Preparation method and application of injectable high-strength bone tissue adhesive
The hydrogel tissue adhesive composed of micro-nano particles and polymers solves the problems of poor bonding effect and risk of secondary injury in fracture treatment, achieves high-strength bone bonding and new bone formation, and significantly improves bone healing. Fracture healing efficiency and safety.
Patent Information
- Application Number
- CN202411108106.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Existing bone adhesives have problems in fracture treatment such as poor bonding effect, risk of secondary injury caused by stress concentration, and inability to effectively fix comminuted fractures and peri-articular fractures. Moreover, traditional methods require a second surgery to remove the fixation device. There is a risk of infection and complications.
It uses a hydrogel tissue adhesive composed of micro-nano particles and polymers to form a continuous porous network through covalent chemical reactions and non-covalent interactions to achieve injectable, moldable and self-healing properties, and combines inorganic components to promote bone regeneration .
It achieves a high-strength bone bonding effect, reduces the risk of secondary injury, promotes new bone formation, and its degradability and porous structure supports cell growth, significantly improving the efficiency and safety of fracture healing.
Smart Images

Figure CN118831200A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomaterials, and in particular relates to a preparation method and application of an injectable high-strength bone tissue adhesive. Background Art
[0002] Fracture treatment usually requires surgery to re-fix the fracture site to achieve bone regeneration and ultimately fracture healing. Traditional fracture fixation methods include the use of metal plates, pins, screws, etc. However, the materials implanted by traditional methods are usually non-degradable and require secondary surgery to remove. There is also the risk of infection of surrounding damaged tissues and osteoporosis at the site of injury due to stress shielding, which ultimately leads to re-fracture. In addition, traditional methods cannot effectively fix comminuted fractures or periarticular fractures. Tissue adhesives based on polymer design are considered to be an effective solution for fixing fractures. Biodegradable polymer adhesives do not require secondary surgery to remove the fixation device and reduce the risk of infection and other complications. Bone adhesives can effectively fix small-sized bone fragments such as comminuted fractures. However, the current tissue adhesive design based on in situ chemical cross-linking reactions in tissues still faces great challenges in achieving effective bone tissue adhesion in vivo. (1) The fracture site is usually in a liquid environment with continuous bleeding and tissue fluid, so the liquid molecules will hinder the effective contact between the adhesive and the tissue, making it difficult for the adhesive to effectively bond with the tissue. (2) Bone tissue itself has high strength and is usually in a continuous stress environment, so the bonding interface and material are prone to yield and failure. In summary, developing biomaterials with high tissue adhesion strength based on the physiological environment characteristics of bone tissue is an urgent problem to be solved in the development of bone tissue adhesion materials.
[0003] At present, common bone adhesives in clinical practice can be divided into two categories: natural material bone adhesives and synthetic material bone adhesives. Natural polymers come from nature, and natural polymers have been widely explored for medical applications such as bone adhesives, sealants or hemostatic agents. Compared with synthetic adhesives, adhesives composed of natural polymers generally exhibit excellent biocompatibility, degradability and non-immunogenicity. However, their mechanical strength is lower. (Such as fibrin glue, bio-glue, gelatin-based materials); synthetic polymers are artificial polymers prepared by chemical reactions. Compared with natural polymers, they generally exhibit higher mechanical strength, which allows them to withstand larger loads. However, their biocompatibility is generally not as good as natural polymers, and heat is often generated during the polymerization process, which may have a negative impact on surrounding tissues. Poor degradability is also a problem for synthetic adhesives. Common synthetic bone adhesives include polyurethane, polycyanoacrylate, polymethyl methacrylate, etc.
[0004] In addition, the above bone adhesive precursors are all in liquid state and easy to flow, so the material is not easy to stay in the desired area. In actual application, the moist environment of the wound or defect will also dilute the adhesive precursor, resulting in poor bonding effect. Summary of the invention
[0005] In order to solve the problems existing in the background technology, the purpose of the present invention is to provide a preparation method and use of an injectable, plastic, high-strength bone tissue adhesive based on a simple mixture of micro-nano particles and polymers. The initial state of the bone adhesive is a gel with injectable and self-repairing properties, which can ensure the filling of bone defects in a physiological environment. When the gel contacts the tissue, the covalent chemical reaction between the polymer and the particles and the tissue is achieved to achieve adhesion to the defective tissue. In addition, the inorganic component has excellent osteogenic activity, which can effectively promote the effective regeneration of bone defects, achieve physical adhesion of fracture defects, and promote the healing of bone tissue.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The invention provides a hydrogel tissue adhesive composed of organic / inorganic particles and polymer chains. The hydrogel tissue adhesive comprises micrometer or nanometer organic particles carrying amino groups, water-soluble high molecular polymers that undergo chemical cross-linking reactions with the amino groups, and micrometer or nanometer inorganic particles that have an osteogenesis-promoting effect. The mass ratio of the organic particles, the inorganic particles, and the water-soluble high molecular polymer is 1-20:1:0.1-5. The volume percentage of the particles in the hydrogel tissue adhesive is 10-80%. The organic / inorganic particles are formed by mixing organic particles and inorganic particles, or are composite particles with a core-shell structure formed by organic particles wrapping inorganic particles. Under the action of water, the hydrogel tissue adhesive can form a continuous and porous particle network through covalent action and / or reversible non-covalent action between particles, thereby giving the hydrogel tissue adhesive injectability, plasticity, and self-repairing properties.
[0008] Based on the above technical solution, further, the reversible non-covalent interaction includes electrostatic adsorption, hydrophilic and hydrophobic interaction, and hydrogen bonding.
[0009] Based on the above technical solution, further, the particle size is 1nm to 50μm; the particle potential is -30mv to +30mv under neutral conditions.
[0010] Based on the above technical solution, further, the volume percentage of particles in the hydrogel tissue adhesive is 20-60%.
[0011] Based on the above technical solution, further, the component of the micron or nanometer organic particles carrying amino groups is one or a combination of two or more of gelatin, chitosan, polylysine, polyethyleneimine, albumin, protamine, fibrin, silk protein, and silkworm cuticle protein.
[0012] Based on the above technical solution, further, the molecular weight of the component of the micrometer or nanometer organic particles carrying amino groups is 0.5-100 kDa.
[0013] Based on the above technical solution, further, the micron or nanometer-scale inorganic particles with osteogenesis-promoting effect account for ≥10wt% of the dry weight of the hydrogel tissue adhesive; the inorganic particles are calcium phosphate, calcium carbonate, calcium silicate, and bioglass inorganic non-metallic material particles; the morphology is one or a combination of two or more of needle-like, fibrous, granular, and blocky.
[0014] Based on the above technical solution, further, the inorganic particles are one or a combination of two or more of silicon dioxide particles, tricalcium phosphate, calcium phosphate, calcium carbonate, nanoclay particles, calcium silicate, and bioglass particles.
[0015] Based on the above technical solution, further, the inorganic particles are hydroxyapatite.
[0016] Based on the above technical solution, further, the surface of the inorganic particles is modified with amino groups.
[0017] Based on the above technical scheme, the process of modifying the surface of inorganic particles with amino groups is further as follows: the inorganic particles are added to n-hexane to obtain a 1-500 mg / mL uniform dispersion, and then 3-aminopropyltriethoxysilane that reacts with the surface hydroxyl groups of the inorganic particles is added, stirred at 50-80°C for 4-12 hours, and the amino-modified inorganic particles are obtained after freeze-drying.
[0018] Based on the above technical solution, further, the active groups of the water-soluble high molecular polymer that undergo chemical cross-linking reaction with the amino group include but are not limited to the following groups: succinimide, aldehyde, maleimide, epoxy, and carboxyl.
[0019] Based on the above technical solution, further, the skeleton of the water-soluble high molecular polymer that undergoes chemical cross-linking reaction with the amino group is one or a combination of two or more of polyethylene glycol, polyacrylic acid, block polyether F-127, block polyether F-108, sodium alginate, hyaluronic acid, chondroitin sulfate, dextran, cellulose, and agarose.
[0020] Based on the above technical solution, further, the shape of the water-soluble high molecular polymer is linear, multi-arm, or hyperbranched, with a molecular weight of 0.5-100 kDa, the water-soluble high molecular polymer accounts for 10-50 wt% of the dry weight of the hydrogel tissue adhesive, and the molar ratio of the amino group to the reactive group in the polymer chain is 0.1-100.
