Ultraviolet curing polyvinylidene fluoride adhesive
By optimizing the formula and forming a cross-linked network structure, the problem of poor bonding effect of traditional adhesives on low surface energy plastics has been solved, and an efficient and environmentally friendly UV-cured polyvinylidene fluoride adhesive has been realized, which is suitable for bonding electronic products.
Patent Information
- Application Number
- CN202410988256.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-25
AI Technical Summary
Traditional UV-curable adhesives have poor bonding effects on low-surface-energy plastics, and suffer from environmental pollution and low production efficiency.
A UV-curable polyvinylidene fluoride adhesive is used to form a cross-linked network structure by optimizing the formula, including reactive diluent, photoinitiator, polyvinylidene fluoride prepolymer with conjugated double bonds and silane coupling agent. Improve bonding properties and reduce surface energy.
It achieves good adhesion to low surface energy plastics, improves temperature and humidity resistance and dielectric properties, simplifies the process, reduces environmental pollution, and improves production efficiency and mechanical properties.
Smart Images

Figure BDA0004958111590000081
Abstract
Description
Technical Field
[0001] The invention relates to the field of ultraviolet light curing adhesives, in particular to an ultraviolet light curing polyvinylidene fluoride adhesive. Background Art
[0002] With the lightweight development of electronic products such as mobile phones, computers, and cameras, the plastic parts in electronic products have been upgraded, and low surface energy plastics are widely used in them. Many parts need to be bonded with adhesives, among which UV adhesives are widely used due to their simple and efficient bonding process, environmental protection and pollution-free. However, traditional UV adhesives have the disadvantages of poor adhesion to low surface energy plastics, weak electrochemical stability, and poor temperature and humidity resistance.
[0003] PVDF adhesives have excellent weather resistance, low surface energy, good electrochemical stability, temperature and humidity resistance, and excellent bonding properties. However, traditional PVDF adhesives must be used with polar solvents, which cause serious environmental pollution, complex processing, and high energy consumption. In addition, existing PVDF adhesives are prone to debonding and failure when used in electronic products under high temperature and high humidity conditions, and have poor adhesion to low-surface-energy plastic substrates.
[0004] For example, CN102994012A discloses a method for preparing an adhesive for bonding fluoroplastics. The invention product uses polyvinylidene fluoride and trifluoroethylene copolymer, polyvinyl alcohol furfural, resorcinol-formaldehyde resin, triethyl citrate, polysiloxane resin, reinforcing silica, benzene, and acetone as raw materials, and uses a melting box and a stirring box as equipment to prepare an adhesive for bonding fluoroplastics. The preparation method has a simple production process and uses general equipment. The product has excellent adhesion, high and low temperature resistance, chemical resistance, high impact strength, and is extremely convenient to use. It is mainly used for bonding between fluoroplastic products, and can also be used for bonding fluoroplastic products and other materials. The disadvantage is that a large amount of organic solvents need to be used, which is easy to cause environmental pollution, and the curing process is cumbersome, which is easy to cause insufficient solvent volatilization, affecting the mechanical properties and bonding properties of the film. At the same time, polyvinylidene fluoride has poor compatibility with other resins in the adhesive, which is easy to cause uneven dispersion of various resins in the film, and unstable performance occurs.
[0005] For example, CN112375169A discloses a novel binder synthesis method, including the following steps: (1) filling a reactor with inert gas and adding reaction raw materials; (2) adding deionized water, initiator and emulsifier into the reactor; (3) introducing monomer vinylidene fluoride and monomer ethylene into the reactor; (4) heating reaction for 10-30h; (5) reducing pressure after the reaction is completed; (6) obtaining a novel binder after condensation, washing, separation, drying and crushing of the reaction product. This invention replaces the F atoms in PVDF with H atoms, reduces crystallinity, improves flexibility, and reduces the probability of HF elimination reaction, effectively avoiding slurry gelation; reduces the amount of vinylidene fluoride used, which can not only reduce material costs, but also reduce the damage of F in VDF to equipment; and the adhesion itself is strong, and there is no need to compound other PVDF to increase adhesion. The disadvantages are that the reaction time of polyvinylidene fluoride is too long, the production efficiency is low, the adhesion of the solvent-based adhesive is poor, the bonding effect with polar materials is not ideal, which limits its application range and has weak thermal stability. It needs to be used with a large amount of organic solvents, which is easy to cause environmental pollution, and the curing process is cumbersome. Summary of the invention
[0006] In order to overcome the defects of the prior art, the purpose of the present invention is to develop a UV-curable polyvinylidene fluoride adhesive having excellent temperature and moisture resistance and electrochemical properties and good adhesion to low surface energy plastics.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a UV-curable polyvinylidene fluoride adhesive, whose raw material composition is as follows, by weight: 20 to 45 parts of active diluent, 1 to 3.5 parts of photoinitiator, 20 to 60 parts of polyvinylidene fluoride prepolymer with conjugated double bonds, 10 to 30 parts of filler, and 0.1 to 3.5 parts of silane coupling agent.
