Manufacturing method of precious metal seamless thin-walled tube
Through the production method of seamless thin-walled pipes and the use of spinning processing and annealing technology, the problems of weld cracking and corrosion of precious metal pipes in high-temperature environments are solved, the uniformity and strength of the pipe wall are achieved, and the service life is extended.
Patent Information
- Application Number
- CN202410854193.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-25
AI Technical Summary
Existing precious metal pipes are prone to weld cracking and corrosion problems in high-temperature environments, and the materials are easily contaminated during the welding process, affecting the quality and service life of the finished product.
The production method of seamless thin-walled pipes is adopted. By smelting precious metal raw materials into ingots and then annealing and forging them, a plate with a thickness greater than the wall thickness of the finished pipe is formed, and then cut into ring-shaped raw materials, and the mold assembly is used for multiple spinning processes. and annealed until a seamless thin-walled tube blank is formed, avoiding welding processes.
It realizes the seamless forming of precious metal pipes, avoids quality problems at the welding position, ensures the uniformity and strength of the pipe wall, extends the service life, and avoids cracking and corrosion in high temperature environments.
Smart Images

Figure CN118831992A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of precious metal product production, in particular to a method for manufacturing a precious metal seamless thin-walled tube. Background Art
[0002] Precious metals or precious metal alloys are often used as smelting tools when melting liquid crystal glass, optical glass, microcrystalline glass or pharmaceutical glass; common precious metals include platinum, rhodium, palladium, iridium, osmium, gold, silver, etc. Precious metal alloys formed by solid solution strengthening mainly include platinum-rhodium alloy, platinum-yellow alloy, platinum-iridium alloy, etc. Precious metal alloys strengthened by dispersion include platinum-rhodium dispersion, platinum-iridium dispersion, etc. In the process of melting glass, the glass at high temperature is clarified and homogenized by precious metal tools, and finally forms solid glass in the form of plates, blocks or tubes.
[0003] The main shape of precious metal smelting tools is a round tube, i.e. a precious metal tube. A common method of making a precious metal tube is to roll the precious metal ingot into a plate that meets the design thickness of the precious metal tube, and then form the plate into a round tube after heat treatment, tube rolling, welding, roundness correction and other processes; since the finished product will have a weld after welding, and the weld is in a cast state, the strength of the weld is lower than the strength of the base material. Even if the weld can be eliminated and leveled by forging, the precious metal tube is in a high-temperature working environment for a long time, and the weld is still very weak, and it is easy to crack at the weld. Another method of making a precious metal tube is to melt the precious metal material and cast it into a cylinder, and then extrude it at room temperature; but the precious metal material is prone to cracking during the extrusion process, resulting in the scrapping of the material; even if it is improved to a hot extrusion method, the precious metal material needs to be in high-temperature contact with the extrusion die during the extrusion process, which is easy to cause the precious metal material to be contaminated, and the precious metal is easily corroded in the subsequent high-temperature working environment, which leads to leakage of the precious metal tube.
[0004] The Chinese invention patent application with publication number CN113714321A discloses a refractory and rare precious metal pipe and its preparation method, including selecting rare precious metal plates with a thickness of millimeters after annealing; selecting different bending methods according to the sizes of different rare precious metal blanks and plates, laser and / or electron beam welding the butt surfaces to form a welded seamless pipe blank; shaping, welding seam grinding, heat treatment; then rolling the welded seamless pipe blank into pipes; acid and alkali washing the rolled pipes. The refractory and rare precious metal pipes prepared by the inventive method can significantly improve the yield rate, have good tensile strength and elongation, and the yield rate is increased by more than 30%, which can improve the utilization rate of refractory rare precious metal raw materials and has broad application prospects.
