Conductive gel powder as well as preparation method and application thereof
By first preparing graphene hydrogel and adding polyamic acid salt and conductive polymer PEDOT:PSS, the problem of poor compatibility between graphene aerogel and polyurethane is solved, and the conductive and mechanical properties of the composite material are improved. Suitable for 3D printing polyurethane materials.
Patent Information
- Application Number
- CN202411327864.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-09-24
AI Technical Summary
In the existing technology, graphene aerogel has poor compatibility with thermoplastic resins such as polyurethane, resulting in insufficient electrical conductivity and mechanical properties of the composite material, and is prone to structural damage especially during the 3D printing process.
Graphene oxide and polyethylene glycol are used as raw materials to prepare graphene hydrogel first, add polyamic acid salt solution and drop it into the graphene hydrogel to build the internal network of the gel, and at the same time, in the polyamic acid salt solution Adding conductive polymer PEDOT:PSS enhances the dispersion and stability of graphene through electrostatic interactions and hydrogen bonds, and improves conductive properties.
It significantly improves the stability of graphene hydrogel and the electrical conductivity and mechanical properties of composite materials. It is suitable for 3D printing polyurethane materials and enhances its electrical conductivity and adjustable mechanical properties.
Smart Images

Figure CN118834412A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of gel material preparation, and particularly relates to a conductive gel powder and a preparation method and application thereof. Background Art
[0002] In modern times, polymer materials have developed rapidly, and fibers, plastics, rubbers and various forms of polymer composites have appeared in every corner of human life. However, the types and quantities of functional polymer materials are far from enough. The main reason is that the functionalization degree of polymer materials is not high, and the mechanical strength of a few functional polymer composites is poor, which greatly limits its scope of use. How to broaden the application field of polymer materials and develop functional polymer composites with strong environmental adaptability is the key to solving the problem.
[0003] Functionalized polymers are one of the effective ways to expand the application range of polymers. They are widely used as structural workpieces, outer packaging, functional devices, etc. Common treatment methods include functionalization of polymer molecular structure, functionalization of polymer surface, and adding functional fillers to polymer matrix. Among them, adding functional fillers to polymer matrix is widely used in the functionalization treatment of polymers because of its advantages of simple process and outstanding effect.
[0004] With the development of graphene science, graphene aerogel came into being. Graphene aerogel is a graphene foam with a continuous structure formed by connecting graphene nanosheets through intermolecular forces such as π-π interactions and van der Waals forces. Because of its structural continuity, it can greatly improve the contact density between graphene nanosheets, and has the advantages of being porous and lightweight, making it more suitable as a functional filler to prepare functional composite materials. It is a material with potential development prospects. Although graphene aerogel and polymer can form functional composite materials with excellent performance after being compounded, how to improve the compatibility of graphene aerogel with polymers when used as fillers is still a major problem. There are many preparation technologies for polyimide / graphene gel materials in the prior art. However, it generally adopts the in-situ gel formation method (CN106750290A, CN110357067A, etc.), the graphene aerogel impregnation method (CN112094426A), and the polyacrylic acid hydrogel loaded graphene method (CN116218018A). The above process either prepares polyamic acid gel or graphene aerogel first, or prepares aerogel after blending polyamic acid and graphene. The matrix structure is a polymer, which is unstable and has poor mechanical properties. When used for 3D printing melt reprocessing, structural damage will occur. In addition, the introduction of polyimide will reduce the conductive properties of the aerogel to a certain extent, affecting the improvement of the conductive properties of the composite material. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a conductive gel powder and a preparation method and application thereof, which overcomes the defect that the gel powder prepared in the prior art has poor compatibility with thermoplastic resins such as polyurethane, while improving the conductive performance of the composite material.