[0008] As a preferred embodiment of the present invention, the active diluent is at least one of acrylpyrrolidone, methyl vinyl sulfone, methacrylamide, vinyl pyrrolidone, propoxylated neopentyl glycol diacrylate, trimethylolpropane triacrylate, and norbornene acrylate.
[0009] As a preferred embodiment of the present invention, the photoinitiator is at least one of 2,4,6-trimethylbenzoyldiphenoxyphosphine, 1-hydroxycyclohexylphenyl ketone and 2,4,6-trimethylbenzoylphenyl phosphonic acid ethyl ester.
[0010] As a preferred embodiment of the present invention, the silane coupling agent is at least one of aminopropyltriethoxysilane and γ-aminopropyltrimethoxysilane.
[0011] As a preferred embodiment of the present invention, the filler is at least one of silicon dioxide, calcium oxide, calcium carbonate and mica.
[0012] As a preferred embodiment of the present invention, the polyvinylidene fluoride prepolymer having conjugated double bonds is prepared according to the following method:
[0013] (1) 500-700 parts of deionized water, 5-15 parts of dispersant, 0.5-2 parts of initiator, 1-3 parts of chain transfer agent, 70-90 parts of vinylidene fluoride monomer and 5-25 parts of acrylate monomer are polymerized at a reaction temperature of 30-90° C., a reaction time of 4-8 hours, and a reaction pressure of 4-8 MPa. After the reaction is completed, the product is filtered, washed, and dried to obtain a polyvinylidene fluoride resin;
[0014] (2) reacting the polyvinylidene fluoride resin obtained in step (1) in an alkaline solution at a reaction temperature of 40 to 80° C. for a reaction time of 0.5 to 3 hours, filtering the obtained product, washing, and drying to obtain a polyvinylidene fluoride prepolymer having conjugated double bonds.
[0015] As a preferred embodiment of the present invention, the dispersant is at least one of methyl cellulose, polyethylene glycol, sodium dodecylbenzene sulfonate and sodium dodecyl sulfate.
[0016] As a preferred embodiment of the present invention, the initiator is at least one of azobisisobutyronitrile, di-tert-butyl peroxide, tert-butylbenzoyl, methyl ethyl ketone peroxide, and dicyclohexyl peroxydicarbonate.
[0017] As a preferred embodiment of the present invention, the chain transfer agent is at least one of acetone, secondary dodecyl mercaptan, acetic acid, n-butanol, and butyl acetate.
[0018] As a preferred embodiment of the present invention, the acrylic acid ester monomer is at least one of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, and hydroxyethyl acrylate.
[0019] In the present invention, the active diluent can be one or a mixture of norbornene acrylate, hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, 2-phenoxyethyl acrylate, lauric acid acrylate, trimethylolpropane triacrylate, 1,6-hexanediol diacrylate, propoxylated neopentyl glycol diacrylate, cyclodecane dimethanol diacrylate, polyethylene glycol (200) diacrylate, vinyl pyrrolidone, acryl pyrrolidone, vinyl formamide, methacrylamide, methyl vinyl sulfone, phenyl vinyl sulfone. As a preferred embodiment of the present invention, the active diluent is at least one of acryl pyrrolidone, methyl vinyl sulfone, methacrylamide, vinyl pyrrolidone, propoxylated neopentyl glycol diacrylate, trimethylolpropane triacrylate, and norbornene acrylate.
[0020] In the present invention, the photoinitiator can be one or a mixture of 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2-hydroxy-4-(2-hydroxyethoxy)-2-methylphenylpropiophenone, benzyl dimethyl ether, 2,4,6-trimethylbenzoyl diphenyl oxide, 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinebenzylphenyl) butanone, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, benzophenone, and 2-isopropylthioxanthone. As a preferred embodiment of the present invention, the photoinitiator is at least one of 2,4,6-trimethylbenzoyldiphenoxyphosphine, 1-hydroxycyclohexylphenyl ketone and 2,4,6-trimethylbenzoylphenyl phosphonic acid ethyl ester.
