according to claim 1 or 2, wherein: The silicon (Si) content in the glass filaments is 95.0 to 100% by mass in terms of silicon dioxide (SiO 2 ).
5. The glass cloth according to claim 1 or 2, wherein: The silicon (Si) content in the glass filaments is 99.0 to 100% by mass in terms of silicon dioxide (SiO 2 ).
6. The glass cloth according to claim 1 or 2, wherein: The glass filaments are treated with a surface treating agent including a silane coupling agent.
7. The glass cloth according to claim 6, wherein: The surface treatment agent comprises the silane coupling agent represented by the following formula (1), X(R) 3-n Yes n ···(1) In formula (1), X is an organic functional group having at least one of an amino group and an unsaturated double bond group, the unsaturated double bond group has free radical reactivity, Y is each independently an alkoxy group, n is an integer of 1 to 3, and R is each independently a group selected from the group consisting of a methyl group, an ethyl group and a phenyl group.
8. The glass cloth according to claim 7, wherein: X in the formula (1) is an organic functional group that does not form a salt with an ionic compound.
9. The glass cloth according to claim 7, wherein: X in the formula (1) does not contain an amine or an ammonium cation.
10. The glass cloth according to claim 7, wherein: X in the formula (1) is an organic functional group having one or more methacryloxy groups or acryloxy groups.
11. The glass cloth according to claim 1 or 2, wherein: The glass cloth has a loss on ignition value of 0.01 mass % or more and less than 0.18 mass %.
12. The glass cloth according to claim 1 or 2, wherein: The dielectric loss tangent of the glass cloth at 10 GHz is in a range of less than 0.00050.
13. The glass cloth according to claim 1 or 2, wherein: The glass cloth has a thickness of 60 μm or less.
14. The glass cloth according to claim 1 or 2, wherein: The unit area weight of the glass cloth (g / m 2 ) had a coefficient of variation of less than 3%.
15. The glass cloth according to claim 1 or 2, wherein: The unit area weight of the glass cloth (g / m 2 ) had a coefficient of variation of less than 1.5%.
16. The glass cloth according to claim 1 or 2, wherein: The glass cloth had a void count of 180 or less after 5 minutes of being impregnated with castor oil.
17. The glass cloth according to claim 1 or 2, which is used for a printed circuit board.
18. A prepreg comprising the glass cloth according to claim 1 or 2, a thermosetting resin and an inorganic filler.
19. A printed circuit board comprising the prepreg according to claim 18.
20. An integrated circuit comprising the printed circuit board according to claim 19.
21. An electronic device comprising the printed circuit board according to claim 19.
22. A method for producing glass cloth, comprising the step of washing the glass cloth with water having a sodium ion content of 20 ppm or less. 23 . The method for producing a glass cloth according to claim 22 , further comprising a step of heating and deoiling the glass cloth after the step of washing the glass cloth.
24. The method for producing glass cloth according to claim 23, wherein: The step of performing heating deoiling includes a step of performing heating deoiling at 700° C. or above.
25. The method for producing glass cloth according to claim 22 or 23, wherein: The step of washing the glass cloth includes immersing the glass cloth in water having a sodium ion content of 20 ppm or less.
26. The method for producing glass cloth according to claim 22 or 23, wherein: The step of washing the glass cloth includes washing the glass cloth with ultrasonic waves while immersing the glass cloth in water having a sodium ion content of 20 ppm or less.
27. The method for producing glass cloth according to claim 22 or 23, wherein: The step of washing the glass cloth includes washing the glass cloth with water having a sodium ion content of 20 ppm or less using a sprayer.
28. The method for producing glass cloth according to claim 22 or 23, wherein: The step of washing the glass cloth includes the step of washing the glass cloth with water having a sodium ion content of 20 ppm or less while conveying the glass cloth.
29. The method for producing glass cloth according to claim 22 or 23, comprising the steps of washing the glass cloth with water having a sodium ion content of 20 ppm or less while conveying the glass cloth and heating the glass cloth at a temperature of 700°C or higher.
30. The method for producing glass cloth according to claim 22 or 23, wherein: The silicon (Si) content in the glass yarn constituting the glass cloth is 95.0 to 100% by mass in terms of silicon dioxide (SiO 2 ).
Citation Information
Patent Citations
A method for producing glass cloth and glass yarn
CN111379063A
Silica glass yarn and silica glass cloth
CN111684117A
Annealed quartz glass cloth and method for manufacturing the same
CN113800778A
Glass cloth manufacturing method and glass yarn
JP2020105683A
Glass cloth, prepreg, and printed wiring board
JP7015972B1