[0006] The specific technical solutions adopted are as follows: A method for preparing a conductive gel powder comprises the following steps: (1) dispersing graphene oxide, a reducing agent and polyethylene glycol in deionized water to obtain a graphene oxide mixed solution, sealing the solution and heating the solution to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol is 1:(0-0.1); wherein the mass of polyethylene glycol is not 0; (2) pouring the polyamic acid solution into deionized water for precipitation, dispersing a certain amount of the precipitated polyamic acid powder in deionized water, adding tertiary amine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1: (0.1-0.6); (3) adding the PEDOT:PSS aqueous solution to the polyamic acid salt solution and stirring to obtain a mixed polyamic acid salt solution; the mass ratio of PEDOT:PSS in the polyamic acid powder and the PEDOT:PSS aqueous solution is 1:(0.01-0.2); (4) adding the mixed polyamic acid salt solution dropwise to the graphene hydrogel solution while stirring, and allowing the solution to stand after the addition is complete to obtain a polyamic acid / PEDOT:PSS / graphene mixed hydrogel; (5) The polyamic acid / PEDOT:PSS / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain a conductive gel powder.
[0007] In order to solve the technical problem of reducing the mechanical properties caused by first preparing polyamic acid gel, graphene aerogel, or directly blending polyamic acid and graphene to prepare aerogel, the inventor used polyethylene glycol and graphene oxide as raw materials to first prepare graphene hydrogel in previous work to construct a graphene-based gel material. The graphene surface active groups prepared by the redox method are relatively large. Polyethylene glycol, as a good modifier, is not only conducive to the dispersion of graphene, but also can form hydrogen bonds with oxygen-containing functional groups such as carboxyl or hydroxyl groups on the surface of graphene, enhance the interaction force between graphene sheets, and improve the stability of the graphene hydrogel structure. The polyamic acid salt aqueous solution is added dropwise to the graphene hydrogel solution so that the polyamic acid salt fully infiltrates the inside of the graphene hydrogel to construct the internal network of the gel. Compared with the process of adding graphene to polyamic acid hydrogel, impregnating graphene aerogel with polyamic acid, and preparing hydrogel in situ, the process of impregnating graphene hydrogel with polyamic acid salt not only further improves the mechanical properties of the gel material, but also improves the compatibility of graphene with thermoplastic materials such as polyurethane, which is conducive to meeting the process of secondary processing of 3D printing. In addition, post-impregnation of graphene hydrogel can further reduce the pore size and increase the number of pore walls. The use of tertiary amines to react with polyamic acid to prepare polyamic acid salt is conducive to improving the solubility of polyamic acid substances, reducing the viscosity of the solution, and improving the wettability of polyamic acid and graphene hydrogel.
[0008] Although the above process improves the stability of the aerogel structure through polyamic acid salt, polyimide, as a polymer material, has poor conductivity. After the graphene aerogel is impregnated with polyamic acid, it will affect the formation of the conductive network, resulting in reduced conductivity of the composite material. In order to solve this problem, the present invention adds a conductive polymer PEDOT:PSS to the polyamic acid salt solution. Sodium polystyrene sulfonate (PSS) is a common surfactant. When PEDOT is polymerized, PSS is introduced as a dopant. The hydrophilic PSS not only helps PEDOT to be more easily dispersed in the aqueous solution, but also PSS - Can be used as PEDOT + In the technical solution of the present invention, due to the electrostatic effect, the conductive polymer PEDOT:PSS is evenly dispersed in the polyamic acid salt solution, which not only plays the role of a surfactant to promote the uniform dispersion of polyimide on the graphene surface, but also acts as a conductive additive to give polyimide conductive properties and improve the conductivity of the gel powder.
[0009] Furthermore, in step (1), the graphene oxide concentration in the graphene oxide mixed solution is 0.5-2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to reducing agent is 1:(0.1-0.5); the heating reaction temperature is 60-90°C, and the time is 1-4h.
[0010] Furthermore, in step (1), the number average molecular weight of polyethylene glycol is 400-5000.
[0011] Furthermore, the polyamic acid solution in step (2) is prepared by polycondensation reaction of diamine monomer and dianhydride monomer as raw materials in an organic solvent; the dianhydride monomer is at least one of 4,4'-biphenyl ether dianhydride, biphenyl tetracarboxylic dianhydride, 1,2,4,5-pyromellitic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, bisphenol A type diether dianhydride, 4,4-oxydiphthalic anhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride; the diamine monomer is at least one of p-phenylenediamine, m-phenylenediamine, diaminodiphenyl sulfone, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane; and the organic solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and N-methylpyrrolidone.
[0012] Furthermore, in step (2), the tertiary amine is at least one of triethylamine, tripropylamine and triethanolamine; and the mass ratio of the polyamic acid powder to the tertiary amine is 1:(0.3-0.6).