[0021] In the present invention, the silane coupling agent can be one or a mixture of two of aminopropyl triethoxysilane, γ-aminopropyl methyl diethoxy silane, γ-aminopropyl triethoxy silane, γ-aminopropyl trimethoxy silane, and γ-glycidyl ether oxypropyl trimethoxy silane. As a preferred embodiment of the present invention, the silane coupling agent is at least one of aminopropyl triethoxy silane and γ-aminopropyl trimethoxy silane.
[0022] The present invention improves the bonding performance of UV-curable adhesives with low surface energy materials by optimizing the polymerization formula, and has the advantages of excellent temperature and moisture resistance, excellent dielectric properties, and low surface energy, thereby solving the problem of poor bonding effect of UV-curable adhesives with low surface energy materials in the prior art. The polyvinylidene fluoride prepolymer in the present invention has conjugated double bonds. Under the action of the ultraviolet light initiator, the double bonds of the polyvinylidene fluoride prepolymer and the double bonds of the polar diluent undergo addition reaction and crosslinking and solidification to form a cross-linked network structure, which greatly improves the molecular weight and the number of polar functional groups of the polymer, and effectively improves the bonding performance between the polymer and the substrate; the present invention can effectively regulate the hardness of the film by flexibly adjusting the functionality of the diluent, greatly broadening the application scenarios of the film. Compared with solvent-based adhesives, the present invention does not contain volatile solvents, is more environmentally friendly, has a simple UV curing process, and the formed cross-linked network structure has better thermal stability and mechanical properties. In the present invention, the introduction of the comonomer acrylate can enhance the ability of the prepolymer polyvinylidene fluoride resin to dissolve in the reactive diluent, and can also reduce the crystallinity of the polyvinylidene fluoride resin to increase its toughness, while preventing the polyvinylidene fluoride resin from removing too much HF in an alkaline environment to affect the performance of the polyvinylidene fluoride resin. After being cured by ultraviolet light, the ultraviolet light-cured polyvinylidene fluoride adhesive of the present invention has excellent temperature and humidity resistance and dielectric properties, and low surface energy, and solves the problem of poor bonding effect between the ultraviolet light-cured adhesive and low surface energy materials, and is particularly suitable for bonding electronic or industrial products of low surface energy materials such as polypropylene, polyethylene, and fluoroplastics, and has a good bonding effect.
[0023] Compared with the prior art, the advantages of the present invention are:
[0024] 1. Compared with the traditional solvent-based homopolymer polyvinylidene fluoride adhesive, the introduction of the comonomer acrylate in the present invention can enhance the ability of the polyvinylidene fluoride resin to dissolve in the solvent, and can also reduce the crystallinity of the polyvinylidene fluoride resin to increase its toughness, while blocking the chain reaction of the polyvinylidene fluoride resin in an alkaline environment to remove HF, thereby improving its alkali resistance. After UV curing, the product has a contact angle of more than 97° and a dielectric constant of the film of more than 4.2.
[0025] 2. The present invention solves the problem of poor bonding effect between UV-curable adhesives and low-surface-energy materials in the prior art. The polyvinylidene fluoride resin in the present invention has conjugated double bonds after being treated with alkali solution to remove HF. Under the action of the UV initiator, the double bonds of the polyvinylidene fluoride prepolymer and the double bonds of the polar diluent undergo addition reaction and crosslinking and solidification to form a crosslinked network structure, which introduces a large number of polar functional groups and greatly increases its molecular weight, effectively improving the bonding strength between the adhesive and the substrate, forming a cured bond between the adhesive and the substrate, and having good adhesion to low-surface-energy plastics. Compared with traditional UV adhesive prepolymers such as polyurethane acrylate, epoxy acrylate and polyacrylate, the CF bond energy in the polyvinylidene fluoride prepolymer is higher, the corrosion resistance is better, the dielectric properties are better, the surface energy is lower, and the adhesion to low-surface-energy plastics is better. The room-temperature bonding strength of PP-PP is above 7.3MPa, and the bonding strength of PP-PP "double 85" is 6.57MPa.