[0021] The present invention also provides a method for preparing the above-mentioned hydrogel tissue adhesive, comprising the following two methods:
[0022] Method 1: includes the following steps:
[0023] (1) Preparation of micrometer or nanometer organic particles carrying amino groups:
[0024] a) When the size of the prepared particles is greater than 5 μm, the preparation process is as follows: dissolving the raw materials in water at 20° C. to 60° C. to obtain an aqueous solution with a concentration of 1 to 100 mg / mL, adding a crosslinking agent, stirring and crosslinking at room temperature for 1 to 20 hours, removing the remaining crosslinking agent, and preparing microsphere particles by spray drying;
[0025] b) When the size of the prepared particles is 1 nm-5 μm and the raw materials are gelatin, polylysine, polyethyleneimine, albumin, and protamine, the raw materials are dissolved in water at 20° C. to 60° C. to obtain an aqueous solution with a concentration of 1 to 100 mg / mL; the pH of the aqueous solution is adjusted to 9 to 14, and a polar organic solvent of 1 to 10 times the volume of the aqueous solution is added dropwise to the aqueous solution, and after stirring for 5 to 60 minutes, a cross-linking agent is added, and the cross-linking is stirred at room temperature for 1 to 20 hours, and the remaining cross-linking agent is removed, and a micro-nano particle dispersion is obtained after washing, and a particle powder is obtained after freeze-drying;
[0026] c) When the size of the prepared particles is 1 nm-5 μm and the raw material is chitosan, the preparation process is the same as step b), the only difference is that the pH of the aqueous solution is adjusted to 3-5;
[0027] d) When the size of the prepared particles is 1 nm-5 μm and the raw material is silk fibroin, firstly, natural silk cocoons are degummed to obtain silk fibroin fibers, and then dissolved in an aqueous solution of lithium bromide or an aqueous solution of calcium chloride / ethanol to obtain a regenerated silk fibroin solution with a concentration of 0.01-0.1 g / mL, and then vacuum freeze-dried to obtain soluble freeze-dried silk fibroin, and then the particles are synthesized according to step b).
[0028] (2) Preparation of hydrogel tissue adhesive:
[0029] The preparation method is obtained by uniformly mixing the micron or nanometer organic particles carrying amino groups prepared in step (1), the water-soluble high molecular polymer that undergoes chemical cross-linking reaction with the amino groups, and the micron or nanometer inorganic particles having the function of promoting osteogenesis.
[0030] Method 2: includes the following steps:
[0031] 1) Preparation of composite particles with core-shell structure:
[0032] The inorganic particles as the inner core layer are ultrasonically dispersed in an aqueous solution in which an organic polymer of the outer shell layer is dissolved, and the concentration of the outer shell material is 1 to 100 mg / mL; the concentration ratio of the inner core material to the outer shell material is 1:2 to 1:50, and the pH is adjusted to 9 to 14. A polar organic solvent is added dropwise to the aqueous solution, and the volume of the polar organic solvent added is 1 to 10 times the volume of the aqueous solution. After stabilization for 10 to 30 minutes, a crosslinking agent is added, and a crosslinking reaction is carried out at room temperature for 1 to 12 hours to obtain a micro-nano particle suspension with a core-shell structure, and the remaining crosslinking agent is removed. After washing, a core-shell particle dispersion is obtained, and after drying, a composite particle powder with a core-shell structure is obtained.
[0033] 2) Preparation of hydrogel tissue adhesive:
[0034] The core-shell structure composite particles prepared in step 1) and the water-soluble high molecular polymer that undergoes chemical cross-linking reaction with the amino group are uniformly mixed to obtain the composite particles.
[0035] Based on the above technical scheme, further, the polar organic solvent is one or a mixed solvent of two or more selected from methanol, ethanol, isopropanol, butanol, acetone, acetonitrile, and tetrahydrofuran; the cross-linking agent is one or a combination of two or more selected from carbodiimide / N-hydroxysuccinimide, glyceraldehyde, glutaraldehyde, formaldehyde, paraformaldehyde, succinaldehyde, and genipin.
[0036] Another aspect of the present invention provides a method for using the hydrogel tissue adhesive, comprising the following steps: uniformly mixing the hydrogel tissue adhesive and water, repeatedly blowing 5 to 25 times through a Luer adapter syringe to obtain an injectable gel and then squeezing it out.
[0037] Based on the above technical solution, further, the mass ratio of the hydrogel tissue adhesive to water is 0.1 to 1:1.
[0038] Another aspect of the present invention provides the use of the above-mentioned hydrogel tissue adhesive as a bone tissue adhesive. The hydrogel tissue adhesive and water are mixed evenly to obtain an injectable gel, which is then extruded to the bone fragment or around an implanted device. After the reaction is solidified, the adhesive is bonded to the bone or the wound surface is sealed with bleeding. The solidification time is 1 to 600 seconds, and the bonding strength is 10 KPa to 5 MPa.
[0039] Another aspect of the present invention provides the use of the above hydrogel tissue adhesive as a drug carrier or a cell carrier, wherein the drug or cell, the hydrogel tissue adhesive and water are uniformly mixed and extruded to the wound site, thereby achieving the effect of drug release.
[0040] Based on the above technical scheme, further, the drug ingredients are one or a combination of two or more of vitamins, amino acids, mineral elements, microecological regulators, growth factors, small molecule drugs, protein macromolecule drugs, nucleic acid drugs, antibiotics, hormone drugs, anesthetic drugs, antiviral drugs, antibacterial drugs, anticancer drugs, and immunomodulatory drugs, which are used for repairing and filling trauma or defects of bone tissue, cartilage tissue, muscle, and blood vessels.
[0041] The present invention has the following beneficial effects:
[0042] 1. Fractures are one of the most common traumatic diseases, endangering the health of tens of millions of people around the world. Among them, severe comminuted fractures will greatly increase the difficulty of surgery, healing time and the incidence of surgical failure. Traditional fixation methods often use metal plates, pins, screws, etc. to stabilize fractures. However, these non-degradable devices need to be removed through a secondary operation. In addition, metal fixation devices may increase the risk of wound infection, tissue damage and re-fracture. In particular, traditional fixation is not effective in treating comminuted fractures or periarticular fractures, and broken bones generally cannot be retained during surgery. The injectable and degradable bone adhesive proposed in the present invention has a larger contact area with bone tissue, thereby reducing the risk of secondary injury due to stress concentration; and can achieve the bonding and fixation of broken bones, and the osteogenic components in the adhesive can promote the formation of new bones. At the same time, it can also be used as a hemostatic material and cell scaffold material for bone wounds.
[0043] 2. The bone filling material with adhesive properties composed of micro-nano particles and polymers of the present invention can undergo a covalent reaction between the particles and the polymer. When not covalently cross-linked, due to the non-covalent interaction between the particles, the material has the characteristics of shear thinning and self-repair, which can ensure the smooth extrusion of the material. This characteristic makes it have broad application prospects in the fields of bone adhesive materials, hemostatic materials and cell scaffolds.
[0044] 3. The bone adhesive material prepared by the present invention has the excellent properties of injectability, self-repair and plasticity, and can also obtain a hydrogel with high mechanical strength and structural stability through covalent cross-linking between particles and polymers. By adjusting the mass fraction of the gel, the storage modulus of the gel can be adjusted between 10 and 500 kPa, which is much higher than the traditional particle gel formed by physical interaction, and ensures the structural integrity and high mechanical strength of the gel in the body. When used for hemostasis of bone wounds, bone filling and bone tissue adhesion, the micro-nano particles in the material components of the present invention can make the material stay better at the defect site. Traditional polymer-based adhesives are easy to flow on the tissue surface due to their flow characteristics and humid environment, and cannot be stably formed at the desired site, which leads to a decrease in filling effect or failure of adhesion. There are non-covalent interactions between the particle components in the present invention, so that the hydrogel is not a liquid that is easy to flow before polymerization, but a colloid with shear thinning properties. After the material is extruded to the desired site, the covalent reaction between the material components allows the material to be stabilized at the defect site and form a firm bonding interface. The bonding strength of the currently used fibrin glue is about 17 KPa; the bonding strength of the polyethylene glycol adhesive Coseal is about 30 KPa, while the bonding strength of the present invention can reach 200 KPa, which is much higher than the currently commercially available fibrin glue and polyethylene glycol adhesive.
[0045] 4. The material of the present invention has a good osteogenesis effect when used as a bone adhesive. First, the inorganic components in the material components of the present invention release ions that promote osteogenesis. In addition, the material of the present invention has a porous microstructure, which provides space for cell growth. In practical applications, the shear-thinning characteristics of the colloidal gel of the material of the present invention ensure that the material can smoothly fill the gaps of the bone defect section or bone fragments. After the material reaches the specified position, the chemical reaction between the polymer and the particles can timely improve the mechanical strength of the material, and a chemical reaction will also occur between the polymer and the tissue, so that the material is firmly combined with the bone tissue, thereby achieving the effect of bone adhesion. After bone adhesion is achieved. Compared with traditional polymer adhesives, the bone adhesive material in the form of hydrogel is composed of degradable polymers (such as collagen or polyethylene glycol) and degradable inorganic materials (bioglass or calcium phosphate). When the integration of crushed bone particles is achieved, it can be gradually degraded and absorbed by the human body, and the surrounding new cells and new tissues will grow into the hydrogel scaffold matrix, and will eventually be completely degraded and absorbed, and replaced by new bone tissue. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a transmission electron microscope image of the albumin nanoparticles in Example 1.