[0005] Although the technical solution disclosed in the above patent application can improve the yield rate of precious metal pipes, the performance of the precious metal pipes is mainly to improve the tensile strength and elongation of the pipes. In addition, when preparing the precious metal pipes, the plates need to be bent and welded, and welds still exist on the pipes, which cannot solve the problem of cracking easily occurring at the welds. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for manufacturing a seamless thin-walled precious metal tube, which can effectively improve the quality of the finished product and the service life of the precious metal tube.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for manufacturing a precious metal seamless thin-walled tube, which comprises the following steps:
[0008] S1. Melt the precious metal raw materials into ingots, forge the ingots after annealing, and cool, clean, and deburr the ingots if there is no cracking during forging;
[0009] S2, rolling and annealing the ingot obtained in S1 until a plate having a thickness greater than 2 to 3 mm of the wall thickness of the finished tube is obtained;
[0010] S3, annealing the plate obtained in S2 and then cooling it, leveling the plate, and then cutting it into a ring-shaped raw material, wherein the inner ring diameter of the ring-shaped raw material is smaller than the inner diameter of the finished pipe, and the ring width of the ring-shaped raw material is larger than the length of the finished pipe;
[0011] S4, prepare a mold assembly consisting of a first mold and a second mold, wherein the first mold is a cylinder whose diameter matches the inner diameter of the finished pipe, the length of the first mold is greater than the ring width of the circular ring-shaped raw material, a rotating shaft is fixed to one end of the first mold, and the other end of the first mold is detachably connected to the second mold, and the second mold is a circular plate structure whose diameter is equal to the inner ring diameter of the circular ring-shaped raw material and smaller than the diameter of the first mold, connect the first mold and the second mold, and sleeve the circular ring-shaped raw material on the second mold, so that the first mold, the circular ring-shaped raw material and the second mold are coaxially assembled;
[0012] S5, repeatedly performing spinning and annealing on the assembly structure obtained in S4, during the spinning process, the rotating shaft of the first mold is connected to the lathe for transmission, and the top pin of the lathe is pressed against the end face of the second mold, and the thickness of the annular raw material is gradually reduced by the spinning process, and the annular raw material is gradually attached to the surface of the first mold, until the thickness difference between the thickness of the annular raw material and the wall thickness of the finished pipe is ±0.05mm, and the distance between the edge of the annular raw material and the end face of the first mold close to the second mold reaches 25-35mm, and the blank of the precious metal seamless thin-walled tube is formed;
[0013] S6. Remove the blank from the mold assembly, trim the front and rear ends of the blank according to the length of the finished pipe, clean it, and complete the preparation after it passes the leakage test.
[0014] As an improvement of the above scheme: in step S1, the weight of the precious metal raw material is 3 to 5 times the weight of the finished pipe; after the precious metal raw material is smelted to obtain ingots, samples are taken to analyze the impurity elements and main component contents, and if they meet the requirements, the surface of the ingot is wiped with alcohol and then annealed.
[0015] As an improvement of the above scheme: in the step S1, the annealing time is 30 to 60 minutes, and the annealing temperature is 1350 to 1500°C; when forging the ingot, a 2 to 5 ton forging hammer is used to forge six sides, and if cracking occurs during forging, the ingot is re-purified and smelted; when cooling the ingot, the ingot is placed on a pad made of alumina or zirconia and cooled to room temperature; when cleaning the ingot, the six sides of the ingot are first milled off on a milling machine, and the removal thickness is 0.1 to 0.15 mm, and the surface roughness of the ingot reaches Ra1.6.
[0016] As an improvement of the above scheme: in the step S2, the pressing amount each time when rolling the ingot is 0.5-1 mm, one side of the ingot is rolled first, and then the other side is rolled in the opposite direction after annealing, and the rolling lengths of the two sides are equal; the annealing time is 30-60 minutes, and the annealing temperature is 1350-1550°C.
[0017] As an improvement of the above scheme: in the step S3, the annealing time is 30 to 60 minutes, and the annealing temperature is 1350 to 1550° C.; after annealing, the plate is air-cooled to room temperature; the flatness of the plate after leveling is within ±0.01 to 0.2 mm; the inner ring diameter of the cut circular ring-shaped raw material is 50 to 70 mm smaller than the inner diameter of the finished pipe, and the outer ring diameter of the circular ring-shaped raw material is 10 to 15 mm smaller than the length of the plate.
[0018] As an improvement of the above scheme: in the step S4, the hardness of the first mold is 60-65HRC, the quenching depth is 2-3mm, the surface roughness of the circumferential surface is Ra<0.4, the length of the first mold is 50-100mm greater than the length of the finished pipe, the surface roughness of the end face of one end of the rotating shaft of the first mold is Ra0.8-1.6, and the surface roughness of the end face of one end of the rotating shaft of the first mold is not set to Ra<0.4; the thickness of the second mold is 10-20mm; the first mold and the second mold are threadedly connected with the stud through the threaded hole, the threaded hole is set on the first mold, and the stud is set on the second mold; after the first mold and the second mold are connected, the opposite end faces of the two are completely fitted.
