Martensitic steel with twin crystal substructure and preparation method of martensitic steel
By adjusting the raw material composition of Cr, Mn, Fe and other elements and the atomized powdering, heating and isostatic pressing process, low activation martensitic steel with twin substructure is generated, which solves the insufficient mechanical properties of existing low activation martensitic steel. and complex preparation process issues, achieving excellent mechanical properties at room temperature and high temperature and simplifying the process flow.
Patent Information
- Application Number
- CN202411214614.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-01
- Publication Date
- 2024-10-25
AI Technical Summary
The existing low-activation martensitic steel has insufficient mechanical properties and complicated preparation processes, resulting in high cost and low efficiency. Too much attention is paid to carbide precipitation strengthening and the strengthening of the martensite matrix is ignored, which easily introduces errors during the preparation process.
Cr, Mn, and Fe are used as the main raw materials through atomization to obtain pre-alloyed powder, which is degassed and hot isostatically pressed. The raw material composition and process parameters are adjusted to generate twin substructures, avoid high-temperature tempering, and simplify Process flow.
The mechanical properties of low-activation martensitic steel are significantly improved, especially showing good strong plasticity at room temperature and 650°C, simplifying the preparation process, reducing cost and time, and improving preparation efficiency.
Smart Images

Figure CN118835148A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of low-activated martensitic steel for nuclear power, in particular to a martensitic steel with a twin substructure and a preparation method thereof. Background Art
[0002] Nuclear fusion reactors require safe, reliable and efficient operation, and the key to achieving this goal lies in the structural materials used in them. Key components (such as the first wall and conversion components) composed of these structural materials maintain the normal operation of the reactor. Compared with other materials, low-activated ferrite heat-resistant steel is considered to be one of the best candidate structural materials for future nuclear fusion systems due to its low cost, good high-temperature creep performance and high-temperature radiation resistance. Compared with austenitic stainless steel, low-activated ferrite / martensitic steel has lower radiation swelling and thermal expansion coefficient, high thermal conductivity and other excellent thermophysical properties, and better resistance to liquid metal corrosion. At the same time, over the past three decades, countries around the world have been actively developing low-activated ferrite steels and have accumulated a lot of experience in the research and development of traditional ferrite / martensitic steels used in the core of nuclear fission reactors.
[0003] At present, the research on low-activated ferrite / martensitic steel widely carried out internationally is mainly focused on the following types: CLAM steel developed in China; F82H steel and JLF series developed in Japan; EUROFER97 being studied in Europe; 9Cr-2WVTa steel being studied in the United States. The above steels are mainly prepared by smelting and casting, and the standard heat treatment process is normalizing plus high-temperature tempering. The normalizing heating process should ensure complete austenitization and dissolution of the precipitate phase. In order to achieve a good combination of strength and plasticity, martensitic steel must be tempered after the normalizing treatment. Although the composition of different types of martensitic steels is slightly different, their microstructures are very similar. There are M at the original austenite grain boundaries, martensite block boundaries and martensite lath boundaries. 23 C6 carbides precipitate, and MX carbonitrides precipitate inside the lath.
[0004] At present, the maximum operating temperature of low-activated martensitic steel is 550°C. The following problems still exist through the existing alloy composition design criteria and preparation process: First, too much attention is paid to the precipitation strengthening effect of carbides, and the strengthening of the martensitic matrix is ignored, resulting in limited improvement in mechanical properties; Second, the existing preparation process is relatively complicated, and after smelting and casting, it still needs to go through multiple processes such as forging and rolling, which requires more time and energy and is prone to introduce errors in the process, making the preparation process costly and inefficient.
[0005] Therefore, it is necessary to invent a martensitic steel with a twin substructure and a preparation method thereof to solve the above problems. Summary of the invention
[0006] In order to solve the problems of insufficient mechanical properties and complex preparation process of existing low-activated martensitic steel, the present invention provides a martensitic steel with a twin substructure and a preparation method thereof.
[0007] The present invention is achieved by adopting the following technical solutions:
[0008] A method for preparing a martensitic steel having a twin substructure comprises the following steps:
[0009] S1: Using Cr, Mn and Fe as main raw materials, a pre-alloyed powder is obtained by atomization powder making, and the mass percentages of the main raw materials of the pre-alloyed powder are Cr: 8% to 10%, Mn: 2% to 3%, and the balance is Fe;
[0010] S2: The pre-alloyed powder is loaded into a stainless steel sheath, and the mixed powder in the stainless steel sheath is degassed at a temperature of 450° C. until the vacuum degree of the stainless steel sheath reaches 0.002 Pa;
[0011] S3: The stainless steel sheath with a vacuum degree of 0.002Pa is sealed and welded, and then placed in a hot isostatic pressing device for curing and molding. The heating rate is 5℃~10℃ / min, the molding temperature is 1150℃, the insulation time is 3h, and the molding pressure is 150MPa. After cooling to room temperature with the furnace, a martensitic steel with a twin substructure is obtained.
