Kovar alloy and copper composite bar and hot extrusion processing technology thereof

Through the hot extrusion processing process, the problem of complex and high cost preparation process of Kovar alloy and Cu composite materials is solved, and the efficient preparation of Kovar-Cu composite rods with dense structure and high bonding strength is achieved, which avoids the defects of welded joints and meets the requirements of Meet the electrical and thermal conductivity requirements of electronic packaging materials.

CN118832276APending Publication Date: 2024-10-25JIANGSU UNIV OF SCI & TECH
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411104968.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

The preparation process of existing Kovar alloy and Cu composite materials is complex and costly, and the welded joints are prone to residual stress, which affects the mechanical properties.

Method used

Using hot extrusion processing technology, the copper rod is extruded into the Kovar alloy sleeve through a vacuum hot-pressing sintering furnace to form diffusion welding to avoid defects in the welding process. A bimetallic composite rod extrusion structure mold and strict Hot pressing processing parameters.

Benefits of technology

The preparation of Kovar-Cu composite rods with dense structure, high bonding strength and no weld defects simplifies the process, reduces costs, improves efficiency, and meets the electrical and thermal conductivity needs of electronic packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118832276A_ABST
    Figure CN118832276A_ABST
Patent Text Reader

Abstract

The invention provides a Kovar alloy and copper composite bar and a hot extrusion machining process thereof. The hot extrusion machining process comprises the following steps that S1, a to-be-machined workpiece is subjected to a pretreatment process; s2, a to-be-machined part is placed in the hot extrusion machining mold, and the to-be-machined part is assembled; s3, hot extrusion processing preparation is conducted, specifically, the mold assembled in the step S2 is placed in a vacuum hot pressing sintering furnace, and it is ensured that a hot pressing head is perpendicular to the to-be-processed workpiece for processing; s4, a vacuum hot-pressing sintering furnace is started, machining parameters are set, hot-pressing machining is conducted on the workpiece in the step S3, and under the action of a hot extrusion pressing head, a copper rod is extruded into the inner wall of the kovar alloy to form diffusion welding; and S5, after extrusion is finished, the vacuum hot pressing sintering furnace is closed, and the kovar alloy and copper composite bar is obtained. The process is simple, short in flow, high in efficiency and low in cost, and the welding seam defect of welding process production is avoided. The prepared Kovar alloy and copper composite bar is compact in structure, free of weld defects and good in mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional composite materials, and in particular relates to a kovar alloy and copper composite rod and a hot extrusion processing technology thereof. Background Art

[0002] With the rapid development of electronic devices and chip technology, the heat generated by electronic components is increasing, which puts higher requirements on the performance of electronic packaging materials. Since copper Cu has excellent thermal conductivity, Cu-based composite materials have become a research hotspot for high-performance electronic packaging materials; Kovar alloy (4J29) is called a "constant expansion alloy" and can maintain a low and stable thermal expansion coefficient below the Curie point. Therefore, the composite material containing Kovar alloy and Cu can not only solve the problem of poor thermal conductivity of Kovar alloy, but also maintain its low thermal expansion coefficient and good weldability, and is an ideal electronic packaging material.

[0003] At present, the preparation of Kovar alloy and Cu composite materials usually adopts welding method, but Kovar alloy and Cu are difficult to be welded by ordinary welding method due to the large difference in melting point. For example, vacuum brazing is very likely to produce large residual stress at the weld joint, thereby reducing the mechanical properties of the weld joint. Hot isostatic pressing diffusion welding method can effectively weld Cu and Kovar alloy, and there are no defects at the weld, but the process is complicated and the cost is high, and the airtightness and electrical properties after sealing are difficult to guarantee.

[0004] The above-mentioned technologies still lack effective solutions to the problems of complex process, long process and high cost in the preparation process of Kovar-Cu composite materials. Summary of the invention

[0005] In response to the above technical problems, the present invention provides a hot extrusion processing technology for Kovar alloy and copper composite rods. The hot extrusion processing method is adopted to prepare a composite rod with good bonding strength, high thermal conductivity and high electrical conductivity through heating and pressurizing processing. The composite rod has the advantages of simple process, short flow, high efficiency and low cost, and avoids the weld defects produced by welding process.

[0006] The present invention also provides a composite rod made of the kovar alloy and copper, which is prepared by the hot extrusion process, has a dense structure, a bonding strength of 26-57Mpa, no weld defects and maintains good mechanical properties.

[0007] The present invention achieves the above technical objectives through the following technical means.