[0019] As an improvement of the above scheme: in the step S5, when the first spinning process is performed, the thickness of the ring-shaped raw material is processed to be 1.5 to 2.5 mm greater than the wall thickness of the finished pipe, and the ring-shaped raw material forms an angle of 140° to 150°; then annealing is performed at an annealing temperature of 1350 to 1450° C. for 30 to 60 minutes, and then cooled to room temperature.
[0020] As an improvement of the above scheme: in the step S6, during the secondary spinning process, the thickness of the ring-shaped raw material is processed to be 1.0 to 1.5 mm greater than the wall thickness of the finished pipe, and the ring-shaped raw material forms an angle of 80° to 100°; then annealing is performed at an annealing temperature of 1400 to 1500° C. for 60 to 90 minutes, and then cooled to room temperature.
[0021] As an improvement of the above scheme: in the step S6, when the spinning process is performed three times, the thickness of the ring-shaped raw material is processed to be greater than the wall thickness of the finished pipe by 0.5 to 1.0 mm, and the ring-shaped raw material forms an angle of 35° to 50°; then annealing is performed at an annealing temperature of 1400 to 1500° C. for 60 to 90 minutes, and cooled to room temperature.
[0022] The beneficial effects of the present invention are as follows: by improving the manufacturing method of the precious metal tube, the present invention does not need to perform welding treatment on the precious metal material, and can directly form the precious metal material into a one-piece precious metal seamless thin-wall tube, thereby effectively eliminating the quality problems caused by the presence of welds on the precious metal tube and avoiding cracks at the welding position; the present invention supports the ring-shaped raw material in a mold to shape it, and uses a face-to-face shaping method to ensure that the inner wall of the precious metal tube is not prone to defects, the wall thickness of the precious metal tube is uniform, and the quality of the finished product of the precious metal tube can be effectively improved. Even if it is in a high-temperature working environment for a long time, it is not easy to crack, corrode and other problems, thereby effectively improving the service life of the precious metal tube. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the mold assembly and the ring-shaped raw material in the present invention when they are not assembled;
[0024] Figure 2 It is a schematic diagram of the mold assembly and the ring-shaped raw material after being assembled in the present invention;
[0025] Figure 3 It is a schematic diagram of the state after the first spinning process is performed on the ring-shaped raw material in the present invention;
[0026] Figure 4 for Figure 3 Side view of the raw material in the shape of a middle ring;
[0027] Figure 5It is a schematic diagram of the state after the ring-shaped raw material is subjected to secondary spinning processing in the present invention;
[0028] Figure 6 for Figure 5 Side view of the raw material in the shape of a middle ring;
[0029] Figure 7 This is a schematic diagram of the state after the ring-shaped raw material is subjected to three spinning processes in the present invention;
[0030] Figure 8 for Figure 7 Side view of the raw material in the shape of a middle ring;
[0031] Fig. 9 It is a schematic diagram of the state after the ring-shaped raw material is subjected to the spinning process in the present invention;
[0032] Fig.10 Schematic diagram of the cutting position of the blank.
[0033] Fig.11 It is a side view of the finished pipe finally obtained by the present invention.
[0034] Markings in the figure are: 100-finished pipe, 200-ring-shaped raw material, 300-first mold, 310-rotating axis, 400-second mold. DETAILED DESCRIPTION
[0035] In order to facilitate the understanding of the present invention, the present invention is further described below in conjunction with the accompanying drawings.
[0036] In the description of the present invention, it should be noted that the directions or positional relationships indicated by terms such as “front”, “rear”, “left”, “right”, “up”, “down”, and “inside” are based on the directions or positional relationships shown in the accompanying drawings and are only for the convenience of description. They do not indicate or imply that the device or component referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they cannot be understood as limitations on the present invention.
[0037] like Fig.11 As shown, the finished product 100 of the precious metal seamless thin-walled tube prepared by the present invention is a round tube structure with uniform wall thickness, and the whole is an integrally formed structure without welding treatment.
[0038] The present invention discloses a method for preparing the above-mentioned precious metal seamless thin-walled tube, and the preparation method is carried out in sequence according to the following steps:
[0039] S1. Prepare precious metal raw materials
[0040] According to the size of the finished tube 100 to be prepared, the precious metal raw materials of corresponding specifications are selected, and the weight of the precious metal raw materials is 3 to 5 times the weight of the finished tube 100; after taking the materials, the precious metal raw materials are melted into ingots, and the ingots are sampled and analyzed to analyze whether the impurity elements and main component contents of the ingots meet the requirements of the finished product. If the analyzed components meet the requirements, the surface of the ingot is wiped with alcohol and sent to an annealing furnace for annealing.