[0047] Figure 2 It is a schematic diagram of the preparation of colloidal gel using a Luer adapter syringe;
[0048] Figure 3 This is the shear thinning diagram of the albumin colloid gel in Example 1.
[0049] Figure 4 This is the transmission electron microscopy morphology of hydroxyapatite in Example 8.
[0050] Figure 5 This is the transmission electron microscopy morphology of the albumin hydroxyapatite composite particles in Example 8.
[0051] Figure 6 This is the shear thinning of the albumin hydroxyapatite composite particles in Example 8.
[0052] Figure 7 This is the stress-strain curve of the albumin particles after cross-linking in Example 13.
[0053] Figure 8 This is a comparison chart of the filling effects of albumin hydroxyapatite composite particles and CA glue in Example 17.
[0054] Fig. 9 This is a comparison chart of the stability of the particle adhesive and Bio-glue in Example 18 in a humid environment.
[0055] Fig.10 This is a comparison chart of the coagulation effects of albumin hydroxyapatite composite particles and bone wax in Example 19.
[0056] Fig.11 This is a staining image of the albumin hydroxyapatite composite particle cell scaffold in Example 20.
[0057] Fig.12 This is the cell death and viability staining image of the albumin hydroxyapatite composite granules in Example 22.
[0058] Fig.13 This is the staining image of alkaline phosphatase (ALP) and Alizarin Red S (ARS), an indicator of late osteogenic differentiation, in the in vitro osteogenesis experiment in Example 24. DETAILED DESCRIPTION
[0059] The following non-limiting examples are provided to enable those skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way. In the following examples, unless otherwise specified, the experimental methods used are all conventional methods, and the materials and reagents used can be purchased from biological or chemical companies.
[0060] Example 1
[0061] 1. Preparation of Albumin Nanoparticles
[0062] At room temperature, 5g of albumin was dissolved in 100mL of deionized water and the pH was adjusted to 10. 200mL of acetone was added within 30min and stirred rapidly to allow the protein molecules to slowly dehydrate and curl into nanoscale spheres. Subsequently, 100μL of cross-linking agent glutaraldehyde was added and stirred for 12h. After cross-linking was completed, 1g of glycine was added to remove the remaining cross-linking agent. Then, the mixture was centrifuged and washed three times at 10,000rpm, and albumin nanoparticle powder was obtained after freeze-drying. A portion of the nanoparticles was made into a suspension and the morphology was observed by transmission electron microscopy. The results are as follows: Figure 1 ; and the hydrated particle size and zeta potential were measured by nano-laser particle size and zeta potential instrument, and the results are shown in Table 1.
[0063] Table 1 Hydration particle size and zeta potential of albumin nanoparticles
[0064] Particle size 491±5nm Potential -20.4±2.1mV
[0065] 2. Albumin colloid gel
[0066] The albumin particle powder aqueous solution of 0.2g / mL, 0.3g / mL, 0.4g / mL, 0.5g / mL and 1g / mL was repeatedly blown 10 times through a Luer adapter syringe to obtain an injectable albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scanning mode of the rotational rheometer, and the self-healing efficiency was obtained by comparing the storage modulus of the particle gel after oscillatory shearing with that before shearing (strain 0.1-1000%). The results are shown in Table 2. The shear thinning performance is shown in Figure 3 As shown, the frequency is 1 Hz and the strain is 0.5%. At this time, the albumin particle gel has a certain self-repair efficiency and shear thinning mechanical characteristics, and has injectable and printable properties.
[0067] Table 2 Storage modulus and self-healing rate of albumin colloid gel
[0068] 0.2g / mL 0.3g / mL 0.5g / mL 1g / mL Storage modulus(KPa) 1.079 7.14 47.84 110.762 Self-repair rate (%) 98.21019 86.5004 48.3381 9.81583
[0069] Example 2 (different materials)
[0070] At room temperature, 5g of gelatin (molecular weight 100kDa), polylysine (molecular weight 20kDa), protamine (molecular weight 620.943Da), chitosan (molecular weight 60kDa), silk fibroin (molecular weight 250kDa after degumming), and silkworm cuticle protein (all the above materials were purchased from Sigma) were dissolved in 100mL of deionized water, and the pH was adjusted to 10 (chitosan pH was adjusted to 3), and 200mL of acetone was added within 30min, and stirred rapidly to allow the molecules to slowly dehydrate and curl to form nanoscale spheres. Subsequently, 100μL of cross-linking agent glutaraldehyde was added and stirred for 12h. After cross-linking was completed, 1g of glycine was added to remove the remaining cross-linking agent. Then, the mixture was centrifuged and washed three times at 10000rpm, and nanoparticle powder was obtained after freeze drying. A portion of the nanoparticle suspension was taken and its hydrated particle size and zeta potential were measured by a nano-laser particle size and zeta potential instrument, and the results are shown in Table 3.
[0071] Table 3 Hydration particle size and zeta potential of nanoparticles prepared from different materials
[0072] gelatin Chitosan Poly-L-lysine Protamine Silk Fibroin Epidermal protein Particle size (nm) 236.6±8.9 333±43 763.6±18.2 146.9±13.9 291±5 812±38 Potential (mv) 3.7±0.6 3.3±0.4 16.9±0.3 6.7±1.08 -17.9±2.1 -19.5±2.1
[0073] It can be seen from Table 3 that the sizes of nanoparticles prepared from different materials are different. This is because different materials have different tolerances to the same solvent conditions (including type and volume ratio). If the material is easily dehydrated, the size of the nanoparticles formed will be smaller, and vice versa.
[0074] 0.3 g of the above nanoparticle powder and 1 mL of deionized water were repeatedly blown through a Luer adapter syringe for 10 times to obtain an injectable particle gel, and the storage modulus G' of the particle gel was obtained using the time scan mode of a rotational rheometer.
[0075] Table 4 Storage modulus and self-healing rate of particle gel
[0076] gelatin Chitosan Poly-L-lysine Protamine Silk Fibroin Epidermal protein Storage modulus(KPa) 21.3 3.7 6.25 1.2 13.5 19.5 Self-repair rate (%) 96.51 84.55 67.33 78.15 85.42 72.12
[0077] Example 3 (different solvents)
[0078] At room temperature, 5g of albumin was dissolved in 100mL of deionized water, and the pH was adjusted to 10. Within 30min, 200mL of methanol, ethanol, isopropanol, acetonitrile, and tetrahydrofuran were added respectively, and stirred rapidly to allow the protein molecules to slowly dehydrate and curl to form nanoscale spheres. Subsequently, 100μL of cross-linking agent glutaraldehyde was added and stirred for 12h. After cross-linking was completed, 1g of glycine was added to remove the remaining cross-linking agent. Then, the mixture was centrifuged and washed three times at 10000rpm, and albumin nanoparticle powder was obtained after freeze drying. A portion of the nanoparticle suspension was taken and its hydrated particle size and zeta potential were measured by a nano-laser particle size and zeta potential instrument. The results are shown in Table 5.
[0079] Table 5 Hydration particle size and zeta potential of albumin nanoparticles
[0080] Methanol Ethanol Isopropyl alcohol Acetonitrile Tetrahydrofuran Particle size (nm) 456.4 256.8 462.2 893.4 399.2 Potential (mv) -19.9 -10.9 -18.6 -13.8 -21.6
[0081] 0.3 g of the above particle powder and 1 mL of deionized water were repeatedly blown through a Luer adapter syringe for 10 times to obtain an injectable albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0082] Table 6 Storage modulus and self-healing rate of albumin particle gel
[0083] Methanol Ethanol Isopropyl alcohol Acetonitrile Tetrahydrofuran Storage modulus(KPa) 5.4 6.9 4.1 3.5 7.6 Self-repair (%) 94.48 95.67 93.64 98.30 95.72
[0084] Example 4 (different cross-linking agents)
[0085] At room temperature, 5g of albumin was dissolved in 100mL of deionized water, and the pH was adjusted to 10. 200mL of acetone was added within 30min, and the mixture was stirred rapidly to allow the protein molecules to slowly dehydrate and curl to form nanoscale spheres. Subsequently, the following cross-linking agents, carbodiimide / N-hydroxysuccinimide (EDC / NHS), glyceraldehyde, succinaldehyde, and genipin were added and stirred for 12h. After cross-linking, 1g of glycine was added to remove the remaining cross-linking agent. Then, the mixture was centrifuged and washed three times at 10000rpm, and albumin nanoparticle powder was obtained after freeze drying. A portion of the nanoparticle suspension was taken and its hydrated particle size and zeta potential were measured by a nano-laser particle size and zeta potential instrument, and the results are shown in Table 7.