[0012] Furthermore, the raw material of the pre-alloyed powder also includes Ti, and the mass percentage of Ti is 0.05% to 0.2%.
[0013] Furthermore, the raw material of the pre-alloyed powder also includes C, and the mass percentage of C is 0% to 0.1%.
[0014] A martensitic steel with a twin substructure is obtained based on the above-mentioned method for preparing the martensitic steel with a twin substructure.
[0015] The key to the present invention lies in the raw material composition design of the pre-alloyed powder and the process parameters of hot isostatic pressing. The main raw materials and mass percentages of the pre-alloyed powder are Cr: 8% to 10%, Mn: 2% to 3%, and the balance is Fe, which determines that the pre-alloyed powder after degassing will undergo austenite transformation through the high-temperature heating process during the hot isostatic pressing process, and ferrite transformation and martensite transformation through the cooling process; different from the 0.5% Mn content in the previous low-activation martensitic steel, the Mn content is increased to 2% to 3% in the present invention, which is conducive to the generation of a certain amount of twins during the martensitic transformation process. The hot isostatic pressing process parameters will affect the austenite transformation during the high-temperature heating process and the martensitic transformation during the cooling process. The raw material composition design of the pre-alloyed powder and the heating rate during the hot isostatic pressing process in the present invention are crucial, and the two together determine the microscopic substructure characteristics of the martensitic structure in the martensitic steel after hot isostatic pressing, thereby significantly affecting the mechanical properties of the prepared low-activation martensitic steel.
[0016] The invention prepares the low-activated martensitic steel by adjusting the raw material composition design of the low-activated martensitic steel and adopting the method of atomizing pulverizing, heating and isostatic pressing. The prepared martensitic steel has a certain amount of twin substructure and exhibits good strength and plasticity at room temperature and 650°C. The plasticity can be ensured without high-temperature tempering heat treatment. The process is simple and purposeful, and is of great significance for further improving the mechanical properties of the existing low-activated martensitic steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is an electron backscatter diffraction (EBSD) photograph of the martensitic steel obtained in Example 1 of the present invention.
[0018] Figure 2 3 is a tensile property curve diagram of the martensitic steel obtained in Example 1 of the present invention at room temperature and 650°C.
[0019] Figure 3 This is an electron backscatter diffraction (EBSD) photograph of the martensitic steel obtained in Example 2 of the present invention.
[0020] Figure 4 It is a tensile property curve diagram of the martensitic steel obtained in Example 2 of the present invention at room temperature and 650°C.
[0021] Figure 5 This is an electron backscatter diffraction (EBSD) photograph of the martensitic steel obtained in Example 3 of the present invention.
[0022] Figure 6 3 is a tensile property curve diagram of the martensitic steel obtained in Example 3 of the present invention at room temperature and 650°C. DETAILED DESCRIPTION
[0023] A method for preparing a martensitic steel having a twin substructure comprises the following steps:
[0024] S1: Using Cr, Mn and Fe as main raw materials, a pre-alloyed powder is obtained by atomization powder making, and the mass percentages of the main raw materials of the pre-alloyed powder are Cr: 8% to 10%, Mn: 2% to 3%, and the balance is Fe;
[0025] S2: The pre-alloyed powder is loaded into a stainless steel sheath, and the mixed powder in the stainless steel sheath is degassed at a temperature of 450° C. until the vacuum degree of the stainless steel sheath reaches 0.002 Pa;
[0026] S3: The stainless steel sheath with a vacuum degree of 0.002Pa is sealed and welded, and then placed in a hot isostatic pressing device for curing and molding. The heating rate is 5℃~10℃ / min, the molding temperature is 1150℃, the insulation time is 3h, and the molding pressure is 150MPa. After cooling to room temperature with the furnace, a martensitic steel with a twin substructure is obtained.
[0027] The following are specific embodiments of the present invention, but the present invention is not limited to the following embodiments.
[0028] Example 1
[0029] S1: Using Cr, Mn and Fe as main raw materials, a pre-alloyed powder is obtained by atomization powder making, and the mass percentages of the main raw materials of the pre-alloyed powder are Cr: 8.7%, Mn: 2.2%, and the balance is Fe;
[0030] S2: The pre-alloyed powder is loaded into a stainless steel sheath, and the mixed powder in the stainless steel sheath is degassed at a temperature of 450° C. until the vacuum degree of the stainless steel sheath reaches 0.002 Pa;
[0031] S3: The stainless steel sheath with a vacuum degree of 0.002Pa is sealed and welded, and then placed in a hot isostatic pressing device for curing and molding. The heating rate is 8°C / min, the molding temperature is 1150°C, the insulation time is 3h, and the molding pressure is 150MPa. After cooling to room temperature with the furnace, a martensitic steel with a twin substructure is obtained.