[0041] The annealing time in this step is 30 to 60 minutes, and the annealing temperature is 1350 to 1500°C. After the annealing treatment is completed, the ingot is taken out of the annealing furnace, and the ingot is placed on a 2 to 5 ton forging hammer to forge six sides respectively. During the forging process, observe whether the ingot cracks. If the ingot cracks, the ingot needs to be re-purified and smelted. If the ingot does not crack during the forging process, the forged ingot is placed on a pad made of alumina or zirconia to cool. After air cooling to room temperature, wipe the forging residual foreign matter left on the surface of the ingot with alcohol.
[0042] After cleaning, the cleaned ingot is placed on a milling machine, and the six sides of the ingot are removed by the milling machine. The removal thickness is 0.1 to 0.15 mm, so that the surface roughness of the ingot reaches Ra1.6; finally, a diamond file is used to remove the burrs on the edges and corners of the ingot, and the precious metal waste chips left after milling and filing are recycled.
[0043] S2. Rolling ingots
[0044] The ingot cleaned in step S1 is rolled. Before rolling, the surface of the ingot is wiped clean with alcohol. The pressing amount during rolling is controlled at 0.5-1 mm each time. The rolling work is carried out on two sides. After rolling on one side, the ingot is sent to an annealing furnace for annealing. The annealing time is 30-60 minutes and the annealing temperature is 1350-1550°C. After annealing, the rolling direction is changed until a plate having a thickness greater than 100 mm and a wall thickness of 2-3 mm of the finished pipe is obtained.
[0045] S3. Cutting the board
[0046] After the rolling process is completed, the plate obtained after rolling is sent to an annealing furnace for annealing, the annealing time is 30 to 60 minutes, and the annealing temperature is 1350 to 1550°C; after annealing, the plate is taken out and air-cooled to room temperature; then the plate is leveled, and the flatness of the plate after leveling is within ±0.01 to 0.2 mm; the leveled plate is cut, and the plate is cut into a circular raw material 200 by a laser cutting device, the outer ring diameter of the circular raw material 200 is smaller than the length of the plate by 10 to 15 mm, the inner ring diameter of the circular raw material 200 is smaller than the inner diameter of the finished pipe 100 by 50 to 70 mm, and the ring width of the circular raw material 200 is greater than the length of the finished pipe 100.
[0047] S4. Preparation of mold components
[0048] In the present invention, a mold assembly is used to assist in shaping the ring-shaped raw material 200. Figure 1 and Figure 2 As shown, the mold assembly consists of a first mold 300 and a second mold 400 .
[0049] Specifically, the main body of the first mold 300 is a cylinder, and a rotating shaft 310 is fixedly arranged at one end of the first mold 300. The rotating shaft 310 is coaxially arranged with the central axis of the first mold 300. The rotating shaft 310 is used to be connected with the lathe in a transmission manner in the subsequent spinning process, so that the lathe can drive the entire first mold 300 to rotate by driving the rotating shaft 310 to rotate; the diameter of the first mold 300 is adapted to the inner diameter of the finished pipe 100, and the diameter of the first mold 300 is slightly smaller than the inner diameter of the finished pipe 100, and the difference range is 0.1 to 0.2mm; the roundness and cylindricity of the first die 300 are controlled within ±0.05mm; the length of the first die 300 is greater than the ring width of the circular ring-shaped raw material 200, which is equivalent to limiting the length of the first die 300 to be greater than the length of the finished pipe 100, and the specific length difference range is 50-100mm, so that after the subsequent spinning process, the circular ring-shaped raw material 200 is completely covered on the first die 300, there will still be uncovered margin on the first die 300, thereby providing sufficient molding area for the circular ring-shaped raw material 200.
[0050] Furthermore, the two end faces of the first mold 300 have different roughnesses. Since the end face of the first mold 300 provided with the rotating shaft 310 is not a working face, this end face is used to cooperate with the lathe, so the roughness requirement is not high, and the surface roughness of this end face is limited to Ra0.8~1.6 in the present invention; the end face of the first mold 300 not provided with the rotating shaft 310 is a working face, and this end face needs to contact the annular raw material 200, so the roughness requirement is relatively high, and the surface roughness of this end face is limited to Ra<0.4 in the present invention. In addition, the hardness of the first mold 300 is 60~65HRC, and the quenching depth is 2~3mm.