[0013] Furthermore, the mass fraction of the PEDOT:PSS aqueous solution in step (3) is 1-5%. Furthermore, the mass ratio of PEDOT to PSS in the PEDOT:PSS aqueous solution is 1:2-2.8. An appropriate amount of PSS can maintain the high conductivity of PEDOT while improving the dispersion performance of PEDOT.
[0014] Furthermore, in step (3), the stirring rate is 400-600 r / min.
[0015] On the other hand, the present invention also provides an application of a conductive gel powder, wherein the conductive gel powder is used in the field of 3D printing polyurethane materials, and comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 1-15 parts of conductive gel powder; 1-5 parts of flow modifier. The conductive gel powder is applied to the field of 3D printing polyurethane materials, which greatly improves the conductivity and mechanical properties of polyurethane materials.
[0016] Beneficial effects: (1) The present invention uses polyethylene glycol and graphene oxide as raw materials to first prepare graphene hydrogel, construct graphene-based gel materials, and improve the stability of the graphene hydrogel structure. The polyamic acid salt aqueous solution is added dropwise to the graphene hydrogel solution, so that the polyamic acid salt fully infiltrates the inside of the graphene hydrogel to construct the internal network of the gel.
[0017] (2) The present invention adds a conductive polymer PEDOT:PSS to the polyamic acid salt solution. The conductive polymer PEDOT:PSS is uniformly dispersed in the polyamic acid salt solution, not only acting as a surfactant to promote the uniform dispersion of polyimide on the graphene surface; but also as a conductive additive to impart conductive properties to the polyimide, thereby improving the conductivity of the gel powder.
[0018] (3) The modified gel powder obtained by the method of the present invention has extremely high electrical conductivity and adjustable mechanical properties, and is expected to be widely used in the field of 3D printing polyurethane materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a scanning electron microscope image of the gel powder prepared in Example 6.
[0020] Figure 2 This is a scanning electron microscope image of the gel powder prepared in Comparative Example 1. DETAILED DESCRIPTION
[0021] The present invention is further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the contents taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application. Among them, in the following examples and comparative examples, the mass fraction of the PEDOT:PSS aqueous solution is 3%, and the mass ratio of PEDOT and PSS in the PEDOT:PSS aqueous solution is 1:2.2.
[0022] Example 1 A method for preparing a conductive gel powder comprises the following steps: (1) Graphene oxide, a reducing agent and polyethylene glycol are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and heated to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol is 1:0.01; the concentration of graphene oxide in the graphene oxide mixed solution is 1 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C, and the time is 2 hours; the number average molecular weight of polyethylene glycol is 800; (2) Pour the polyamic acid solution into deionized water for precipitation, disperse a certain amount of the precipitated polyamic acid powder in deionized water, add tertiary amine, and stir until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1:0.1; the polyamic acid solution is prepared by polycondensing diamine monomer and dianhydride monomer as raw materials in an organic solvent; the dianhydride monomer is 4,4-oxydiphthalic anhydride; the diamine monomer is 4,4'-diaminodiphenylmethane; the molar ratio of dianhydride monomer to diamine monomer is 1:1.03; the organic solvent is N,N-dimethylformamide; the tertiary amine is triethanolamine; the mass ratio of polyamic acid powder to tertiary amine is 1:0.3; (3) adding the PEDOT:PSS aqueous solution to the polyamic acid salt solution and stirring to obtain a mixed polyamic acid salt solution; the mass ratio of PEDOT:PSS in the polyamic acid powder and the PEDOT:PSS aqueous solution is 1:0.01; the stirring rate is 500 r / min; (4) adding the mixed polyamic acid salt solution dropwise to the graphene hydrogel solution while stirring, and allowing the solution to stand after the addition is complete to obtain a polyamic acid / PEDOT:PSS / graphene mixed hydrogel; (5) The polyamic acid / PEDOT:PSS / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain a conductive gel powder.
[0023] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 5 parts of conductive gel powder; 2 parts of zinc stearate.