[0086] Table 7 Hydration particle size and zeta potential of albumin nanoparticles
[0087] EDC / NHS Glyceraldehyde Succinaldehyde Kinipen Particle size (nm) 463.8 511.4 539.5 397.3 Potential (mv) -13.5 -21.6 -27.9 -21.1
[0088] 0.3 g of the above particle powder and 1 mL of deionized water were repeatedly blown through a Luer adapter syringe for 10 times to obtain an injectable albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0089] Table 8 Storage modulus and self-healing rate of albumin particle gel
[0090] EDC / NHS Glyceraldehyde Succinaldehyde Kinipen Storage modulus(KPa) 8.6 7.5 4.9 8.1 Self-repair (%) 97.10 95.67 95.84 96.81
[0091] Example 5 Different Sizes
[0092] First, a 5 wt % albumin aqueous solution was quickly added to a 10 wt % glutaraldehyde solution (the volume ratio of the two was 1:1) to form a dispersion of albumin particles, and then the particles were prepared by a spray drying process with a nozzle diameter of 0.75 mm. The prepared precursor solution was With the assistance of the pressure nozzle, the feed flow rate is 15mL / min and the air flow rate is 140m 3 / h, and the atomization pressures were 0.06, 0.04, and 0.01 MPa to produce albumin particles with particle sizes of 5 μm, 20 μm, and 50 μm.
[0093] 0.3 g of the above-mentioned particle powder and 1 mL of deionized water were repeatedly blown through a Luer adapter syringe for 10 times to obtain an injectable albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scanning mode of the rotational rheometer, and the self-healing efficiency was obtained by comparing the storage modulus of the particle gel after oscillatory shearing with that before shearing (strain 0.1-1000%).
[0094] Table 9 Storage modulus and self-repair rate of albumin particles with different particle sizes
[0095] 5μm 20μm 50μm Storage modulus(KPa) 2.69 1.6 0.85 Self-repair rate (%) 82 73 65
[0096] It can be seen from Table 9 that compared with nano-scale particles, the mechanical strength of micron-scale colloidal gel is lower than that of nano-scale colloidal gel when not covalently cross-linked, but it still has the properties of shear thinning and self-healing.
[0097] Example 6 (Albumin-inorganic mixed particles)
[0098] 0.3g albumin particle powder, 1mL deionized water and 50mg, 100mg, 500mg hydroxyapatite nanoparticles (purchased from McLean, particle size 60-80nm) were repeatedly blown 10 times through a Luer adapter syringe to obtain an injectable particle gel. The storage modulus G' of the particle gel was obtained using the time scanning mode of the rotational rheometer, and the self-healing efficiency was obtained by comparing the storage modulus of the particle gel after oscillatory shearing with that before shearing (strain 0.1-1000%).
[0099] Table 10 Storage modulus and self-healing rate of particle gels with different amounts of hydroxyapatite added
[0100] 50mg 100mg 500mg Storage modulus(KPa) 10.23 50.26 100.37 Self-repair rate (%) 87.56 78.56 84.12
[0101] 0.3 g of albumin particle powder, 1 mL of deionized water and 100 mg of silica nanoparticles, calcium silicate nanoparticles, tricalcium phosphate, calcium carbonate, nanoclay particles, and bioglass nanoparticles (the above materials were purchased from McLean, with a particle size of 60-80 nm) were repeatedly blown 10 times through a Luer adapter syringe to obtain an injectable albumin particle gel. The storage modulus of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0102] Table 11 Storage modulus and self-healing rate of particle gels with different types of nanoparticles added
[0103] Silicon dioxide Calcium silicate Tricalcium phosphate Calcium carbonate Nano Clay Bioglass Storage modulus(KPa) 32.5 29.3 24.12 20.62 29.5 27.9 Self-repair rate (%) 72.67 64.22 69.45 58.91 87.48 74.047
[0104] 0.3 g of albumin particle powder, 1 mL of deionized water and 100 mg of needle-shaped hydroxyapatite, fibrous hydroxyapatite, and block calcined bone (all of the above materials were purchased from McLean) were repeatedly blown 10 times through a Luer adapter syringe to obtain an injectable albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0105] Table 12 Storage modulus and self-healing efficiency of particle gels with different shapes of hydroxyapatite added
[0106]
[0107]
[0108] Example 7 HA amino modification
[0109] 100 mg / ml hydroxyapatite (HA, purchased from McLean) particles were added to 100 mL of n-hexane to obtain a uniform emulsion, 5 ml of 3-aminopropyltriethoxysilane was added, stirred at 60°C for 8 h, and freeze-dried to obtain amino-modified hydroxyapatite HA-NH2. The nanoparticle suspension was taken and its hydrated particle size and zeta potential were measured by a nano-laser particle size and zeta potential instrument, and the results are shown in Table 13.
[0110] Table 13 Hydration particle size and zeta potential of amino-modified hydroxyapatite
[0111] Particle size 261±5nm Potential +10.3±1.4mV
[0112] 0.3 g albumin particle powder, 1 mL deionized water and 100 mg HA-NH2 were repeatedly blown through a Luer adapter syringe 10 times to obtain an injectable particle gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer. The self-healing efficiency was obtained by comparing the storage modulus of the particle gel after oscillatory shearing with that before shearing (strain 0.1-1000%).
[0113] Table 14 Storage modulus and self-healing rate of particle gel with amino-hydroxyapatite added
[0114] 100mg Storage modulus(KPa) 103.42 Self-repair rate (%) 98.56
[0115] Example 8 (Albumin Hydroxyapatite Composite Nanoparticles)
[0116] 1. Preparation of Hydroxyapatite Nanoparticles
[0117] Hydroxyapatite nanoparticles were prepared by liquid phase chemical precipitation. 100 ml H2PO4 (75 mM) was added dropwise to 100 ml Ca(OH)2 (125 mM) and stirred at room temperature for 14-16 hours. The solution pH was then adjusted to 7 and centrifuged and washed three times to obtain hydroxyapatite nanoparticles. A portion of the nanoparticle suspension was taken for transmission electron microscopy testing. The size and morphology of the particles were as follows: Figure 4 shown.
[0118] 2. Preparation of albumin-hydroxyapatite composite nanoparticles (albumin@HA NPs)
[0119] First, ultrasonically disperse hydroxyapatite in 100 ml of albumin aqueous solution, with an albumin material concentration of 50 mg / ml; the ratio of hydroxyapatite to albumin material concentration is 1\8, adjust the pH of the aqueous solution to 10, add 200 mL of acetone within 30 min, stabilize for 15 minutes, add 100 μL of glutaraldehyde to obtain a covalently cross-linked particle suspension, and after cross-linking, add 1 g of glycine to remove the remaining cross-linking agent. Then, centrifuge and wash three times at 10,000 rpm, and freeze-dry to obtain albumin nanoparticle powder with a core-shell structure. Take a portion of the nanoparticle suspension and measure its hydrated particle size and zeta potential using a nano-laser particle size and zeta potential instrument.
[0120] Table 15 Hydration particle size and zeta potential of core-shell albumin nanoparticles
[0121] Particle size 484.2nm Potential -21.35mV
[0122] The suspension of core-shell albumin nanoparticles was tested by transmission electron microscopy. The size and morphology of the particles were Figure 5 As shown, the hydroxyapatite is needle-shaped, the size of the hydroxyapatite / albumin core-shell particles is about 500 nm, and through transmission electron microscopy, it can be clearly observed that the dark black hydroxyapatite is wrapped inside the light gray albumin particles to form a core-shell structure.
[0123] 3. Preparation of Albumin@HA NP Colloidal Gel
[0124] 0.3 g of albumin@HA particle powder and 1 mL of deionized water were repeatedly blown through a Luer adapter syringe 10 times to obtain an injectable albumin@HA particle gel. The storage modulus G' of the particle gel was obtained using the time scanning mode of the rotational rheometer. The self-healing efficiency was obtained by comparing the storage modulus of the particle gel after oscillatory shearing with that before shearing (strain 0.1-1000%). The results are shown in Table 2. The shear thinning performance is shown in Figure 6 As shown. At this time, the albumin particle gel has a certain self-repair efficiency and shear thinning mechanical characteristics, and has injectable and printable properties.