[0051] Specifically, the second mold 400 is a circular plate, and the second mold 400 is mainly used to limit the circular ring-shaped raw material 200. The diameter of the second mold 400 is equal to the inner ring diameter of the circular ring-shaped raw material 200, and the diameter of the second mold 400 is smaller than the diameter of the first mold 300. The thickness of the second mold 400 is 10 to 20 mm.
[0052] The structure after the mold assembly used in the present invention is assembled with the ring-shaped raw material 200 is as follows: Figure 2As shown, the first mold 300 and the second mold 400 are threadedly connected through the threaded hole and the stud. In order to ensure that the end faces of the first mold 300 and the second mold 400 fit together, the threaded hole is set on the first mold 300, and the stud is fixed on the second mold 400. The aperture size range of the threaded hole is 20-25mm, and the depth size range is 40-60mm. The size parameters of the stud are compatible with the threaded hole; after the first mold 300 and the second mold 400 are threadedly connected, the opposite end faces of the two are completely fitted. The first mold 300, the annular raw material 200 and the second mold 400 are coaxially assembled, and the second mold 400 is embedded with the inner ring of the annular raw material 200, so that the annular raw material 200 is sleeved on the second mold 400.
[0053] S5. Spinning
[0054] After the mold assembly is assembled with the annular raw material 200, the resulting assembly structure is subjected to repeated spinning and annealing treatments. During the spinning process, the rotating shaft 310 of the first mold 300 is connected to the lathe, and the ejector pin of the lathe is pressed against the end surface of the second mold 400. Figures 3 to 9 As shown, the spinning process causes the circular ring-shaped raw material 200 to gradually fit against the surface of the first mold 300, and the thickness of the circular ring-shaped raw material 200 gradually decreases until the thickness difference between the thickness of the circular ring-shaped raw material 200 and the wall thickness of the finished tube 100 is ±0.05mm, and the distance between the edge of the circular ring-shaped raw material 200 and the end face of the first mold 300 close to the second mold 400 reaches 25 to 35mm, forming a blank of a precious metal seamless thin-walled tube.
[0055] In this step, multiple spinning processes are performed, and annealing is performed after each spinning process. Take three spinning processes as an example.
[0056] like Figure 3 and Figure 4 As shown, when the first spinning process is performed, an ultrasonic measuring instrument is used to monitor the thickness of the ring-shaped raw material 200 in real time during the spinning process, and the overall thickness of the ring-shaped raw material 200 is processed to be 1.5-2.5 mm greater than the wall thickness of the finished pipe 100, and an angle of 140°-150° is formed between the two sides of the ring-shaped raw material 200, and the thickness of the ring-shaped raw material 200 decreases from the center of the ring-shaped raw material 200 to the edge of the ring-shaped raw material 200; then annealing at an annealing temperature of 1350-1450°C for 30-60 minutes, and cooling to room temperature.
[0057] like Figure 5 and Figure 6As shown, when the secondary spinning process is performed, an ultrasonic measuring instrument is used to monitor the thickness of the ring-shaped raw material 200 in real time during the spinning process, and the overall thickness of the ring-shaped raw material 200 is processed to be greater than the wall thickness of the finished pipe 100 by 1.0 to 1.5 mm, and an angle of 80° to 100° is formed between the two sides of the ring-shaped raw material 200, and the thickness of the ring-shaped raw material 200 decreases from the center position of the ring-shaped raw material 200 to the edge of the ring-shaped raw material 200; then annealing is performed at an annealing temperature of 1400 to 1500°C for 60 to 90 minutes, and cooled to room temperature.
[0058] like Figure 7 and Figure 8 As shown, when the three spinning processes are performed, an ultrasonic measuring instrument is used to monitor the thickness of the ring-shaped raw material 200 in real time during the spinning process, and the overall thickness of the ring-shaped raw material 200 is processed to be greater than the wall thickness of the finished pipe 100 by 0.5 to 1.0 mm, and an angle of 35° to 50° is formed between the two sides of the ring-shaped raw material 200, and the thickness of the ring-shaped raw material 200 decreases from the center position of the ring-shaped raw material 200 to the edge of the ring-shaped raw material 200; then annealing is performed at an annealing temperature of 1400 to 1500°C for 60 to 90 minutes, and cooled to room temperature.