[0024] Example 2 A method for preparing a conductive gel powder comprises the following steps: (1) Graphene oxide, a reducing agent and polyethylene glycol are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and heated to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol is 1:0.1; the concentration of graphene oxide in the graphene oxide mixed solution is 1 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C, and the time is 2 hours; the number average molecular weight of polyethylene glycol is 800; (2) Pour the polyamic acid solution into deionized water for precipitation, disperse a certain amount of the precipitated polyamic acid powder in deionized water, add tertiary amine, and stir until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1:0.6; the polyamic acid solution is prepared by polycondensing diamine monomer and dianhydride monomer as raw materials in an organic solvent; the dianhydride monomer is 1,2,4,5-pyromellitic dianhydride; the diamine monomer is diaminodiphenyl sulfone; the molar ratio of dianhydride monomer to diamine monomer is 1:1.03; the organic solvent is N,N-dimethylformamide; the tertiary amine is tripropylamine; the mass ratio of polyamic acid powder to tertiary amine is 1:0.6; (3) adding the PEDOT:PSS aqueous solution to the polyamic acid salt solution and stirring to obtain a mixed polyamic acid salt solution; the mass ratio of PEDOT:PSS in the polyamic acid powder and the PEDOT:PSS aqueous solution is 1:0.2; and the stirring rate is 500 r / min; (4) adding the mixed polyamic acid salt solution dropwise to the graphene hydrogel solution while stirring, and allowing the solution to stand after the addition is complete to obtain a polyamic acid / PEDOT:PSS / graphene mixed hydrogel; (5) The polyamic acid / PEDOT:PSS / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain a conductive gel powder.
[0025] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 5 parts of conductive gel powder; 5 parts of zinc stearate.
[0026] Example 3 A method for preparing a conductive gel powder comprises the following steps: (1) Graphene oxide, a reducing agent and polyethylene glycol are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and heated to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol is 1:0.03; the concentration of graphene oxide in the graphene oxide mixed solution is 1 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C and the time is 2 hours; the number average molecular weight of polyethylene glycol is 800; (2) Pour the polyamic acid solution into deionized water for precipitation, disperse a certain amount of the precipitated polyamic acid powder in deionized water, add tertiary amine, and stir until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1:0.2; the polyamic acid solution is prepared by polycondensation reaction of diamine monomer and dianhydride monomer as raw materials in an organic solvent; the dianhydride monomer is a mixture of 4,4'-biphenyl ether dianhydride and biphenyltetracarboxylic acid dianhydride in a molar ratio of 1:1; the diamine monomer is 4,4'-diaminodiphenyl ether; the molar ratio of dianhydride monomer to diamine monomer is 1:1.03; the organic solvent is a mixture of N,N-dimethylformamide and N,N-dimethylacetamide; the tertiary amine is triethylamine; the mass ratio of polyamic acid powder to tertiary amine is 1:0.4; (3) adding the PEDOT:PSS aqueous solution to the polyamic acid salt solution and stirring to obtain a mixed polyamic acid salt solution; the mass ratio of PEDOT:PSS in the polyamic acid powder and the PEDOT:PSS aqueous solution is 1:0.05; and the stirring rate is 500 r / min; (4) adding the mixed polyamic acid salt solution dropwise to the graphene hydrogel solution while stirring, and allowing the solution to stand after the addition is complete to obtain a polyamic acid / PEDOT:PSS / graphene mixed hydrogel; (5) The polyamic acid / PEDOT:PSS / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain a conductive gel powder.
[0027] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 6 parts of conductive gel powder; 2 parts of zinc stearate.
[0028] Example 4 A method for preparing a conductive gel powder comprises the following steps: (1) Graphene oxide, a reducing agent and polyethylene glycol are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and heated to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol is 1:0.08; the concentration of graphene oxide in the graphene oxide mixed solution is 1 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C, and the time is 2 hours; the number average molecular weight of polyethylene glycol is 800; (2) Pour the polyamic acid solution into deionized water for precipitation, disperse a certain amount of the precipitated polyamic acid powder in deionized water, add tertiary amine, and stir until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1:0.5; the polyamic acid solution is prepared by polycondensation reaction of diamine monomer and dianhydride monomer as raw materials in an organic solvent; the dianhydride monomer is 3,3',4,4'-benzophenonetetracarboxylic dianhydride; the diamine monomer is 4,4'-diaminodiphenylmethane; the molar ratio of dianhydride monomer to diamine monomer is 1:1.03; the organic solvent is N,N-dimethylformamide; the tertiary amine is triethylamine; the mass ratio of polyamic acid powder to tertiary amine is 1:0.5; (3) adding the PEDOT:PSS aqueous solution to the polyamic acid salt solution and stirring to obtain a mixed polyamic acid salt solution; the mass ratio of PEDOT:PSS in the polyamic acid powder and the PEDOT:PSS aqueous solution is 1:0.18; the stirring rate is 500 r / min; (4) adding the mixed polyamic acid salt solution dropwise to the graphene hydrogel solution while stirring, and allowing the solution to stand after the addition is complete to obtain a polyamic acid / PEDOT:PSS / graphene mixed hydrogel; (5) The polyamic acid / PEDOT:PSS / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain a conductive gel powder.