[0125] Table 16 Storage modulus and self-healing rate of albumin@HA particle gel
[0126] 0.3g Storage modulus 23.1kPa Self-repair rate (%) 89%
[0127] Example 9
[0128] The hydroxyapatite of Example 8 was ultrasonically dispersed in 100 ml of albumin aqueous solution, and the albumin material concentration was 50 mg / ml; the ratio of hydroxyapatite to albumin material concentration was 1\8, the pH of the aqueous solution was adjusted to 1-11, 200 mL of acetone was added within 30 min, and after stabilization for 15 minutes, 100 μL of glutaraldehyde was added to obtain a covalently cross-linked particle suspension, and the cross-linking reaction was carried out at room temperature for 12 h; after the cross-linking was completed, 1 g of glycine was added to remove the remaining cross-linking agent. Then, it was centrifuged and washed three times at 10,000 rpm, and the nanoparticle powder was obtained after freeze-drying. A portion of the nanoparticle suspension was taken to measure its hydrated particle size and zeta potential using a nano-laser particle size and zeta potential instrument.
[0129] Table 17 Hydration particle size and zeta potential of albumin nanoparticles
[0130]
[0131]
[0132] It can be seen from Table 17 that composite protein particles can be prepared in the pH range of 6 to 11. When the solution pH is 1 or 2, no nanoparticles are obtained after multiple high-speed centrifugation of the product solution, indicating that this pH condition is not sufficient to form stable nanospheres. Fine control of the solution pH is crucial for the synthesis of such composite protein nanomaterials.
[0133] Example 10
[0134] The hydroxyapatite of Example 8 was ultrasonically dispersed in 100 ml of albumin aqueous solution, and the albumin material concentration was 50 mg / ml; the ratio of hydroxyapatite to albumin material concentration was 1\8, the pH of the aqueous solution was adjusted to 10, acetone was added within 30 min, and after stabilization for 15 minutes, 100 μL of glutaraldehyde was added to obtain a covalently cross-linked particle suspension, wherein the volume of polar organic solvent acetone added was 0.5, 1, 2, 4, 8, 10, and 12 times the volume of the aqueous solution; the cross-linking reaction was carried out at room temperature for 12 h; after the cross-linking was completed, 1 g of glycine was added to remove the remaining cross-linking agent. Then, the mixture was centrifuged and washed three times at 10,000 rpm, and nanoparticle powder was obtained after freeze drying. A portion of the nanoparticle suspension was taken to determine whether particles were generated by nano-laser particle size.
[0135] Table 18 Particle generation of the prepared nanoparticle suspension
[0136] Acetone multiple Are there particles? 0.5 no 1 yes 2 yes 4 yes 8 yes 10 yes 12 Particle aggregation and precipitation
[0137] From the results in Table 18, it can be seen that when the volume ratio of organic solvent to water is in the range of 1 to 10, nanoparticle powder can be obtained.
[0138] Embodiment 11
[0139] The hydroxyapatite of Example 8 was ultrasonically dispersed in 100 ml of albumin aqueous solution, and the albumin material concentration was 50 mg / ml; the concentration ratio of hydroxyapatite to albumin material was 1\1, 1\2, 1\4, 1\8, 1\16, the pH of the aqueous solution was adjusted to 10, 200 mL of acetone was added within 30 min, and after stabilization for 15 minutes, 100 μL of glutaraldehyde was added to obtain a covalently cross-linked particle suspension, and the cross-linking reaction was carried out at room temperature for 12 h; after the cross-linking was completed, 1 g of glycine was added to remove the remaining cross-linking agent. Then, the mixture was centrifuged and washed three times at 10,000 rpm, and nanoparticle powder was obtained after freeze-drying. A portion of the nanoparticle suspension was taken to determine whether particles were generated by nano-laser particle size.
[0140] Table 19 Particle generation of the prepared nanoparticle suspension
[0141] Hydroxyapatite / albumin Are there particles? 1\1 no 1\2 no 1\4 no 1\8 yes 1\16 yes
[0142] From the results in Table 19, it can be seen that the mass ratio of hydroxyapatite to albumin ranges from 1\8 to 1\16, and nanoparticle powder can be obtained.
[0143] Example 12 (different kernels)
[0144] First, silica nanoparticles, calcium silicate nanoparticles, tricalcium phosphate, calcium carbonate, nanoclay particles, and bioglass nanoparticles were ultrasonically dispersed in 100 ml of albumin aqueous solution, and the concentration of albumin material was 50 mg / ml; the ratio of the above materials to the albumin material concentration was 1\8, the pH of the above aqueous solution was adjusted to 10, 200 mL of acetone was added within 30 minutes, and after stabilization for 15 minutes, 100 μL of glutaraldehyde was added to obtain a covalently cross-linked particle suspension, and the cross-linking reaction was carried out at room temperature for 12 hours; after the cross-linking was completed, 1 g of glycine was added to remove the remaining cross-linking agent. Then, the mixture was centrifuged and washed three times at 10,000 rpm, and the albumin nanoparticle powder was obtained after freeze drying. A portion of the nanoparticle suspension was taken to measure its hydrated particle size and zeta potential by a nano-laser particle size and zeta potential instrument.
[0145] Table 20 Hydration particle size and zeta potential of albumin nanoparticles
[0146] Silicon dioxide Calcium silicate Tricalcium phosphate Calcium carbonate Nano Clay Bioglass Particle size (nm) 598.6 497.3 491.8 557.9 893.4 462.2 Potential (mV) -11.9 -23.5 -21.6 -17.9 -13.8 -18.6
[0147] Comparative Example 1
[0148] Albumin powder and gelatin powder were dissolved in water to obtain a 200 mg / mL solution. At room temperature, 200 mg / mL albumin is a liquid, while gelatin can form a gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer, and the results are shown in Table 21. At the same concentration, the modulus of the albumin particles is higher than that of the albumin solution.
[0149] Table 21 Storage modulus of albumin and gelatin
[0150] Albumin solution Gelatin solution Storage modulus(KPa) 0.035 12.24
[0151] Example 13 (Nanoparticle cross-linking)
[0152] 1. 0.3 g of albumin particle powder and 1 mL of deionized water were mixed with 10 mg (10 mg / mL), 100 mg (100 mg / mL), and 500 mg (500 mg / mL) of 8-arm PEG-NHS (molecular weight 5000) respectively, and then repeatedly blown 10 times through a Luer adapter syringe to obtain a cross-linked albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0153] After obtaining the albumin nanoparticle gel according to the above formula, the gel was immersed in PBS at 37°C to measure its swelling value. The results are shown in Table 22.
[0154] The albumin nanoparticle gel was prepared according to the above formula, and a cylindrical gel was obtained using a mold with a diameter of 5 mm and a height of 10 mm. The mechanical properties of the gel were measured by a universal mechanical testing machine. The compression speed was 1 mm / min. The stress-strain curve is shown in Figure 7-1 shown.
[0155] Table 22 Storage modulus and swelling percentage of albumin nanoparticle gel
[0156] Amount of PEG 10mg / mL 100mg / mL 500mg / mL Storage modulus (Kpa) 45.71 50.696 168.32 Swelling value (%) 250.45 160.23 150.56
[0157] 2. Mix albumin / hydroxyapatite (0.3 g albumin, 100 mg HA) mixed particle powder and 1 mL deionized water with 10 mg (10 mg / mL), 100 mg (100 mg / mL), and 500 mg (500 mg / mL) 8-arm PEG-NHS, respectively, and repeatedly blow 10 times through a Luer adapter syringe to obtain a cross-linked albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0158] After obtaining the albumin albumin-hydroxyapatite nanoparticle gel according to the above formula, the gel was immersed in PBS at 37°C to measure its swelling value. The results are shown in Table 23.
[0159] The albumin / hydroxyapatite nanoparticle gel was prepared according to the above formula, and a cylindrical gel was obtained using a mold with a diameter of 5 mm and a height of 10 mm. The mechanical properties of the gel were measured by a universal mechanical testing machine. The compression speed was 1 mm / min. The stress-strain curve is shown in Figure 7-2 shown.
[0160] Table 23 Storage modulus and swelling percentage of albumin particle gel
[0161]
[0162]
[0163] 3. Mix albumin / HA-NH2 (0.3 g albumin and 100 mg HA-NH2) mixed particle powder and 1 mL deionized water with 10 mg (10 mg / mL), 100 mg (100 mg / mL), and 500 mg (500 mg / mL) 8-arm PEG-NHS, respectively, and then repeatedly blow 10 times through a Luer adapter syringe to obtain a cross-linked albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0164] After obtaining the albumin-hydroxyapatite nanoparticle gel according to the above formula, the gel was immersed in PBS at 37°C to measure its swelling value. The results are shown in Table 24.