[0026] 3. The present invention can effectively adjust the hardness of the film by flexibly adjusting the functionality of the diluent, greatly broadening the application scenarios of the film. Compared with solvent-based adhesives, the present invention does not contain volatile solvents, is more environmentally friendly, has a simple UV curing process, high production efficiency, and the formed cross-linked network structure has better thermal stability and mechanical properties. At the same time, UV curing adhesives can flexibly adjust the type and proportion of polar diluents, making it easier to control the molecular weight of the adhesive and its various properties. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the following description is only used to explain the present invention but not to limit the present invention.
[0028] Example 1
[0029] A UV-curable polyvinylidene fluoride adhesive comprises the following materials: 7 g of vinyl pyrrolidone, 15 g of acryl pyrrolidone, 12 g of methyl vinyl sulfone, 2 g of 2,4,6-trimethylbenzoyldiphenylphosphine, 1 g of 1-hydroxycyclohexylphenyl ketone, 30 g of polyvinylidene fluoride resin prepolymer, 30 g of silicon dioxide powder (average particle size 10 μm), 2 g of aminopropyltriethoxysilane and 1 g of gamma-aminopropyltrimethoxysilane.
[0030] Wherein, the preparation method of polyvinylidene fluoride resin prepolymer is as follows:
[0031] (1) 600 g of deionized water, 8 g of 1 wt% methyl cellulose, 2.5 g of acetone and 1 g of di-tert-butyl peroxide were sequentially added into a reactor, and then 80 g of vinylidene fluoride monomer and 20 g of methyl acrylate were added into the reactor for supercritical polymerization reaction. The reaction pressure was 4.5 MPa, the reaction temperature was 52° C., and the reaction time was 4 h. After the reaction was completed, the polymerization product was filtered, washed, and dried to obtain polyvinylidene fluoride resin powder.
[0032] (2) Add the obtained polyvinylidene fluoride resin powder to a 5wt% NaOH solution, wherein the mass ratio of the polyvinylidene fluoride resin powder to the NaOH solution is 1:10, and heat in a 50°C water bath for 1 h to remove HF, filter, and re-wash the HF-removed polyvinylidene fluoride powder, and dry to obtain a polyvinylidene fluoride resin prepolymer containing conjugated double bonds.
[0033] Example 2
[0034] A UV-curable polyvinylidene fluoride adhesive comprises the following materials: 7 g of methacrylamide, 10 g of vinyl pyrrolidone, 4 g of propoxylated neopentyl glycol diacrylate, 0.5 g of 2,4,6-trimethylbenzoyldiphenoxyphosphine, 1 g of ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 35 g of polyvinylidene fluoride resin prepolymer, 20 g of silicon dioxide powder (average particle size 10 μm), and 2.6 g of gamma-aminopropyltrimethoxysilane.
[0035] Wherein, the preparation method of polyvinylidene fluoride resin prepolymer is as follows:
[0036] (1) 650 g of deionized water, 10 g of polyethylene glycol with a concentration of 1 wt%, 2.5 g of acetone and 1.1 g of methyl ethyl ketone peroxide are sequentially added into a reactor, and then 80 g of vinylidene fluoride monomer and 15 g of ethyl acrylate are added into the reactor for supercritical polymerization reaction. The reaction pressure is 5 MPa, the reaction temperature is 48° C., and the reaction time is 7 h. After the reaction is completed, the polymerization product is filtered, washed, and dried to obtain polyvinylidene fluoride resin powder.
[0037] (2) Add the obtained polyvinylidene fluoride resin powder to a 5wt% NaOH solution, wherein the mass ratio of the polyvinylidene fluoride resin powder to the NaOH solution is 1:30, and heat in a 40°C water bath for 2h to remove HF, filter, and re-wash the HF-removed polyvinylidene fluoride powder, and dry to obtain a polyvinylidene fluoride resin prepolymer containing conjugated double bonds.
[0038] Example 3
[0039] A UV-curable polyvinylidene fluoride adhesive comprises the following materials: 13 g of methyl vinyl sulfone, 10 g of vinyl pyrrolidone, 8 g of trimethylolpropane triacrylate, 9 g of norbornene acrylate, 0.7 g of 2,4,6-trimethylbenzoyldiphenylphosphine, 1 g of ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 40 g of polyvinylidene fluoride resin prepolymer, 15 g of calcium carbonate powder (average particle size 10 μm), and 0.8 g of gamma-aminopropyltrimethoxysilane.