[0029] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 6 parts of conductive gel powder; 4 parts of zinc stearate.
[0030] Example 5 A method for preparing a conductive gel powder comprises the following steps: (1) Graphene oxide, a reducing agent and polyethylene glycol are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and heated to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol is 1:0.04; the concentration of graphene oxide in the graphene oxide mixed solution is 1 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C and the time is 2 h; the number average molecular weight of polyethylene glycol is 800; (2) Pour the polyamic acid solution into deionized water for precipitation, disperse a certain amount of the precipitated polyamic acid powder in deionized water, add tertiary amine, and stir until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1:0.6; the polyamic acid solution is prepared by polycondensation reaction of diamine monomer and dianhydride monomer as raw materials in an organic solvent; the dianhydride monomer is a mixture of 4,4'-biphenyl ether dianhydride and biphenyltetracarboxylic acid dianhydride in a molar ratio of 1:1; the diamine monomer is a mixture of diaminodiphenyl sulfone and 4,4'-diaminodiphenyl ether in a molar ratio of 1:1; the molar ratio of dianhydride monomer to diamine monomer is 1:1.03; the organic solvent is N,N-dimethylacetamide; the tertiary amine is triethylamine; the mass ratio of polyamic acid powder to tertiary amine is 1:0.5; (3) adding the PEDOT:PSS aqueous solution to the polyamic acid salt solution and stirring to obtain a mixed polyamic acid salt solution; the mass ratio of PEDOT:PSS in the polyamic acid powder and the PEDOT:PSS aqueous solution is 1:0.05; and the stirring rate is 500 r / min; (4) adding the mixed polyamic acid salt solution dropwise to the graphene hydrogel solution while stirring, and allowing the solution to stand after the addition is complete to obtain a polyamic acid / PEDOT:PSS / graphene mixed hydrogel; (5) The polyamic acid / PEDOT:PSS / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain a conductive gel powder.
[0031] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 7 parts of conductive gel powder; 5 parts of zinc stearate.
[0032] Example 6 A method for preparing a conductive gel powder comprises the following steps: (1) Graphene oxide, a reducing agent and polyethylene glycol are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and heated to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol is 1:0.05; the concentration of graphene oxide in the graphene oxide mixed solution is 1 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C, and the time is 2 hours; the number average molecular weight of polyethylene glycol is 800; (2) Pour the polyamic acid solution into deionized water for precipitation, disperse a certain amount of the precipitated polyamic acid powder in deionized water, add tertiary amine, and stir until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1:0.4; the polyamic acid solution is prepared by polycondensation reaction of diamine monomer and dianhydride monomer as raw materials in an organic solvent; the dianhydride monomer is a mixture of bisphenol A type diether dianhydride and 4,4-oxydiphthalic anhydride in a molar ratio of 1:1; the diamine monomer is 4,4'-diaminodiphenyl ether; the molar ratio of dianhydride monomer to diamine monomer is 1:1.03; the organic solvent is N,N-dimethylformamide; the tertiary amine is triethylamine; the mass ratio of polyamic acid powder to tertiary amine is 1:0.5; (3) adding the PEDOT:PSS aqueous solution to the polyamic acid salt solution and stirring to obtain a mixed polyamic acid salt solution; the mass ratio of PEDOT:PSS in the polyamic acid powder and the PEDOT:PSS aqueous solution is 1:0.1; and the stirring rate is 500 r / min; (4) adding the mixed polyamic acid salt solution dropwise to the graphene hydrogel solution while stirring, and allowing the solution to stand after the addition is complete to obtain a polyamic acid / PEDOT:PSS / graphene mixed hydrogel; (5) The polyamic acid / PEDOT:PSS / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain a conductive gel powder.