[0165] The albumin-hydroxyapatite nanoparticle gel was prepared according to the above formula, and a cylindrical gel was obtained using a mold with a diameter of 5 mm and a height of 10 mm. The mechanical properties of the gel were measured by a universal mechanical testing machine. The compression speed was 1 mm / min. The stress-strain curve is shown in Figure 7-3 shown.
[0166] Table 24 Storage modulus and swelling percentage of albumin-hydroxyapatite nanoparticle gel
[0167] 10mg / mL 100mg / mL 500mg / mL Storage modulus (Kpa) 152.89 224.46 418.41 Swelling (%) 184.32 153.47 131.26
[0168] 4. 0.3 g of albumin@HA particle powder and 1 mL of deionized water were mixed with 10 mg (10 mg / mL), 100 mg (100 mg / mL), and 500 mg (500 mg / mL) of 8-arm PEG-NHS, respectively, and then repeatedly blown 10 times through a Luer adapter syringe to obtain a cross-linked albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0169] After obtaining the albumin-hydroxyapatite nanoparticle gel according to the above formula, the gel was immersed in PBS at 37°C to measure its swelling value. The results are shown in Table 25.
[0170] The albumin-hydroxyapatite nanoparticle gel was prepared according to the above formula, and a cylindrical gel was obtained using a mold with a diameter of 5 mm and a height of 10 mm. The mechanical properties of the gel were measured by a universal mechanical testing machine. The compression speed was 1 mm / min. Figure 7-4 shown.
[0171] Table 25 Storage modulus and swelling percentage of albumin-hydroxyapatite nanoparticle gel
[0172] 10mg / mL 100mg / mL 500mg / mL Storage modulus (Kpa) 63.19 180.34 230.52 Swelling (%) 174.94 163.8 152.64
[0173] Comparative Example 2
[0174] 0.3 g of albumin powder, 1 mL of deionized water, and 10 mg (10 mg / mL), 100 mg (100 mg / mL), and 500 mg (500 mg / mL) of 8-arm PEG-NHS with a molecular weight of 5000 were mixed and repeatedly blown 10 times through a Luer adapter syringe to obtain a cross-linked albumin gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0175] Table 26 Storage modulus of gels prepared from albumin powder
[0176] 10mg / mL 100mg / mL 500mg / mL Storage modulus (Kpa) 24.35 50.24 134.12
[0177] Compared with Table 26, it can be seen that at the same concentration, the storage modulus of the cross-linked albumin nanoparticles is higher than that of the albumin hydrogel before cross-linking.
[0178] Example 14 (different cross-linking agents)
[0179] 0.3 g of albumin particle powder and 1 mL of deionized water were mixed with 100 mg of 5000 molecular weight linear, 4-arm, 8-arm PEG-NHS, and hyperbranched PEG-NHS, respectively, and then repeatedly blown 10 times through a Luer adapter syringe to obtain a cross-linked albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0180] Table 27 Storage modulus of cross-linked albumin gel
[0181] PEG Type Linear PEG-NHS 4-Arm PEG-NHS 8-Arm PEG-NHS Hyperbranched PEG-NHS Storage modulus (Kpa) 29.52 33.32 50.696 83.14
[0182] 0.3 g of albumin particle powder and 1 mL of deionized water were mixed with 100 mg of 8-arm PEG-NHS with molecular weights of 5000, 10000, and 20000, respectively, and then repeatedly blown 10 times through a Luer adapter syringe to obtain a cross-linked albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0183] Table 28 Storage modulus of cross-linked albumin gel
[0184] PEG molecular weight 5000 10000 20000 Storage modulus (Kpa) 50.696 33.60 11.61
[0185] 0.3 g of albumin particle powder and 1 mL of deionized water were mixed with 100 mg of PF127-NHS (Shenzhen Meiluo Technology Co., Ltd.), PF108-NHS (Shenzhen Meiluo Technology Co., Ltd.), sodium alginate-NHS (Qiyue Biotechnology), hyaluronic acid-NHS (Shaanxi Xingbei Aike Biotechnology), chondroitin sulfate-NHS (Ruixi Biotechnology), dextran-NHS (Ruixi Biotechnology), cellulose-NHS (Qiyue Biotechnology), polyacrylic acid-NHS (Qiyue Biotechnology), and agarose-NHS (Beike Nanotechnology), and then repeatedly blown 10 times through a Luer adapter syringe to obtain a cross-linked albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0186] Table 29 Storage modulus of cross-linked albumin gel
[0187]
[0188]
[0189] Example 15 (different groups)
[0190] 0.3 g of albumin particle powder and 1 mL of deionized water were mixed with 100 mg of maleimide polyethylene glycol with a molecular weight of 5000, epoxy polyethylene glycol, aldehyde polyethylene glycol, and carboxyl-terminated polyethylene glycol (molecular weight 5000), respectively, and then repeatedly blown 10 times through a Luer adapter syringe to obtain a cross-linked albumin particle gel. The storage modulus G' of the particle gel was obtained using the time scan mode of the rotational rheometer.
[0191] Table 30 Storage modulus of cross-linked albumin gel
[0192] Group Type Maleimide Epoxy Aldehyde carboxyl Storage modulus (Kpa) 39.8 15.26 31.10 18.79
[0193] Example 16 (Adhesive Application)
[0194] Using the nanoparticle hydrogel in Example 8.3, 0.3g albumin@HA+PEG-NHS: 0.3g of albumin@HA particle powder and 1mL of deionized water were mixed with 10mg (10mg / mL), 100mg (100mg / mL), and 500mg (500mg / mL) of 8-arm PEG-NHS, respectively, and then repeatedly blown through a Luer adapter syringe and overlapped and bonded to the surface of two bone pieces (5.0cm×2.0cm rectangle), where the overlap area is (1.5cm×2.0cm rectangle). A tensile tester with a 500N force sensor was used to shear and peel the overlapped samples (peeling rate: 10mm / min), and the stress-strain curve of the peeling process was obtained, and the bonding strength was defined by the maximum stress point of the curve. At the same time, the curing time of the corresponding component materials was measured: the timing started immediately after the material was extruded, and when the bone pieces could not be bonded together, the material was considered to be completely cured. As can be seen from Table 31, the bonding strength of the nanoparticle hydrogel of the present invention is higher than that of a pure polymer system or a single nanoparticle system, and is also higher than commercially available protein adhesive products.
[0195] Table 31 Adhesion strength and curing time of different nanoparticle hydrogels
[0196] 10mg / mL 100mg / mL 500mg / mL Adhesion strength (Kpa) 100.25±23.73 180.13±27.88 5300.52±96.89 Curing time(s) 268.39±12 124.92±7.88 52.12±14.8
[0197] Comparative Example 3
[0198] 1. After 0.3g of albumin particle powder and 1mL of deionized water are mixed evenly, they are quickly overlapped and bonded on the surface of two bone pieces (5.0cm×2.0cm rectangle), where the overlap area is (1.5cm×2.0cm rectangle). Use a tensile tester with a 500N force sensor to perform shear peeling (peeling rate: 10mm / min) on the overlapped samples, and obtain the stress-strain curve of the peeling process. The maximum stress point of the curve is used to define the bonding strength.
[0199] 2. After 0.3g of albumin particle powder, 100mg HA and 1mL of deionized water were mixed evenly, they were quickly overlapped and bonded on the surface of two bone pieces (5.0cm×2.0cm rectangle), where the overlap area was (1.5cm×2.0cm rectangle). A tensile tester with a 500N force sensor was used to perform shear peeling (peeling rate: 10mm / min) on the overlapped samples to obtain the stress-strain curve of the peeling process, and the maximum stress point of the curve was used to define the bonding strength.
[0200] 3. Bio-glue (purchased from Cryolife) was overlapped and bonded to the surface of two bone pieces (5.0 cm × 2.0 cm rectangle), where the overlap area was (1.5 cm × 2.0 cm rectangle). A tensile tester with a 500N force sensor was used to perform shear peeling (peeling rate: 10 mm / min) on the overlapped samples to obtain the stress-strain curve of the peeling process, and the maximum stress point of the curve was used to define the bonding strength.
[0201] 4. Fibrin glue (Yueling brand) was overlapped and bonded to the surface of two bone pieces (5.0 cm × 2.0 cm rectangle), where the overlap area was (1.5 cm × 2.0 cm rectangle). A tensile tester with a 500N force sensor was used to perform shear peeling (peeling rate: 10 mm / min) on the overlapped samples to obtain the stress-strain curve of the peeling process, and the maximum stress point of the curve was used to define the bonding strength.
