Preparation method of long-chain branched polypropylene with high melt strength

By adding specific components and grafting reactions during the reactive extrusion process of polypropylene, a long branched chain structure is formed, which solves the problems of polypropylene degradation and side reactions, improves its melt strength, and meets the requirements for high melt strength. need.

CN118834331APending Publication Date: 2024-10-25SINOCHEM PETROCHEMICAL RESEARCH INSTITUTE (QUANZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411133591.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-10-25

Smart Images

  • Figure CN118834331A_ABST
    Figure CN118834331A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of long-chain branched polypropylene with high melt strength. The preparation method comprises the following steps: directly adding raw materials such as isotactic polypropylene, a grafting monomer, an auxiliary grafting monomer, a free radical initiator and the like into an extruder, and extruding to obtain the polypropylene resin with the thermally reversible branched structure. In the preparation process of the polypropylene resin, polypropylene degradation can be effectively avoided, the branching reaction of polypropylene is enhanced, and a polypropylene material with high melt strength is obtained, so that the polypropylene resin has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polypropylene materials, and in particular relates to a method for preparing long-chain branched polypropylene with high melt strength. Background Art

[0002] Polypropylene (PP) has a series of advantages such as excellent comprehensive performance, light weight and low price. It is a thermoplastic polymer widely used in daily life. However, ordinary polypropylene has short branches and narrow molecular weight distribution. Its softening point is very close to the melting point. During the processing, the melt strength and melt viscosity will drop sharply. There is no strain hardening effect, which makes it difficult to meet the application requirements of extrusion, casting, blow molding, biaxial stretching and foaming. Studies have shown that the introduction of branched structures in polypropylene can increase the entanglement points between macromolecular chains, increase the friction resistance between molecular chains, and improve the melt strength. The preparation methods of long-chain branched polypropylene (LCB-PP) mainly include irradiation, catalytic polymerization and reactive extrusion. Among them, the reactive extrusion method is simple to operate, has low equipment requirements, and has a variety of implementation paths. It is suitable for industrial production, so it is the most widely used method, but it is often easy to degrade PP and side reactions occur during the preparation process, resulting in a decrease in PP performance. Therefore, how to reduce β fracture in the reactive extrusion process of high melt strength polypropylene has become an urgent problem to be solved. Summary of the invention

[0003] The object of the present invention is to provide a method for preparing long-chain branched polypropylene with high melt strength, so as to solve the problem that polypropylene resin in the prior art is prone to degradation during the reaction extrusion process.

[0004] To achieve the above object, the present invention adopts the following technical solution: A long-chain branched polypropylene with high melt strength, the preparation method of which is to mix isotactic polypropylene A, grafting monomer component B having a structure of formula (I), component C having a structure of formula (II), auxiliary grafting monomer component D, free radical initiator E, and free radical stabilizer F, and extrude through an extruder, collect, and cool to obtain the obtained product; , , In formula (I), R 1 for or , R 2 is O or S; in formula (II), R 3 It is a C1~C6 straight chain alkane or C6~C 14 The aromatic group is preferably p-phenyl, p-diphenylmethane, n-butyl or n-hexyl.

[0005] Furthermore, the auxiliary grafting monomer component D is one or more of styrene, divinylbenzene, and p-(3-butenyl)styrene.

[0006] Furthermore, the free radical initiator E is a thermal decomposition free radical initiator, an organic peroxide or an azo initiator, preferably an alkyl peroxide, a hydrogenated peroxide, an acyl peroxide or a peroxycarbonate.

[0007] Furthermore, the free radical stabilizer F is selected from at least one of hindered phenol antioxidants, phosphite antioxidants, and alkyl ester antioxidants.

[0008] Furthermore, the addition amount of the graft monomer component B is 0.01%-5% of the mass of the isotactic polypropylene A, preferably 0.1%-2%.

[0009] Furthermore, the addition amount of component C is 0.01%-5% of the mass of the isotactic polypropylene A, preferably 0.05%-2%.

[0010] Furthermore, the mass ratio of the auxiliary grafting monomer component D to the grafting monomer component B is (1-5):1, preferably 1:1.

[0011] Furthermore, the amount of the free radical initiator E added is 0.01%-1% of the mass of the isotactic polypropylene A, preferably 0.05-0.5%.

[0012] Furthermore, the addition amount of the free radical stabilizer F is 0.05%-1% of the mass of the isotactic polypropylene A, preferably 0.1-0.5%.

[0013] Furthermore, the extruder is a twin-screw extruder having at least six zones, wherein the temperature of the first zone is 90°C~230°C, the temperature of the second zone is 150°C~230°C, the temperature of the third zone is 180°C~230°C, and the temperature of the subsequent zones is 190°C~230°C.

[0014] Further, the total residence time of the mixed components in the extruder is 30 seconds to 300 seconds.