[0008] A hot extrusion process for a kovar alloy and copper composite rod comprises the following steps:

[0009] Step S1: pre-treating the Kovar alloy sleeve and the copper rod to be processed;

[0010] Step S2: placing the workpiece pre-treated in step S1 in a hot extrusion processing die to assemble the workpiece;

[0011] Step S3: hot extrusion processing preparation, placing the hot extrusion processing mold of the workpiece to be processed assembled in step S2 in a vacuum hot pressing sintering furnace, ensuring that the hot extrusion head of the vacuum hot pressing sintering furnace is vertical to the workpiece to be processed;

[0012] Step S4: starting the vacuum hot pressing sintering furnace, setting processing parameters, and performing hot pressing processing on the workpiece to be processed in step S3. Under the action of the hot extrusion head of the vacuum hot pressing sintering furnace, the copper rod is pressed into the Kovar alloy cylinder to form diffusion welding;

[0013] Step S5: After the extrusion is completed, the vacuum hot pressing sintering furnace is closed, and the Kovar alloy and copper composite rod is taken out after the temperature drops to room temperature. The Kovar alloy and copper composite rod has the advantages of dense structure, no defects, and high bonding strength.

[0014] In the above scheme, in step S1, the pretreatment of the workpiece includes pickling and polishing the inner wall of the hollow part of the Kovar alloy sleeve with a hydrochloric acid solution with a mass percentage of 18-20%, and polishing the surface of the copper rod.

[0015] In the above scheme, the Kovar alloy sleeve has a straight cylindrical shape, and the internal hollow portion includes a connected cone front section and a straight cylindrical section.

[0016] Furthermore, the outer diameter of the Kovar alloy sleeve is 45-50 mm, the inner diameter of the front cone section is 19-20 mm, and the inner diameter of the straight section is 15-17 mm.

[0017] In the above solution, the copper rod has a diameter of 19-20 mm and a length of 45-50 mm.

[0018] In the above scheme, in the step S2, the hot extrusion processing die adopts a bimetallic composite rod extrusion structure die; the bimetallic composite rod extrusion structure die includes an upper pad, a pressure head, a guide plate, an inner support ring, an outer support ring and a lower pad; the inner support ring and the outer support ring are arranged on the lower pad, and the inner support ring is located in the outer support ring, and the inner support ring is provided with a first channel for placing a Kovar alloy sleeve; the guide plate is placed above the inner support ring and the outer support ring, and the guide plate is provided with a second channel for placing a copper rod, and the positions of the first channel and the second channel correspond vertically; the upper pad is located above the pressure head, and the pressure head cooperates with the second channel, and the pressure head is pushed along the second channel by the upper pad to extrude the copper rod into the inner hollow part of the Kovar alloy sleeve.

[0019] In the above scheme, in step S3, when assembling the processing mold, ensure that the pressing head is in close contact with the upper pad, and the hot extrusion pressing head of the vacuum hot pressing sintering furnace is vertical to the workpiece to be processed.

[0020] In the above scheme, in step S4, the hot pressing processing parameters are: heating temperature is 700-800°C, heating rate is 10°C / min, holding time is 0.5-1h, and hot pressing pressure is 30-40MPa.

[0021] A kovar alloy and copper composite rod is prepared according to the kovar alloy and copper composite rod hot extrusion processing technology.

[0022] In the above scheme, the kovar alloy and copper composite rod has a dense structure without defects and a bonding strength of 26-57 MPa.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention provides a kovar alloy and copper composite rod and a hot pressing processing technology thereof. According to the different characteristics of the kovar alloy and copper, a hot extrusion processing mold and process design are performed, and the heating temperature and the insulation time in the hot extrusion process are strictly controlled. The kovar alloy and copper having a large difference in melting point and a large difference in hot extrusion temperature are successfully prepared to obtain a kovar alloy-wrapped copper core composite rod. The preparation is simple, the process is short, and the efficiency is high. The composite rod prepared by the process method has the characteristics of high electrical conductivity and good thermal conductivity, and can meet the needs of the electronics, electrical, communications and other industries for such materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A schematic diagram of a die for a hot extrusion process of a Kovar alloy and copper composite rod according to an embodiment of the present invention.

[0026] Figure 2 for Figure 1 Top view after removing the upper pad, pressure head, guide plate and copper rod.

[0027] Figure 3 This is a diagram showing the bonding strength of a statistical composite rod according to an embodiment of the present invention.