[0202] Table 32 Adhesion strength of different types of nanoparticle hydrogels
[0203] Examples Adhesion strength Example 16 180.13Kpa Comparative Example 3.1 115.11Kpa Comparative Example 3.2 14.63Kpa Comparative Example 3.3 17.56Kpa Comparative Example 3.4 14.6Kpa
[0204] Example 17 (Application of bone filling)
[0205] Using the nanoparticle hydrogel in Example 8.3, 0.3g albumin@HA+100mgPEG-NHS: 0.3g of albumin@HA particle powder, 1mL of deionized water and 100mg (100mg / mL) 8-arm PEG-NHS were mixed and repeatedly blown through a Luer adapter syringe, and then quickly squeezed into the bone defect site to fill the bone defect.
[0206] Comparative Example 4
[0207] Medical CA glue (brand: Baiyun) was used as a control and squeezed into the bone defect to fill the bone defect.
[0208] The results are as follows Figure 8 As shown, from Figure 8 It can be seen that, compared with medical CA glue, the nanoparticle hydrogel of the present invention has a better filling effect.
[0209] Example 18 (Liquid Environment)
[0210] Using the nanoparticle hydrogel in Example 8.3, 0.3 g BSA albumin @ HA + PEG-NHS: 0.3 g BSA albumin @ HA particle powder, 1 mL deionized water and 100 mg (100 mg / mL) 8-arm PEG-NHS were mixed and repeatedly blown through a Luer adapter syringe and then overlapped and bonded to the surface of two bone slices (5.0 cm × 2.0 cm rectangle) soaked in PBS ( Fig. 9), where the overlapped area is (1.5 cm × 2.0 cm rectangle). A tensile tester with a 500N force sensor was used to perform shear peeling on the overlapped sample (peeling rate: 10 mm / min), and a stress-strain curve of the peeling process was obtained, and the maximum stress point of the curve was used to define the bonding strength.
[0211] Comparative Example 5
[0212] Bio-glue (purchased from Cryolife) was overlapped and bonded to the surfaces of two bone slices (5.0 cm × 2.0 cm rectangle) soaked in PBS ( Fig. 9 ), where the overlapped area is (1.5cm×2.0cm rectangle). A tensile tester with a 500N force sensor was used to perform shear peeling on the overlapped sample (peeling rate: 10mm / min), and a stress-strain curve of the peeling process was obtained. The maximum stress point of the curve was used to define the bonding strength. It can be seen from the figure that the colloidal adhesive of the present invention can exist stably in a liquid environment, while Bio-glue will diffuse in the liquid, resulting in a decrease in bonding strength.
[0213] Table 33 Adhesion strength in a humid environment
[0214] Examples Adhesion strength Embodiment 18 200.54Kpa Comparative Example 5 11Kpa
[0215] Example 19 (Bone hemostasis application)
[0216] Using the nanoparticle hydrogel in Example 8.3, 0.3g albumin@HA+100mgPEG-NHS: 0.3g of albumin@HA particle powder, 1mL of deionized water and 100mg (100mg / mL) 8-arm PEG-NHS were mixed and repeatedly blown and squeezed out through a Luer adapter syringe to obtain a hydrogel), and the coagulation performance of the bone adhesive was investigated by an in vitro coagulation experiment. The specific implementation steps are as follows: First, 50μL of fresh blood was dripped onto the sample surface after the nanoparticle hydrogel gel. Next, after incubation in an oven at 37°C for 2-10min, the sample surface was rinsed with PBS solution, and the supernatant was taken to measure the absorbance of hemoglobin in the solution with a UV-visible spectrophotometer at a wavelength of 540nm.
[0217] Johnson's bone wax was used for in vitro coagulation experiments. The specific implementation steps are as follows: first, 50 μL of fresh blood was dropped onto the sample surface covered with bone wax. Next, the sample surface was incubated in an oven at 37°C for 2-10 min, and then the sample surface was rinsed with PBS solution. The supernatant was taken and the absorbance of hemoglobin in the solution was measured using a UV-visible spectrophotometer at a wavelength of 540 nm.
[0218] The results are as follows Fig.10As shown in the figure, it can be seen that the nanoparticle hydrogel of the present invention has a better effect of promoting blood coagulation than bone wax.
[0219] Example 20 (Cell Scaffold)
[0220] Taking the particle gel prepared by 0.3g albumin@HA+100mgPEG-NHS as an example, MC3T3-E1 cells were mixed with the hydrogel (cell concentration was 5.0×10 3 cells / mL), and extruded to obtain a cell-laden colloidal gel scaffold with stable mechanics; after culturing at 37°C and 5% carbon dioxide concentration for 72 h, the cells were stained with a fluorescent live / dead assay to evaluate the viability of the hydrogel-encapsulated cells, where green fluorescence represented live cells and red fluorescence represented dead cells.
[0221] The results are as follows Fig.11 As shown in the figure, it can be seen that the scaffold structure is clear and complete, and the survival rate of living cells is high. The material of the present invention can be used as a cell scaffold.
[0222] Example 21 (Drug-carrying application)
[0223] Taking the particle gel prepared by 0.3g albumin@HA+100mgPEG-NHS as an example, the drug release behavior was studied. First, the gel was mixed with arginine, vitamin D, and GLuc mRNA natural active factor VEGF. Then the gel was placed in PBS at 37°C and shaken on a shaker to simulate the in vivo environment. At the predetermined time point, the absorbance of the supernatant was measured with a UV-visible spectrophotometer and compared with the standard curve to determine the release amount at each time point.
[0224] Table 34 Cumulative release of various drugs at different time points
[0225] 1d 4d 7d 14d 28d Arginine 10.18% 16.84% 25.04% 33.48% 48.42% Vitamin D 13.99% 34.20% 51.26% 64.95% 78.95% GLuc mRNA 10.44% 25.82% 34.87% 73.87% 80.06% VEGF 16.80% 27.36% 49.68% 59.43% 63.20%
[0226] The above results indicate that albumin colloidal gel can be used as a drug carrier to ensure long-term drug release.
[0227] Example 22 (Cell experiment)
[0228] Taking the particle gel prepared by 0.3g albumin@HA+100mgPEG-NHS as an example, the biocompatibility of the material was investigated by in vitro cell culture experiments. The specific implementation steps are as follows: After the adhesive is extruded, solidified, and freeze-dried, the gel is soaked in a culture medium (concentration 0.2g / mL) and set aside after 24 hours; bone marrow mesenchymal stem cells (MC3T3-E1 pre-osteoblast cell line) are digested with trypsin and inoculated on the surface of the adhesive, the culture medium is aspirated and replaced with gel extract, and then cultured at 37°C and 5% carbon dioxide concentration for 72 hours. The cells in the gel extract are evaluated by fluorescent live / dead assay to evaluate the effect of hydrogel on cell viability, where green fluorescence represents live cells and red fluorescence represents dead cells.
[0229] The results are as follows Fig.12 As shown, the results indicate that the adhesive has good biocompatibility.
[0230] Example 23 (Subcutaneous Implantation Experiment)
[0231] The particle gel prepared using 0.3g albumin@HA+100mgPEG-NHS was injected subcutaneously on both sides of the mouse using a 22G needle, with a total of 100μL of gel material: the mice were killed after 1, 4, 8 and 12 weeks of feeding, and the implanted materials were removed and weighed to evaluate the material's in vivo degradation performance.
[0232] 100 mg of CA gel was injected subcutaneously into both sides of the mouse using a 22G needle, with a total of 100 μL of gel material. The mice were killed after 1, 4, 8, and 12 weeks of feeding, and the implanted materials were removed and weighed for comparison of degradation performance.
[0233] Table 35 Degradation rate of granular gel material at different time points
[0234] time Albumin degradation rate (%) CA degradation rate (%) 1 week 13.88 1.54 4 weeks 20.26 3.21 8 weeks 44.25 8.85 12 weeks 53.03 13.48
[0235] The above results indicate that the composite protein particle gel of the present invention can stably fill the subcutaneous tissue of mice for 12 weeks.
[0236] Example 24 (In vitro osteogenesis experiment)
[0237] The particle gel was prepared using 0.3g albumin@HA+100mgPEG-NHS. Tissue adhesive or CA glue was injected into the bottom of a 24-well plate, sterilized after complete solidification, and then washed 3 times with PBS. MC-3T3-E1 cells (5×10 4 Cells were inoculated into well plates (1000 cells / well) and cultured in DMEM containing 2.5% FBS for 7 and 14 days. Cell mineralization and ALP secretion were observed under a light microscope using an Alizarin red staining kit and an ALP staining kit, respectively.