[0015] The present invention adopts dual monomer components and bismaleimide compounds to co-graft polypropylene. Figure 1 During the reaction extrusion process, the grafting monomer containing styrene groups will preferentially react with the free radicals of PP rupture to form stable styrene alkyl groups. Then the grafting monomer containing furan groups will further react with the formed styrene alkyl groups and be grafted into polypropylene, thereby inhibiting the occurrence of β-fracture and other side reactions of polypropylene. The product is finally connected to the maleimide compound through a thermally reversible dynamic covalent bond to achieve the formation of a long-chain branched structure of polypropylene.

[0016] Compared with the prior art, the present invention has the following beneficial effects: The invention prepares long-chain branched polypropylene with high melt strength through a simple extrusion reaction. In the preparation process, a high-activity auxiliary grafting monomer is added to react quickly with free radicals generated by PP fracture, thereby reducing the degradation of PP; then a low-activity grafting monomer is used to react with new free radicals to promote the generation of branches, thereby improving the melt strength of polypropylene. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a reaction principle diagram for preparing long-chain branched polypropylene with high melt strength according to the present invention.

[0018] Figure 2 The infrared spectra of the polypropylene resins prepared in Example 2 and Comparative Examples 1 and 3 are shown.

[0019] Figure 3 The rheological curves (190°C) showing the storage modulus of the polypropylene resins prepared in Examples 2 and 3 and Comparative Examples 1 and 3 as a function of shear rate.

[0020] Figure 4 The rheological curves (190°C) showing the change of loss tangent with shear rate of the polypropylene resins prepared in Examples 2 and 3 and Comparative Examples 1 and 3.

[0021] Figure 5 The Cole-Cole rheological curves (190°C) of the polypropylene resins prepared in Examples 2 and 3 and Comparative Examples 1 and 3. DETAILED DESCRIPTION

[0022] A preparation method for long-chain branched polypropylene with high melt strength comprises the steps of continuously feeding isotactic polypropylene A, grafting monomer component B having a structure of formula (I), component C having a structure of formula (II), auxiliary grafting monomer component D, free radical initiator E, and free radical stabilizer F into a twin-screw extruder having at least six zones, and extruding, collecting, and cooling the extruder to obtain the obtained product; , , In formula (I), R 1 for or , R 2 is O or S; in formula (II), R 3 It is a C1~C6 straight chain alkane or C6~C 14 Aromatic base.

[0023] The addition amount of grafting monomer component B is 0.01%-5% of the mass of isotactic polypropylene A. The addition amount of component C is 0.01%-5% of the mass of isotactic polypropylene A. The mass ratio of grafting monomer component D to grafting monomer component B is (1-5):1. The addition amount of free radical initiator E is 0.01%-1% of the mass of isotactic polypropylene A. The addition amount of free radical stabilizer F is 0.05%-1% of the mass of isotactic polypropylene A.

[0024] The grafting aid monomer component D is one or more of styrene, divinylbenzene, and p-(3-butylene)styrene. The free radical initiator E is a thermal decomposition free radical initiator, an organic peroxide or an azo initiator, preferably an alkyl peroxide, a hydrogenated peroxide, an acyl peroxide, or a peroxycarbonate. The free radical stabilizer F is selected from at least one of a hindered phenol antioxidant, a phosphite antioxidant, and an alkyl ester antioxidant.

[0025] The temperature of the first zone of the extruder is 90°C to 230°C, the temperature of the second zone is 150°C to 230°C, the temperature of the third zone is 180°C to 230°C, and the temperature of the subsequent zones is 190°C to 230°C.

[0026] The total residence time of the mixed components in the extruder is from 30 seconds to 300 seconds.

[0027] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0028] Example 1 In parts by mass, 100 parts of isotactic polypropylene (A), 0.5 parts of 2-vinylfuran (B1), 0.25 parts of bismaleimide (C), 0.5 parts of styrene (D1), 0.2 parts of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (DHBP, E), 0.1 parts of antioxidant 1010 (F1), and 0.2 parts of antioxidant 168 (F2) are continuously fed into a twin-screw extruder, and the temperature of the first zone of the extruder is set to 100° C., the temperature of the second zone is set to 160° C., the temperature of the third zone is set to 190° C., the temperature of the fourth zone is set to 200° C., the temperature of the fifth zone is set to 200° C., and the temperature of the sixth zone is set to 190° C. The total residence time of the mixed components in the extruder is controlled to be 180 seconds. The extruded product is cooled and pelletized to obtain long-chain branched polypropylene.