[0028] In the figure, 1. upper pad; 2. pressure head; 3. guide plate; 4. copper rod; 5. inner support ring; 6. Kovar alloy sleeve; 7. outer support ring; 8. lower pad. DETAILED DESCRIPTION

[0029] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0030] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "front", "back", "left", "right", "up", "down", "axial", "radial", "vertical", "horizontal", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0031] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0032] Example 1

[0033] A hot extrusion process for a kovar alloy and copper composite rod comprises the following steps:

[0034] Step S1: pre-treating the Kovar alloy sleeve 6 and the copper rod 4 to be processed;

[0035] Step S2: placing the workpiece pre-treated in step S1 in a hot extrusion processing die to assemble the workpiece;

[0036] Step S3: hot extrusion processing preparation, placing the hot extrusion processing mold of the workpiece to be processed assembled in step S2 in a vacuum hot pressing sintering furnace, ensuring that the hot extrusion head of the vacuum hot pressing sintering furnace is vertical to the workpiece to be processed;

[0037] Step S4: start the vacuum hot pressing sintering furnace, set the processing parameters, perform hot pressing processing on the workpiece to be processed in step S3, and under the action of the hot extrusion head of the vacuum hot pressing sintering furnace, extrude the copper rod into the Kovar alloy cylinder 6 to form diffusion welding;

[0038] Step S5: After the extrusion is completed, the vacuum hot pressing sintering furnace is closed, and the mold is removed after the temperature drops to room temperature to obtain the Kovar alloy and copper composite rod. The Kovar alloy and copper composite rod has the advantages of dense structure, no defects, and high bonding strength.

[0039] In this embodiment, in step S1, the pretreatment of the workpiece includes pickling and polishing the inner wall of the hollow part of the Kovar alloy sleeve 6 with a hydrochloric acid solution with a mass percentage of 18-20%, and polishing the surface of the copper rod 4.

[0040] In this embodiment, the Kovar alloy sleeve 6 has a straight cylindrical shape, and the inner hollow portion includes a connected cone front section and a straight cylindrical section.

[0041] like Figure 1 and 2 As shown, in this embodiment, the hot extrusion processing die adopts a bimetallic composite rod extrusion structure die; the bimetallic composite rod extrusion structure die includes an upper pad 1, a ram 2, a guide plate 3, an inner support ring 5, an outer support ring 7 and a lower pad 8; the inner support ring 5 and the outer support ring 7 are arranged on the lower pad 8, and the inner support ring 5 is located in the outer support ring 7, and the inner support ring 5 is provided with a first channel for placing the Kovar alloy sleeve 6; the guide plate 3 is placed above the inner support ring 5 and the outer support ring 7, and the guide plate 3 is provided with a second channel for placing the copper rod 4, and the positions of the first channel and the second channel correspond vertically; the upper pad 1 is located above the ram 2, and the ram 2 cooperates with the second channel, and the ram 2 is pushed by the upper pad 1 along the second channel to extrude the copper rod 4 into the inner hollow part of the Kovar alloy sleeve 6.

[0042] In step S3, when assembling the processing mold, ensure that the pressing head 2 is in close contact with the upper pad 1, and the hot extrusion pressing head of the vacuum hot pressing sintering furnace is perpendicular to the workpiece to be processed.

[0043] In step S4, the hot pressing processing parameters are: heating temperature is 800° C., heating rate is 10° C. / min, holding time is 0.5 h, and hot pressing pressure is 35 MPa.

[0044] In this embodiment, the prepared Kovar alloy and copper composite rod has a dense structure without defects and a bonding strength of 57Mpa. Figure 2 shown.

[0045] Example 2

[0046] The specific preparation steps are the same as those in Example 1. The difference between this example and Example 1 is that:

[0047] The hot extrusion parameters in step S4 are: the heating temperature is set to 700° C., the holding time is 0.5 h, and the other parameters are the same as those in Example 1.

[0048] The bonding strength of the composite rod prepared using the parameters of this embodiment is 26MPa. Figure 1 , 2 shown.

[0049] Example 3

[0050] The specific preparation steps are the same as those in Example 1. The difference between this example and Example 1 is that:

[0051] The hot extrusion parameters in step S4 are: heating temperature is 800° C., holding time is 1 h, and other parameters are the same as those in Example 1.

[0052] The bonding strength of the composite rod prepared using the parameters of this embodiment is 45MPa. Figure 2 shown.

[0053] The present invention prepares the composite rod of Kovar alloy and copper by hot extrusion processing, heats to the bonding temperature by using a vacuum hot pressing sintering furnace, and produces hot pressing effect by vertical downward pressure of a pressure head to achieve metallurgical bonding. The present invention gives full play to the advantages of hot pressing diffusion welding technology, processes the composite rod of Kovar alloy and copper, and successfully prepares the composite rod of Kovar alloy wrapped with copper core from two materials of Kovar alloy and copper with large difference in melting point and hot extrusion temperature, which is simple to prepare, short in process and high in efficiency. The composite rod prepared by the process method has dense structure, bonding strength of 26-57MPa, no weld defects and maintains good mechanical properties.