[0033] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 5 parts of conductive gel powder; 4 parts of zinc stearate.
[0034] Comparative Example 1 A method for preparing a conductive gel powder comprises the following steps: (1) Graphene oxide, a reducing agent, polyethylene glycol, and a PEDOT:PSS aqueous solution are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and heated to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol is 1:0.05; the concentration of graphene oxide in the graphene oxide mixed solution is 1 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C and the time is 2 h; the number average molecular weight of polyethylene glycol is 800; the mass ratio of PEDOT:PSS in the graphene oxide and PEDOT:PSS aqueous solution is 1:0.04; (2) Pour the polyamic acid solution into deionized water for precipitation, disperse a certain amount of the precipitated polyamic acid powder in deionized water, add tertiary amine, and stir until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1:0.4; the polyamic acid solution is prepared by polycondensation reaction of diamine monomer and dianhydride monomer as raw materials in an organic solvent; the dianhydride monomer is a mixture of bisphenol A type diether dianhydride and 4,4-oxydiphthalic anhydride in a molar ratio of 1:1; the diamine monomer is 4,4'-diaminodiphenyl ether; the molar ratio of dianhydride monomer to diamine monomer is 1:1.03; the organic solvent is N,N-dimethylformamide; the tertiary amine is triethylamine; the mass ratio of polyamic acid powder to tertiary amine is 1:0.5; (3) adding the polyamic acid salt solution dropwise to the graphene hydrogel solution while stirring, and allowing the solution to stand after the addition is complete to obtain a polyamic acid / PEDOT:PSS / graphene mixed hydrogel; (4) The polyamic acid / PEDOT:PSS / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain a conductive gel powder.
[0035] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 5 parts of conductive gel powder; 4 parts of zinc stearate.
[0036] Comparative Example 2 A method for preparing a conductive gel powder comprises the following steps: (1) Graphene oxide, a reducing agent and polyethylene glycol are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and heated to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol is 1:0.05; the concentration of graphene oxide in the graphene oxide mixed solution is 1 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C, and the time is 2 hours; the number average molecular weight of polyethylene glycol is 800; (2) Pour the polyamic acid solution into deionized water for precipitation, disperse a certain amount of the precipitated polyamic acid powder in deionized water, add tertiary amine, and stir until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1:0.4; the polyamic acid solution is prepared by polycondensation reaction of diamine monomer and dianhydride monomer as raw materials in an organic solvent; the dianhydride monomer is a mixture of bisphenol A type diether dianhydride and 4,4-oxydiphthalic anhydride in a molar ratio of 1:1; the diamine monomer is 4,4'-diaminodiphenyl ether; the molar ratio of dianhydride monomer to diamine monomer is 1:1.03; the organic solvent is N,N-dimethylformamide; the tertiary amine is triethylamine; the mass ratio of polyamic acid powder to tertiary amine is 1:0.5; (3) adding the PEDOT:PSS aqueous solution to the polyamic acid salt solution and stirring to obtain a mixed polyamic acid salt solution; the mass ratio of PEDOT:PSS in the polyamic acid powder and the PEDOT:PSS aqueous solution is 1:0.5; and the stirring rate is 500 r / min; (4) adding the mixed polyamic acid salt solution dropwise to the graphene hydrogel solution while stirring, and allowing the solution to stand after the addition is complete to obtain a polyamic acid / PEDOT:PSS / graphene mixed hydrogel; (5) The polyamic acid / PEDOT:PSS / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain a conductive gel powder.
[0037] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 5 parts of conductive gel powder; 4 parts of zinc stearate.