[0059] After the above-mentioned repeated spinning and annealing treatment, Fig. 9 As shown, the annular raw material 200 is finally made to completely fit on the surface of the first mold 300 to obtain a blank of a precious metal seamless thin-walled tube.
[0060] S6. Trimming
[0061] Remove the blank of the precious metal seamless thin-walled tube from the die assembly, such as Fig.10 As shown, the front and rear ends of the blank are trimmed so that the trimmed length of the blank is equal to the designed length of the finished pipe 100. After trimming, it is cleaned and tested for leakage. If no leakage occurs, it is determined to be a qualified product, completing the production of the precious metal seamless thin-walled tube, and obtaining a precious metal seamless thin-walled tube with uniform wall thickness.
[0062] Example
[0063] Taking the production of precious metal seamless thin-walled tubes with an inner diameter of 150 mm, a wall thickness of 1.2 mm, and a length of 400 mm as an example, the finished tubes are made according to the following steps:
[0064] S1. Weigh 20kg of precious metal raw materials and melt them into ingots, and sample and analyze the ingots; wipe the surface of the ingots that meet the analysis requirements with alcohol and put them into an annealing furnace, and anneal them at an annealing temperature of 1350℃ for 45min; take out the ingots after annealing, place them on a 2-ton forging hammer and forge six sides respectively. If there is no cracking during the forging process, place the forged ingot on an alumina pad with a thickness of 30mm and a length and width of 40mm to cool to room temperature, and wipe the forging residual foreign matter on the surface of the ingot with alcohol after cooling; use a milling machine to remove the six sides of the cleaned ingot, and the surface roughness reaches Ra1.6 after removing the surface layer with a thickness of 0.15mm. Finally, use a diamond file to remove the burrs on the edges and corners of the ingot, and recycle the precious metal scraps left after milling and filing.
[0065] S2. Roll the cleaned ingot in step S1. Before rolling, wipe the surface of the ingot with alcohol. The pressing amount during rolling is controlled at 0.5 mm each time. The rolling work is carried out on two sides. After rolling to a length of 540 mm on one side, the ingot is sent to an annealing furnace and annealed at an annealing temperature of 1400° C. for 30 minutes. After annealing, the rolling direction is changed and the rolling length of the other side is also 540 mm, until a plate with a thickness of 3.2 mm is obtained.
[0066] S3. After the rolling process is completed, the plate obtained after rolling is sent to an annealing furnace for annealing at an annealing temperature of 1400°C for 30 minutes; after annealing, the plate is taken out and air-cooled to room temperature; then the plate is leveled, and the flatness of the plate after leveling is 0.01mm; after the plate is leveled, the plate is cut into circular raw materials using laser cutting equipment, and the outer ring diameter of the circular raw material is 530mm, and the inner ring diameter is 100mm.
[0067] S4. Prepare a first mold with a diameter of 149.8 mm, a hardness of 64 HRC, a quenching depth of 2 mm, and a main body length of 500 mm, and process a threaded hole with a diameter of 25 mm and a depth of 40 mm in the center of the working surface of the first mold, and install a rotating shaft in the center of the non-working surface of the first mold; prepare a second mold with a diameter of 100 mm and a thickness of 10 mm, and install a stud in the center of the second mold; assemble the first mold and the second mold together so that the relative end faces of the first mold and the second mold fit together, and put the annular raw material on the second mold so that the annular raw material fits with the working surface of the first mold.
[0068] S5, connecting the rotating shaft of the first mold to the lathe by transmission, pressing the ejector pin of the lathe against the end surface of the second mold, performing multiple spinning processes on the annular raw material by the lathe, and performing annealing after each spinning process.
[0069] During the first spinning process, an ultrasonic measuring instrument is used to monitor the thickness of the ring-shaped raw material in real time during the spinning process. The overall thickness of the ring-shaped raw material is processed to 2.7 mm, and an angle of 140° is formed between the two sides of the ring-shaped raw material. The thickness of the ring-shaped raw material decreases from the center of the ring-shaped raw material to the edge of the ring-shaped raw material; then annealing is performed at an annealing temperature of 1350°C for 30 minutes and cooled to room temperature.