[0029] Example 2 In parts by mass, 100 parts of isotactic polypropylene (A), 0.5 parts of furfuryl methacrylate (B2), 0.25 parts of bismaleimide (C), 0.5 parts of styrene (D1), 0.2 parts of DHBP (E), 0.1 parts of antioxidant 1010 (F1), and 0.2 parts of antioxidant 168 (F2) are continuously fed into a twin-screw extruder, and the temperature of the first zone of the extruder is set to 100°C, the temperature of the second zone is set to 160°C, the temperature of the third zone is set to 190°C, the temperature of the fourth zone is set to 200°C, the temperature of the fifth zone is set to 200°C, and the temperature of the sixth zone is set to 190°C. The total time that the mixed components stay in the extruder is controlled to be 180 seconds. The extruded product is cooled and pelletized to obtain long-chain branched polypropylene.

[0030] Example 3 In parts by mass, 100 parts of isotactic polypropylene (A), 1 part of furfuryl methacrylate (B2), 0.5 parts of bismaleimide (C), 1 part of styrene (D1), 0.4 parts of DHBP (E), 0.1 parts of antioxidant 1010 (F1) and 0.2 parts of antioxidant 168 (F2) are continuously fed into a twin-screw extruder, and the temperature of the first zone of the extruder is set to 100°C, the temperature of the second zone is set to 160°C, the temperature of the third zone is set to 190°C, the temperature of the fourth zone is set to 200°C, the temperature of the fifth zone is set to 200°C, and the temperature of the sixth zone is set to 190°C. The total residence time of the mixed components in the extruder is controlled to be 180 seconds. The extruded product is cooled and pelletized to obtain long-chain branched polypropylene.

[0031] Example 4 In parts by mass, 100 parts of isotactic polypropylene (A), 0.5 parts of furfuryl methacrylate (B2), 0.25 parts of bismaleimide (C), 0.5 parts of divinylbenzene (D2), 0.2 parts of DHBP (E), 0.1 parts of antioxidant 1010 (F1), and 0.2 parts of antioxidant 168 (F2) are continuously fed into a twin-screw extruder, and the temperature of the first zone of the extruder is set to 100°C, the temperature of the second zone is set to 160°C, the temperature of the third zone is set to 190°C, the temperature of the fourth zone is set to 200°C, the temperature of the fifth zone is set to 200°C, and the temperature of the sixth zone is set to 190°C. The total residence time of the mixed components in the extruder is controlled to be 180 seconds. The extruded product is cooled and pelletized to obtain long-chain branched polypropylene.

[0032] Example 5 100 parts of isotactic polypropylene (A), 0.5 parts of furfuryl methacrylate (B2), 0.25 parts of bismaleimide (C), 0.5 parts of p-(3-butylene) styrene (D3), 0.2 parts of DHBP (E), 0.1 parts of antioxidant 1010 (F1) and 0.2 parts of antioxidant 168 (F2) were continuously fed into a twin-screw extruder, and the temperature of the first zone of the extruder was set to 100°C, the temperature of the second zone was set to 160°C, the temperature of the third zone was set to 190°C, the temperature of the fourth zone was set to 200°C, the temperature of the fifth zone was set to 200°C, and the temperature of the sixth zone was set to 190°C. The total residence time of the mixed components in the extruder was controlled to be 180 seconds. The extruded product was cooled and pelletized to obtain long-chain branched polypropylene.

[0033] Comparative Example 1 100 parts of isotactic polypropylene (A), 0.2 parts of DHBP (E), 0.1 parts of antioxidant 1010 (F1) and 0.2 parts of antioxidant 168 (F2) were continuously fed into a twin-screw extruder, and the temperature of the first zone of the extruder was set to 100°C, the temperature of the second zone was set to 160°C, the temperature of the third zone was set to 190°C, the temperature of the fourth zone was set to 200°C, the temperature of the fifth zone was set to 200°C, and the temperature of the sixth zone was set to 190°C. The total residence time of the mixed components in the extruder was controlled to be 180 seconds. The extruded product was cooled and pelletized to obtain polypropylene.

[0034] Comparative Example 2 100 parts of isotactic polypropylene (A), 1 part of styrene (D1), 0.2 parts of DHBP (E), 0.1 parts of antioxidant 1010 (F1) and 0.2 parts of antioxidant 168 (F2) were continuously fed into a twin-screw extruder, and the temperature of the first zone of the extruder was set to 100°C, the temperature of the second zone was set to 160°C, the temperature of the third zone was set to 190°C, the temperature of the fourth zone was set to 200°C, the temperature of the fifth zone was set to 200°C, and the temperature of the sixth zone was set to 190°C. The total time the mixed components stayed in the extruder was controlled to be 180 seconds. The extruded product was cooled and pelletized to obtain polypropylene.