[0040] Wherein, the preparation method of polyvinylidene fluoride resin prepolymer is as follows:
[0041] (1) 580 g of deionized water, 12 g of polyethylene glycol with a concentration of 1 wt%, 2.3 g of secondary dodecyl mercaptan and 1.2 g of azobisisobutyronitrile were sequentially added into a reactor, and then 75 g of vinylidene fluoride monomer and 10 g of hydroxyethyl acrylate were added into the reactor for supercritical polymerization reaction. The reaction pressure was 5.5 MPa, the reaction temperature was 65° C., and the reaction time was 6 h. After the reaction was completed, the polymerization product was filtered, washed, and dried to obtain polyvinylidene fluoride resin powder.
[0042] (2) Add the obtained polyvinylidene fluoride resin powder to a 5wt% NaOH solution, wherein the mass ratio of the polyvinylidene fluoride resin powder to the NaOH solution is 1:20, and heat in a 45°C water bath for 1.5h to remove HF, filter, and re-wash the HF-removed polyvinylidene fluoride powder, and dry to obtain a polyvinylidene fluoride resin prepolymer containing conjugated double bonds.
[0043] Example 4
[0044] A UV-curable polyvinylidene fluoride adhesive comprises the following materials: 7 g of norbornene acrylate, 10 g of methacrylamide, 8 g of vinyl pyrrolidone, 8 g of trimethylolpropane triacrylate, 1 g of 2,4,6-trimethylbenzoyldiphenylphosphine, 1.2 g of ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 50 g of polyvinylidene fluoride resin prepolymer, 25 g of calcium carbonate powder (average particle size 10 μm), and 1 g of gamma-aminopropyltrimethoxysilane.
[0045] Wherein, the preparation method of polyvinylidene fluoride resin prepolymer is as follows:
[0046] (1) 530 g of deionized water, 10 g of polyethylene glycol with a concentration of 1 wt%, 1.2 g of secondary acetic acid and 1.8 g of dicyclohexyl peroxydicarbonate were added to a reactor in sequence, and then 80 g of vinylidene fluoride monomer and 8 g of butyl acrylate were added to the reactor for supercritical polymerization reaction. The reaction pressure was 5.3 MPa, the reaction temperature was 66° C., and the reaction time was 8 h. After the reaction was completed, the polymerization product was filtered, washed, and dried to obtain polyvinylidene fluoride resin powder.
[0047] (2) Add the obtained polyvinylidene fluoride resin powder to a 5wt% NaOH solution, wherein the mass ratio of the polyvinylidene fluoride resin powder to the NaOH solution is 1:50, and heat in a 55°C water bath for 0.75h to remove HF, filter, and re-wash the HF-removed polyvinylidene fluoride powder, and dry to obtain a polyvinylidene fluoride resin prepolymer containing conjugated double bonds.
[0048] Example 5
[0049] A UV-curable polyvinylidene fluoride adhesive comprises the following materials: 7 g of methyl vinyl sulfone, 10 g of vinyl pyrrolidone, 3 g of trimethylolpropane triacrylate, 7 g of methacrylamide, 2 g of 2,4,6-trimethylbenzoyldiphenylphosphine, 1 g of ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 45 g of polyvinylidene fluoride resin prepolymer, 30 g of calcium carbonate powder (average particle size 10 μm), and 1.8 g of gamma-aminopropyltrimethoxysilane.
[0050] Wherein, the preparation method of polyvinylidene fluoride resin prepolymer is as follows:
[0051] (1) 630 g of deionized water, 10 g of polyethylene glycol with a concentration of 1 wt%, 1.5 g of n-butanol and 0.8 g of azobisisobutyronitrile were added to a reactor in sequence, and then 80 g of vinylidene fluoride monomer and 16 g of ethyl methacrylate copolymer were added to the reactor for supercritical polymerization reaction. The reaction pressure was 7.0 MPa, the reaction temperature was 78° C., and the reaction time was 6 h. After the reaction was completed, the polymerization product was filtered, washed, and dried to obtain polyvinylidene fluoride resin powder.
[0052] (2) Add the obtained polyvinylidene fluoride resin powder to a 5wt% NaOH solution, wherein the mass ratio of the polyvinylidene fluoride resin powder to the NaOH solution is 1:40, and heat in a 60°C water bath for 0.5h to remove HF, filter, and re-wash the HF-removed polyvinylidene fluoride powder, and dry to obtain a polyvinylidene fluoride resin prepolymer containing conjugated double bonds.
[0053] Comparative Example
[0054] The product was prepared according to the method of Example 1 of Chinese Patent Publication No. CN112375169A.