[0238] Compared with CA glue and the blank group, the tissue adhesive of the present invention showed more blue precipitation and more red calcium nodules ( Fig.13 ). This indicates that the tissue adhesive of the present invention has a more excellent osteogenic effect.
Claims
1. A hydrogel tissue adhesive composed of organic / inorganic particles and polymer chains, characterized in that: The hydrogel tissue adhesive comprises micron or nanometer organic particles carrying amino groups, water-soluble high molecular polymers that undergo chemical cross-linking reactions with amino groups, and micron or nanometer inorganic particles that promote osteogenesis; the mass ratio of organic particles, inorganic particles, and water-soluble high molecular polymers is 1-20:1:0.1-5; the volume percentage of particles in the hydrogel tissue adhesive is 10-80%; the organic / inorganic particles are formed by mixing organic particles and inorganic particles, or are composite particles with a core-shell structure formed by organic particles wrapping inorganic particles. Under the action of water, the hydrogel tissue adhesive can form a continuous, porous particle network through covalent and / or reversible non-covalent interactions between particles, giving the hydrogel tissue adhesive injectability, plasticity, and self-repairing properties.
2. The hydrogel tissue adhesive according to claim 1, characterized in that The particle size is 1nm~50μm; under neutral conditions, the particle potential is -30mv~+30mv.
3. The hydrogel tissue adhesive according to claim 1, characterized in that The component of the micron or nanometer organic particles carrying amino groups is one or a combination of two or more of gelatin, chitosan, polylysine, polyethyleneimine, albumin, protamine, fibrin, silk protein, and silkworm epidermal protein; the molecular weight of the component of the micron or nanometer organic particles carrying amino groups is 0.5-100 kDa; The micron or nanometer inorganic particles that promote osteogenesis account for ≥10wt% of the dry weight of the hydrogel tissue adhesive; the inorganic particles are inorganic non-metallic material particles of calcium phosphate, calcium carbonate, calcium silicate, and bioglass; and the morphology is one or a combination of two or more of the following: needle-like, fibrous, granular, and block-like; The active groups of the water-soluble high molecular polymer that undergo chemical cross-linking reaction with the amino group include but are not limited to the following groups: succinimide, aldehyde, maleimide, epoxy, carboxyl; the skeleton of the water-soluble high molecular polymer that undergoes chemical cross-linking reaction with the amino group is one or a combination of two or more of polyethylene glycol, polyacrylic acid, block polyether F-127, block polyether F-108, sodium alginate, hyaluronic acid, chondroitin sulfate, dextran, cellulose, and agarose.
4. The hydrogel tissue adhesive according to claim 3, characterized in that: The surfaces of the inorganic particles are modified with amino groups. The process of modifying the surfaces of the inorganic particles with amino groups is as follows: the inorganic particles are added into n-hexane to obtain a 1-500 mg / mL uniform dispersion, and then 3-aminopropyltriethoxysilane which reacts with the hydroxyl groups on the surfaces of the inorganic particles is added, stirred at 50-80° C. for 4-12 hours, and the amino-modified inorganic particles are obtained after freeze-drying.
5. The hydrogel tissue adhesive according to claim 3, characterized in that: The water-soluble high molecular polymer has a linear, multi-arm, or hyperbranched shape, a molecular weight of 0.5-100 kDa, and the water-soluble high molecular polymer accounts for 10-50 wt% of the dry weight of the hydrogel tissue adhesive, and the molar ratio of amino groups to reactive groups in the polymer chain is 0.1-100.
6. The method for preparing the hydrogel tissue adhesive according to any one of claims 1 to 5, characterized in that: There are two methods: Method 1: includes the following steps: (1) Preparation of micrometer or nanometer organic particles carrying amino groups: a) When the size of the prepared particles is greater than 5 μm, the preparation process is as follows: dissolving the raw materials in water at 20° C. to 60° C. to obtain an aqueous solution with a concentration of 1 to 100 mg / mL, adding a crosslinking agent, stirring and crosslinking at room temperature for 1 to 20 hours, removing the remaining crosslinking agent, and preparing microsphere particles by spray drying; b) When the size of the prepared particles is 1 nm-5 μm and the raw materials are gelatin, polylysine, polyethyleneimine, albumin, and protamine, the raw materials are dissolved in water at 20° C. to 60° C. to obtain an aqueous solution with a concentration of 1 to 100 mg / mL; the pH of the aqueous solution is adjusted to 9 to 14, and a polar organic solvent of 1 to 10 times the volume of the aqueous solution is added dropwise to the aqueous solution, and after stirring for 5 to 60 minutes, a cross-linking agent is added, and the cross-linking is stirred at room temperature for 1 to 20 hours, and the remaining cross-linking agent is removed, and a micro-nano particle dispersion is obtained after washing, and a particle powder is obtained after freeze-drying; c) When the size of the prepared particles is 1 nm-5 μm and the raw material is chitosan, the preparation process is the same as step b), the only difference is that the pH of the aqueous solution is adjusted to 3-5; d) When the size of the prepared particles is 1 nm-5 μm and the raw material is silk fibroin, firstly, natural silk cocoons are degummed to obtain silk fibroin fibers, and then dissolved in an aqueous solution of lithium bromide or an aqueous solution of calcium chloride / ethanol to obtain a regenerated silk fibroin solution with a concentration of 0.01-0.1 g / mL, and then vacuum freeze-dried to obtain soluble freeze-dried silk fibroin, and then the particles are prepared according to step b). (2) Preparation of hydrogel tissue adhesive: The preparation method is obtained by uniformly mixing the micron or nanometer organic particles carrying amino groups prepared in step (1), the water-soluble high molecular polymer that undergoes chemical cross-linking reaction with the amino groups, and the micron or nanometer inorganic particles having the function of promoting osteogenesis. Method 2: includes the following steps: 1) Preparation of composite particles with core-shell structure: The inorganic particles as the inner core layer are ultrasonically dispersed in an aqueous solution in which an organic polymer of the outer shell layer is dissolved, and the concentration of the outer shell material is 1 to 100 mg / mL; the concentration ratio of the inner core material to the outer shell material is 1:2 to 1:50, and the pH is adjusted to 9 to 14. A polar organic solvent is added dropwise to the aqueous solution, and the volume of the polar organic solvent added is 1 to 10 times the volume of the aqueous solution. After stabilization for 10 to 30 minutes, a crosslinking agent is added, and a crosslinking reaction is carried out at room temperature for 1 to 12 hours to obtain a micro-nano particle suspension with a core-shell structure, and the remaining crosslinking agent is removed. After washing, a core-shell particle dispersion is obtained, and after drying, a composite particle powder with a core-shell structure is obtained. 2) Preparation of hydrogel tissue adhesive: The core-shell structure composite particles prepared in step 1) and the water-soluble high molecular polymer that undergoes chemical cross-linking reaction with the amino group are uniformly mixed to obtain the composite particles.
7. The preparation method according to claim 6, characterized in that: The polar organic solvent is one or a mixed solvent of two or more selected from methanol, ethanol, isopropanol, butanol, acetone, acetonitrile and tetrahydrofuran; the cross-linking agent is one or a combination of two or more selected from carbodiimide / N-hydroxysuccinimide, glyceraldehyde, glutaraldehyde, formaldehyde, paraformaldehyde, succinaldehyde and genipin.
8. The method for using the hydrogel tissue adhesive according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: uniformly mixing the hydrogel tissue adhesive according to any one of claims 1 to 5 and water, repeatedly blowing 5 to 25 times through a Luer adapter syringe to obtain an injectable gel and then squeezing it out.
9. Use of the hydrogel tissue adhesive according to any one of claims 1 to 5 as a bone tissue adhesive.
10. Use of the hydrogel tissue adhesive according to any one of claims 1 to 5 as a drug carrier or a cell carrier.
Citation Information
Patent Citations
Preparation method of mesoporous apatite nano-drug carrier with pH responsiveness and cellular targeting property for hepatoma cell
CN104587488A
Gelatin / gellan gum / hydroxyapatite composite hydrogel and preparation method thereof
CN111793225A
Preparation method of bionic scaffold loaded with lysophosphatidic acid nanoparticles
CN113827768A
Preparation method and application of silk fibroin / hydroxyapatite composite micro-nano particle material
CN115054733A
Synergistic osteogenesis dynamic enhanced crosslinking method for inorganic composite hydrogel
CN116763996A
Cited By
Degradable bone filling material as well as preparation method and application thereof
CN119424744A
Injectable self-healing self-assembly milt extract hydrogel as well as preparation method and application thereof
CN119971124A
Patterned biological barrier membrane with self-adhesion function and preparation method thereof