[0035] Comparative Example 3 100 parts of isotactic polypropylene (A), 0.5 parts of furfuryl methacrylate (B2), 0.25 parts of bismaleimide (C), 0.2 parts of DHBP (E), 0.1 parts of antioxidant 1010 (F1) and 0.2 parts of antioxidant 168 (F2) were continuously fed into a twin-screw extruder, and the temperature of the first zone of the extruder was set to 100°C, the temperature of the second zone was set to 160°C, the temperature of the third zone was set to 190°C, the temperature of the fourth zone was set to 200°C, the temperature of the fifth zone was set to 200°C, and the temperature of the sixth zone was set to 190°C. The total residence time of the mixed components in the extruder was controlled to be 180 seconds. The extruded product was cooled and pelletized to obtain polypropylene.

[0036] The performance tests of the polypropylene resins prepared in the examples and comparative examples are shown in Table 1 and Figures 2~5 .

[0037] Table 1 Performance test results of polypropylene resin

[0038] It can be seen from the results that compared with the pure polypropylene prepared in Comparative Example 1, the MFR of the long-chain branched polypropylene prepared in the examples has decreased, which indicates that the addition of the grafting monomer can increase the long-chain branching effect of polypropylene, effectively avoid the degradation of polypropylene and the generation of side reactions, and improve the melt strength of polypropylene, so that its melt strength reaches more than 35cN. In contrast, the MFR of the polypropylene prepared by Comparative Example 2 containing only component D (styrene) is significantly reduced, which indicates that the grafting of component D (styrene) can avoid the degradation of polypropylene, but its gel content increases. In Comparative Example 3, when using components B (furfuryl methacrylate) and C (bismaleimide), although the melt strength is improved, the MFR has increased significantly, which indicates that the Diels-Alder reaction between components B and C is the key to generating a long-chain branched structure and thus improving the melt strength of polypropylene, but due to the lack of component D (styrene), the polypropylene is severely degraded during the extrusion process, which further proves that the grafting of component D (styrene) can effectively avoid the degradation of polypropylene.

[0039] At the same time, from Figure 3 , 4 It can be seen that Examples 2 and 3 and Comparative Example 3 all exhibit typical long-chain branching rheological laws. The Cole-Cole curve of linear polypropylene is a semicircular structure, and the larger the molecular weight of the polymer, the larger the semicircular radius; when the long-chain branching structure exists, the Cole-Cole curve will deviate from the semicircular shape in the high viscosity region, and the higher the content of the long-chain branching structure, the more obvious the deviation phenomenon. Figure 5Comparative Example 3 and Examples 2 and 3 show a significant deviation from the semicircular structure. This indicates that compared with Comparative Example 1, the other three examples all have long chain structures, and the content of long chain branched structures in Examples 2 and 3 is much greater than that in Comparative Example 3.

[0040] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A method for preparing long-chain branched polypropylene with high melt strength, characterized in that: The isotactic polypropylene A, the grafting monomer component B having the structure of formula (I), the component C having the structure of formula (II), the auxiliary grafting monomer component D, the free radical initiator E, and the free radical stabilizer F are mixed, extruded through an extruder, collected, and cooled to obtain the long-chain branched polypropylene with high melt strength; 、 , In formula (I), R 1 for or , R 2 is O or S; in formula (II), R 3 It is a C1~C6 straight chain alkane or C6~C 14 Aromatic base.

2. The preparation method according to claim 1, characterized in that: The addition amount of the grafting monomer component B is 0.01%-5% of the mass of the isotactic polypropylene A.

3. The preparation method according to claim 1, characterized in that: The addition amount of component C is 0.01%-5% of the mass of isotactic polypropylene A.

4. The preparation method according to claim 1, characterized in that: The mass ratio of the grafting monomer component D to the grafting monomer component B is (1-5):1; The auxiliary grafting monomer component D is one or more of styrene, divinylbenzene, and p-(3-butenyl)styrene.

5. The preparation method according to claim 1, characterized in that: The addition amount of the free radical initiator E is 0.01%-1% of the mass of the isotactic polypropylene A; the free radical initiator E is a thermal decomposition free radical initiator, an organic peroxide or an azo initiator.

6. The preparation method according to claim 1, characterized in that: The addition amount of the free radical stabilizer F is 0.05%-1% of the mass of the isotactic polypropylene A; the free radical stabilizer F is selected from at least one of hindered phenol antioxidants, phosphite antioxidants, and alkyl ester antioxidants.

7. The preparation method according to claim 1, characterized in that: The extruder is a twin-screw extruder with at least six zones, wherein the temperature of the first zone is 90°C to 230°C, the temperature of the second zone is 150°C to 230°C, the temperature of the third zone is 180°C to 230°C, and the temperature of the subsequent zones is 190°C to 230°C.

8. The preparation method according to claim 1, characterized in that: The total residence time of the mixed components in the extruder is from 30 seconds to 300 seconds.

9. A long-chain branched polypropylene with high melt strength prepared by the method of claim 1.