[0055] Performance Test:
[0056] The product performances obtained in Examples 1 to 5 and Comparative Example 1 were tested respectively, and the specific performances are shown in Table 1, where:
[0057] PP-PP room temperature bonding strength test: in accordance with GB / T7124-2008 adhesive tensile shear strength test standard.
[0058] PP-PP "double 85" bonding strength test: The cured bonding sample is placed in a high temperature and high humidity oven, and its bonding strength is tested after standing for 1000 hours at 85°C and 85% relative humidity according to GB / T5170-2016 standard and compared with the bonding strength measured at room temperature.
[0059] Contact angle test: Tested according to GB / T30447-2013 contact angle measurement method.
[0060] Dielectric constant test: According to GB / T31838.6-2021 dielectric constant test.
[0061] It can be seen from the data in Table 1 that the UV-curable polyvinylidene fluoride adhesives prepared in Examples 1 to 5 of the present invention have strong hydrophobic properties and low surface energy, and have better adhesion to low surface energy plastic PP (polypropylene). At the same time, the dielectric constant of the adhesive film is relatively high, and can be widely used in the field of electronic product bonding.
[0062] Table 1 Product performance of Examples 1 to 5 and Comparative Example 1
[0063]
Claims
1. A UV-curable polyvinylidene fluoride adhesive, characterized in that: The raw material composition is as follows by weight: 20 to 45 parts of active diluent, 1 to 3.5 parts of photoinitiator, 20 to 60 parts of polyvinylidene fluoride prepolymer with conjugated double bonds, 10 to 30 parts of filler, and 0.1 to 3.5 parts of silane coupling agent.
2. The UV-curable polyvinylidene fluoride adhesive according to claim 1, characterized in that: The active diluent is at least one of acryl pyrrolidone, methyl vinyl sulfone, methacrylamide, vinyl pyrrolidone, propoxylated neopentyl glycol diacrylate, trimethylolpropane triacrylate, and norbornene acrylate.
3. The UV-curable polyvinylidene fluoride adhesive according to claim 1, characterized in that: The photoinitiator is at least one of 2,4,6-trimethylbenzoyldiphenoxyphosphine, 1-hydroxycyclohexylphenyl ketone and 2,4,6-trimethylbenzoylphenyl phosphonic acid ethyl ester.
4. The UV-curable polyvinylidene fluoride adhesive according to claim 1, characterized in that: The silane coupling agent is at least one of aminopropyltriethoxysilane and γ-aminopropyltrimethoxysilane.
5. The UV-curable polyvinylidene fluoride adhesive according to claim 1, characterized in that: The filler is at least one of silicon dioxide, calcium oxide, calcium carbonate and mica.
6. The UV-curable polyvinylidene fluoride adhesive according to claim 1, characterized in that: The polyvinylidene fluoride prepolymer having conjugated double bonds is prepared according to the following method: (1) by weight, 500-700 parts of deionized water, 5-15 parts of dispersant, 0.5-2 parts of initiator, 1-3 parts of chain transfer agent, 70-90 parts of vinylidene fluoride monomer and 5-25 parts of acrylate monomer are polymerized at a reaction temperature of 30-90° C., a reaction time of 4-8 hours, and a reaction pressure of 4-8 MPa. After the reaction, the product is filtered, washed, and dried to obtain a polyvinylidene fluoride resin; (2) reacting the polyvinylidene fluoride resin obtained in step (1) in an alkaline solution at a reaction temperature of 40 to 80° C. for a reaction time of 0.5 to 3 hours, filtering the obtained product, washing, and drying to obtain a polyvinylidene fluoride prepolymer having conjugated double bonds.
7. The UV-curable polyvinylidene fluoride adhesive according to claim 6, characterized in that: The dispersant is at least one of methyl cellulose, polyethylene glycol, sodium dodecylbenzene sulfonate and sodium dodecyl sulfate.
8. The UV-curable polyvinylidene fluoride adhesive according to claim 6, characterized in that: The initiator is at least one of azobisisobutyronitrile, di-tert-butyl peroxide, tert-butylbenzoyl, methyl ethyl ketone peroxide, and dicyclohexyl peroxydicarbonate.
9. The UV-curable polyvinylidene fluoride adhesive according to claim 6, characterized in that: The chain transfer agent is at least one of acetone, secondary dodecyl mercaptan, acetic acid, n-butanol and butyl acetate.
10. The UV-curable polyvinylidene fluoride adhesive according to claim 6, characterized in that: The acrylic acid ester monomer is at least one of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate and hydroxyethyl acrylate.
Citation Information
Cited By