[0054] It should be understood that although this specification is described according to various embodiments, not every embodiment contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.

[0055] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A hot extrusion process for a kovar alloy and copper composite rod, characterized in that: The following steps are involved: Step S1: pre-treating the Kovar alloy sleeve (6) and the copper rod (4) to be processed; Step S2: placing the workpiece pre-treated in step S1 in a hot extrusion processing die to assemble the workpiece; Step S3: placing the hot extrusion processing die of the workpiece to be processed assembled in step S2 in a vacuum hot pressing sintering furnace; Step S4: starting the vacuum hot pressing sintering furnace, setting processing parameters, and performing hot pressing processing on the workpiece to be processed in step S3. Under the action of the hot extrusion head of the vacuum hot pressing sintering furnace, the copper rod (4) is pressed into the Kovar alloy cylinder (6) to form diffusion welding; Step S5: After the extrusion is completed, the vacuum hot pressing sintering furnace is closed, and the Kovar alloy and copper composite rods are taken out after the temperature drops to room temperature.

2. The hot extrusion process of Kovar alloy and copper composite rod according to claim 1, characterized in that: In the step S1, the pretreatment of the workpiece includes pickling and polishing the inner wall of the hollow part of the Kovar alloy sleeve (6) with a hydrochloric acid solution having a mass percentage of 18-20%, and polishing the surface of the copper rod (4).

3. The hot extrusion process of Kovar alloy and copper composite rod according to claim 1, characterized in that: The Kovar alloy sleeve (6) has a straight cylindrical shape, and its internal hollow portion comprises a connected cone front section and a straight cylindrical section.

4. The hot extrusion process of Kovar alloy and copper composite rod according to claim 3, characterized in that: The outer diameter of the Kovar alloy sleeve (6) is 45-50 mm, the inner diameter of the cone front section is 19-20 mm, and the inner diameter of the straight section is 15-17 mm.

5. The hot extrusion process of Kovar alloy and copper composite rod according to claim 1, characterized in that: The copper rod (4) has a diameter of 19-20 mm and a length of 45-50 mm.

6. The hot extrusion process of Kovar alloy and copper composite rod according to claim 1, characterized in that: In the step S2, the hot extrusion processing die adopts a bimetallic composite rod extrusion structure die; the bimetallic composite rod extrusion structure die comprises an upper pad (1), a pressure head (2), a guide plate (3), an inner support ring (5), an outer support ring (7) and a lower pad (8); the inner support ring (5) and the outer support ring (7) are arranged on the lower pad (8), and the inner support ring (5) is located in the outer support ring (7), and the inner support ring (5) is provided with a first channel for placing a Kovar alloy sleeve (6); the guide plate (3) is placed above the inner support ring (5) and the outer support ring (7), and the guide plate (3) is provided with a second channel for placing a copper rod (4), and the positions of the first channel and the second channel correspond vertically; the upper pad (1) is located above the pressure head (2), and the pressure head (2) cooperates with the second channel, and the pressure head (2) is pushed along the second channel by the upper pad (1) to extrude the copper rod (4) into the inner hollow part of the Kovar alloy sleeve (6).

7. The hot extrusion process of Kovar alloy and copper composite rod according to claim 6, characterized in that: In the step S3, when assembling the processing mold, ensure that the pressing head (2) and the upper pad (1) maintain close contact, and the hot extrusion pressing head of the vacuum hot pressing sintering furnace is vertical to the workpiece to be processed.

8. The hot extrusion process of Kovar alloy and copper composite rod according to claim 1, characterized in that: In step S4, the hot pressing processing parameters are: heating temperature is 700-800°C, heating rate is 10°C / min, holding time is 0.5-1h, and hot pressing pressure is 30-40MPa.

9. A composite rod of Kovar alloy and copper, characterized in that: The kovar alloy and copper composite rod is prepared by the hot extrusion processing process according to any one of claims 1 to 8.

10. The Kovar alloy and copper composite rod according to claim 9, characterized in that: The bonding strength of the Kovar alloy and the copper composite rod is 26-57 MPa.

Citation Information

Cited By

  • Diffusion welding method based on interface normal solid pressurization

    CN119501262A

  • Composite bar and welding method

    CN119910293A

  • Method for preparing copper-steel composite rod at low cost through vacuum hot pressing furnace

    CN120791109A

  • A method for low cost production of copper-steel composite rods by vacuum hot pressing furnace