[0070] During the secondary spinning process, an ultrasonic measuring instrument is used to monitor the thickness of the ring-shaped raw material in real time during the spinning process. The overall thickness of the ring-shaped raw material is processed to 2.2 mm, and an angle of 80° is formed between the two sides of the ring-shaped raw material. The thickness of the ring-shaped raw material decreases from the center of the ring-shaped raw material to the edge of the ring-shaped raw material; then annealing is performed at an annealing temperature of 1400°C for 60 minutes and cooled to room temperature.
[0071] When the three spinning processes are performed, an ultrasonic measuring instrument is used to monitor the thickness of the ring-shaped raw material in real time during the spinning process. The overall thickness of the ring-shaped raw material is processed to 1.7 mm, and a 35° angle is formed between the two sides of the ring-shaped raw material. The thickness of the ring-shaped raw material decreases from the center of the ring-shaped raw material to the edge of the ring-shaped raw material; then annealing is performed at an annealing temperature of 1400°C for 90 minutes and cooled to room temperature.
[0072] After the above-mentioned repeated spinning and annealing treatments, the overall thickness of the ring-shaped raw material is thinned to 1.2±0.05mm, and the distance between the edge of the ring-shaped raw material and the end face of the first mold close to one end of the second mold reaches 35mm, thereby obtaining a blank of a precious metal seamless thin-walled tube.
[0073] S6. Remove the blank of the precious metal seamless thin-walled tube from the mold assembly, select an area with a thickness of 1.2 mm on the blank, trim off the head and tail of the blank with a reference length of 400 mm, clean the trimmed parts, and perform leakage detection after cleaning. If the detection is qualified, a finished product of a precious metal seamless thin-walled tube that meets the requirements can be obtained.
[0074] The wall thickness of the precious metal seamless thin-walled tube obtained in the above embodiment is ±0.05mm, the roundness is ±0.2mm, and the cylindricity is ±0.2mm. It has good strength and uniform tube wall thickness. It is not prone to cracking and corrosion even when used in a high-temperature working environment for a long time, and its service life is significantly improved.
Claims
1. A method for manufacturing a seamless thin-walled precious metal tube, characterized in that: Follow these steps in order: S1. Melt the precious metal raw materials into ingots, forge the ingots after annealing, and cool, clean, and deburr the ingots if there is no cracking during forging; S2, rolling and annealing the ingot obtained in S1 until a plate having a thickness greater than the wall thickness of the finished tube (100) by 2 to 3 mm is obtained; S3, annealing the plate obtained in S2 and then cooling it, leveling the plate, and then cutting it into a ring-shaped raw material (200), wherein the inner ring diameter of the ring-shaped raw material (200) is smaller than the inner diameter of the finished pipe (100), and the ring width of the ring-shaped raw material (200) is larger than the length of the finished pipe (100); S4. Prepare a mold assembly consisting of a first mold (300) and a second mold (400), wherein the first mold (300) is a cylinder having a diameter matching the inner diameter of the finished tube (100), the length of the first mold (300) is greater than the ring width of the annular raw material (200), a rotating shaft (310) is fixed to one end of the first mold (300), and the other end of the first mold (300) is detachably connected to the second mold (400), and the second mold (400) is a circular plate structure having a diameter equal to the inner ring diameter of the annular raw material (200) and smaller than the diameter of the first mold (300), connect the first mold (300) and the second mold (400), and sleeve the annular raw material (200) on the second mold (400), so that the first mold (300), the annular raw material (200) and the second mold (400) are coaxially assembled; S5, repeatedly performing spinning and annealing on the assembly structure obtained in S4, during the spinning process, the rotating shaft (310) of the first mold (300) is connected to the lathe by transmission, and the top pin of the lathe is pressed against the end face of the second mold (400), and the spinning process gradually reduces the thickness of the annular raw material (200) and the annular raw material (200) is gradually attached to the surface of the first mold (300), until the thickness difference between the thickness of the annular raw material (200) and the wall thickness of the finished tube (100) is ±0.05 mm, and the distance between the edge of the annular raw material (200) and the end face of the first mold (300) close to the second mold (400) reaches 25 to 35 mm, and the blank of the precious metal seamless thin-walled tube is formed; S6. The blank is removed from the mold assembly, and the front and rear ends of the blank are trimmed according to the length of the finished tube (100). After cleaning and passing the leakage test, the production of the precious metal seamless thin-walled tube is completed.