[0038] Comparative Example 3 A method for preparing a conductive gel powder comprises the following steps: (1) Graphene oxide and a reducing agent are dispersed in deionized water to obtain a graphene oxide mixed solution, which is then sealed and heated to obtain a graphene hydrogel solution; the graphene oxide concentration in the graphene oxide mixed solution is 1 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the heating reaction temperature is 70°C and the time is 2 h; (2) Pour the polyamic acid solution into deionized water for precipitation, disperse a certain amount of the precipitated polyamic acid powder in deionized water, add tertiary amine, and stir until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1:0.4; the polyamic acid solution is prepared by polycondensation reaction of diamine monomer and dianhydride monomer as raw materials in an organic solvent; the dianhydride monomer is a mixture of bisphenol A type diether dianhydride and 4,4-oxydiphthalic anhydride in a molar ratio of 1:1; the diamine monomer is 4,4'-diaminodiphenyl ether; the molar ratio of dianhydride monomer to diamine monomer is 1:1.03; the organic solvent is N,N-dimethylformamide; the tertiary amine is triethylamine; the mass ratio of polyamic acid powder to tertiary amine is 1:0.5; (3) adding the PEDOT:PSS aqueous solution to the polyamic acid salt solution and stirring to obtain a mixed polyamic acid salt solution; the mass ratio of PEDOT:PSS in the polyamic acid powder and the PEDOT:PSS aqueous solution is 1:0.1; and the stirring rate is 500 r / min; (4) adding the mixed polyamic acid salt solution dropwise to the graphene hydrogel solution while stirring, and allowing the solution to stand after the addition is complete to obtain a polyamic acid / PEDOT:PSS / graphene mixed hydrogel; (5) The polyamic acid / PEDOT:PSS / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain a conductive gel powder.
[0039] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 5 parts of conductive gel powder; 4 parts of zinc stearate.
[0040] The 3D printed polyurethane materials in Examples 1-6 and Comparative Examples 1-3 were printed into strips, and the tensile properties of the strips were tested with reference to GB / T528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber, and the conductivity of the 3D printed polyurethane materials was tested using a conductivity tester.
[0041] Figure 1 This is a scanning electron microscope image of the conductive gel powder prepared in Example 6. It can be seen from the figure that the gel powder prepared by the present invention has a rich pore structure and good uniformity, and can be well compounded with thermoplastic polyurethane resin, which is beneficial to the improvement of the tensile strength and conductive properties of 3D printed polyurethane materials. Figure 2 This is a scanning electron microscope image of the conductive gel powder prepared in Comparative Example 1; the conductive polymer PEDOT:PSS is added to the graphene oxide in advance. Due to the electrostatic interaction between the conductive polymer PEDOT:PSS and the graphene oxide, the graphenes are easily agglomerated with each other, destroying the formation of the gel structure. It can be seen from Examples 1-6 and Comparative Examples 1-3 that the present invention uses polyethylene glycol and graphene oxide as raw materials to first prepare graphene hydrogels, construct graphene-based gel materials, and improve the stability of the graphene hydrogel structure. Then the conductive polymer PEDOT:PSS is added to the polyamic acid salt solution. The conductive polymer PEDOT:PSS is uniformly dispersed in the polyamic acid salt solution, which not only plays the role of a surfactant and promotes the uniform dispersion of polyimide on the graphene surface; but also itself, as a conductive additive, gives the polyimide conductive properties and improves the conductivity of the gel powder. Comparative Example 1 directly adds the conductive polymer PEDOT:PSS to the graphene oxide, which cannot play the role of giving the polyimide conductivity and uniform dispersion, which is not conducive to the improvement of the mechanical properties of the composite material. Comparative Example 2 shows that when the conductive polymer PEDOT:PSS is added in excessive amounts, its conductivity is limited and the mechanical properties of the material are reduced. Comparative Example 3 shows that polyethylene glycol, as a good modifier, is not only conducive to the dispersion of graphene, but also can form hydrogen bonds with oxygen-containing functional groups such as carboxyl or hydroxyl groups on the surface of graphene, thereby enhancing the interaction between graphene sheets and improving the stability of the graphene hydrogel structure.
[0042] The above basic examples of the present invention and their further selected examples can be freely combined to form multiple embodiments, all of which are embodiments that can be adopted and claimed by the present invention. In the scheme of the present invention, each selected example can be arbitrarily combined with any other basic example and selected example. Those skilled in the art will know that there are many combinations.