2. The method for manufacturing a seamless thin-walled precious metal tube according to claim 1, characterized in that: In the step S1, the weight of the precious metal raw material is 3 to 5 times the weight of the finished tube (100); after the precious metal raw material is smelted to obtain an ingot, a sample is taken to analyze the impurity elements and main component content, and if the requirements are met, the surface of the ingot is wiped with alcohol and then annealed.
3. The method for manufacturing a precious metal seamless thin-walled tube according to claim 1 or 2, characterized in that: In the step S1, the annealing time is 30 to 60 minutes, and the annealing temperature is 1350 to 1500° C. When forging the ingot, a 2 to 5 ton forging hammer is used to forge six sides, and if cracking occurs during forging, the ingot is re-purified and smelted; when cooling the ingot, the ingot is placed on a pad made of aluminum oxide or zirconium oxide and cooled to room temperature; when cleaning the ingot, the six sides of the ingot are first milled off on a milling machine, and the removal thickness is 0.1 to 0.15 mm, and the surface roughness of the ingot reaches Ra1.
6.
4. The method for manufacturing a seamless thin-walled precious metal tube according to claim 1, characterized in that: In step S2, the pressing amount each time when rolling the ingot is 0.5-1 mm, one side of the ingot is rolled first, and then the other side is rolled in the opposite direction after annealing, and the rolling lengths of the two sides are equal; the annealing time is 30-60 minutes, and the annealing temperature is 1350-1550°C.
5. The method for manufacturing a seamless thin-walled precious metal tube according to claim 1, characterized in that: In the step S3, the annealing time is 30 to 60 minutes, and the annealing temperature is 1350 to 1550° C.; after annealing, the plate is air-cooled to room temperature; after leveling, the flatness of the plate is within ±0.01 to 0.2 mm; the inner ring diameter of the cut circular ring-shaped raw material (200) is 50 to 70 mm smaller than the inner diameter of the finished pipe (100), and the outer ring diameter of the circular ring-shaped raw material (200) is 10 to 15 mm smaller than the length of the plate.
6. The method for manufacturing a seamless thin-walled precious metal tube according to claim 1, characterized in that: In the step S4, the hardness of the first mold (300) is 60-65 HRC, the quenching depth is 2-3 mm, the surface roughness Ra of the peripheral surface is less than 0.4, the length of the first mold (300) is greater than the length of the finished pipe (100) by 50-100 mm, the surface roughness Ra of the end surface of one end of the first mold (300) provided with the rotating shaft (310) is 0.8-1.6, and the surface roughness Ra of the end surface of the end of the first mold (300) not provided with the rotating shaft (310) is less than 0.4; the thickness of the second mold (400) is 10-20 mm; the first mold (300) and the second mold (400) are threadedly connected through a threaded hole and a stud, the threaded hole is provided on the first mold (300), and the stud is provided on the second mold (400); after the first mold (300) and the second mold (400) are connected, the opposite end surfaces of the two are completely fitted.
7. The method for manufacturing a seamless thin-walled precious metal tube according to claim 1, characterized in that: In the step S5, during the first spinning process, the thickness of the annular raw material (200) is processed to be 1.5 to 2.5 mm greater than the wall thickness of the finished tube (100), and the annular raw material (200) forms an angle of 140° to 150°; then, the raw material is annealed at an annealing temperature of 1350 to 1450° C. for 30 to 60 minutes, and cooled to room temperature.
8. The method for manufacturing a seamless thin-walled precious metal tube according to claim 7, characterized in that: In the step S5, during the secondary spinning process, the thickness of the annular raw material (200) is processed to be 1.0 to 1.5 mm greater than the wall thickness of the finished tube (100), and the annular raw material (200) forms an angle of 80° to 100°; then, annealing is performed at an annealing temperature of 1400 to 1500° C. for 60 to 90 minutes, and then cooled to room temperature.
9. The method for manufacturing a seamless thin-walled precious metal tube according to claim 8, characterized in that: In the step S6, the spinning process is performed three times until the thickness of the annular raw material (200) is greater than the wall thickness of the finished tube (100) by 0.5 to 1.0 mm, and the annular raw material (200) forms an angle of 35° to 50°; then, the annular raw material (200) is annealed at an annealing temperature of 1400 to 1500° C. for 60 to 90 minutes, and cooled to room temperature.
Citation Information
Cited By
Manufacturing method of tapered main rod for precious metal stirrer
CN120532892A