[0043] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a conductive gel powder, characterized in that: The following steps are involved: (1) dispersing graphene oxide, a reducing agent and polyethylene glycol in deionized water to obtain a graphene oxide mixed solution, sealing the solution and heating the solution to obtain a graphene hydrogel solution; the mass ratio of graphene oxide to polyethylene glycol is 1:(0-0.1); wherein the mass of polyethylene glycol is not 0; (2) pouring the polyamic acid solution into deionized water for precipitation, dispersing a certain amount of the precipitated polyamic acid powder in deionized water, adding tertiary amine, and stirring until the polyamic acid powder is completely dissolved to obtain a polyamic acid salt solution; the mass ratio of graphene oxide to polyamic acid powder is 1: (0.1-0.6); (3) adding the PEDOT:PSS aqueous solution to the polyamic acid salt solution and stirring to obtain a mixed polyamic acid salt solution; the mass ratio of PEDOT:PSS in the polyamic acid powder and the PEDOT:PSS aqueous solution is 1:(0.01-0.2); (4) adding the mixed polyamic acid salt solution dropwise to the graphene hydrogel solution while stirring, and allowing the solution to stand after the addition is complete to obtain a polyamic acid / PEDOT:PSS / graphene mixed hydrogel; (5) The polyamic acid / PEDOT:PSS / graphene mixed hydrogel is freeze-dried, thermally imidized, and crushed to obtain a conductive gel powder.
2. The method for preparing a conductive gel powder according to claim 1, characterized in that: Step (1) The graphene oxide concentration in the graphene oxide mixed solution is 0.5-2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:(0.1-0.5); the heating reaction temperature is 60-90° C., and the time is 1-4 hours.
3. The method for preparing a conductive gel powder according to claim 1, characterized in that: The number average molecular weight of polyethylene glycol in step (1) is 400-5000.
4. The method for preparing a conductive gel powder according to claim 1, characterized in that: The polyamic acid solution in step (2) is prepared by polycondensation reaction of diamine monomer and dianhydride monomer as raw materials in an organic solvent; the dianhydride monomer is at least one of 4,4'-biphenyl ether dianhydride, biphenyl tetracarboxylic dianhydride, 1,2,4,5-pyromellitic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, bisphenol A type diether dianhydride, 4,4-oxydiphthalic anhydride and 1,2,4,5-cyclohexanetetracarboxylic dianhydride; the diamine monomer is at least one of p-phenylenediamine, m-phenylenediamine, diaminodiphenyl sulfone, 4,4'-diaminodiphenyl ether and 4,4'-diaminodiphenylmethane; and the organic solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and N-methylpyrrolidone.
5. The method for preparing a conductive gel powder according to claim 1, characterized in that: In step (2), the tertiary amine is at least one of triethylamine, tripropylamine and triethanolamine; and the mass ratio of the polyamic acid powder to the tertiary amine is 1:(0.3-0.6).
6. The method for preparing a conductive gel powder according to claim 1, characterized in that: The mass fraction of the PEDOT:PSS aqueous solution in step (3) is 1-5%.
7. The method for preparing a conductive gel powder according to claim 1, characterized in that: The stirring rate in step (3) is 400-600 r / min.
8. A conductive gel powder, characterized in that: The conductive gel powder is prepared by the preparation method of any one of claims 1 to 7.
9. An application of the conductive gel powder as claimed in claim 8, characterized in that: Conductive gel powder is used in the field of 3D printing polyurethane materials.
10. A 3D printing polyurethane material, characterized in that: Contains the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 1-15 parts of conductive gel powder; 1-5 parts of flow modifier; the conductive gel powder is the conductive gel powder according to claim 8.
Citation Information
Patent Citations
Preparation method of BN / epoxy resin heat conductive insulation composite material
CN109280332A
Method for preparing graphene / polyimide composite aerogel
CN110591142A
High-temperature-resistant and low-temperature-resistant piezoresistive sensing polyimide composite aerogel and preparation method thereof
CN110776741A
Modified polyimide aerogel, preparation method and application thereof
CN111909418A
High-conductivity flexible polyimide composite film and preparation method thereof
CN113337116A
Cited By
Antistatic aerogel for 3D printing and preparation method and application thereof
CN120818176A
Antistatic aerogel for 3D printing and preparation method and application thereof
CN120818176B
High-performance antistatic aerogel for 3D printing as well as preparation method and application thereof
CN120865604A
An antistatic aerogel for high-performance 3D printing and a preparation method and application thereof
CN120865604B
High-strength conductive aerogel powder as well as preparation method and application thereof
CN121427169A