[0032] Figure 1 This is an electron backscatter diffraction (EBSD) photograph of the martensitic steel obtained in this embodiment. It can be seen from the figure that the matrix structure of the martensitic steel obtained in this embodiment is martensitic laths, and the area marked with white circles in the figure is twins, which means that under the raw material composition and process conditions of this embodiment, the substructure in the martensitic laths has twin substructures in addition to dislocations. Figure 2The tensile properties curve of the martensitic steel obtained in this embodiment at room temperature and 650°C is shown in Figure 1. At room temperature, its tensile strength is 870MPa and its elongation is 10%; at 650°C, its tensile strength is 250MPa and its elongation is 23%. It can be seen that although the alloy composition of the low-activated steel in this embodiment is relatively simple, it still exhibits good mechanical properties at room temperature and 650°C. In addition, the low-activated martensitic steel prepared by the method of atomized powder heating and isostatic pressing can exhibit good plasticity without normalizing and high-temperature tempering.
[0033] Example 2
[0034] S1: Using Cr, Mn, Fe and Ti as raw materials, a pre-alloyed powder is obtained by atomization powder making, and the mass percentages of the raw materials of the pre-alloyed powder are Cr: 8.7%, Mn: 2.2%, Ti: 0.1%, and the balance is Fe;
[0035] S2: The pre-alloyed powder is loaded into a stainless steel sheath, and the mixed powder in the stainless steel sheath is degassed at a temperature of 450° C. until the vacuum degree of the stainless steel sheath reaches 0.002 Pa;
[0036] S3: The stainless steel sheath with a vacuum degree of 0.002Pa is sealed and welded, and then placed in a hot isostatic pressing device for curing and molding. The heating rate is 8°C / min, the molding temperature is 1150°C, the insulation time is 3h, and the molding pressure is 150MPa. After cooling to room temperature with the furnace, a martensitic steel with a twin substructure is obtained.
[0037] Figure 3 : This is an electron backscatter diffraction (EBSD) photograph of the martensitic steel obtained in this embodiment. It can be seen from the figure that the matrix structure of the martensitic steel obtained in this embodiment is a martensitic lath, and the area marked by the white circle in the figure is a twin, which means that under the raw material composition and process conditions of this embodiment, the substructure in the martensitic lath has a twin substructure in addition to the dislocation. Figure 4 The tensile properties curve of the martensitic steel obtained in this embodiment at room temperature and 650°C is shown in Figure 2. At room temperature, its tensile strength is 780MPa and its elongation is 14%; at 650°C, its tensile strength is 206MPa and its elongation is 47%. It can be seen that although the alloy composition of the low-activated steel in this embodiment is relatively simple, it still exhibits good mechanical properties at room temperature and 650°C. In addition, the low-activated martensitic steel prepared by the method of atomized powder heating and isostatic pressing can exhibit good plasticity without normalizing and high-temperature tempering.
[0038] Example 3
[0039] S1: Using Cr, Mn, Fe, Ti and C as raw materials, a pre-alloyed powder is obtained by atomization powder making, and the mass percentages of the raw materials of the pre-alloyed powder are Cr: 8.7%, Mn: 2.2%, Ti: 0.15%, C: 0.06%, and the balance is Fe;
[0040] S2: The pre-alloyed powder is loaded into a stainless steel sheath, and the mixed powder in the stainless steel sheath is degassed at a temperature of 450° C. until the vacuum degree of the stainless steel sheath reaches 0.002 Pa;
[0041] S3: The stainless steel sheath with a vacuum degree of 0.002Pa is sealed and welded, and then placed in a hot isostatic pressing device for curing and molding. The heating rate is 8°C / min, the molding temperature is 1150°C, the insulation time is 3h, and the molding pressure is 150MPa. After cooling to room temperature with the furnace, a martensitic steel with a twin substructure is obtained.
[0042] Figure 5 This is an electron backscatter diffraction (EBSD) photograph of the martensitic steel obtained in this embodiment. It can be seen from the figure that the matrix structure of the martensitic steel obtained in this embodiment is martensitic laths, and the area marked with white circles in the figure is twins, which means that under the raw material composition and process conditions of this embodiment, the substructure in the martensitic laths has twin substructures in addition to dislocations. Figure 6 The tensile properties curve of the martensitic steel obtained in this embodiment at room temperature and 650°C is shown in Figure 1. At room temperature, its tensile strength is 1173MPa and its elongation is 14%; at 650°C, its tensile strength is 247MPa and its elongation is 32%. It can be seen that when the raw materials of the low-activated martensitic steel are Cr, Mn, Ti, C and Fe, the low-activated steel in this embodiment still exhibits excellent mechanical properties at room temperature and 650°C.
[0043] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a martensitic steel having a twin substructure, characterized in that: The following steps are involved: S1: Using Cr, Mn and Fe as main raw materials, a pre-alloyed powder is obtained by atomization powder making, and the mass percentages of the main raw materials of the pre-alloyed powder are Cr: 8% to 10%, Mn: 2% to 3%, and the balance is Fe; S2: The pre-alloyed powder is loaded into a stainless steel sheath, and the mixed powder in the stainless steel sheath is degassed at a temperature of 450° C. until the vacuum degree of the stainless steel sheath reaches 0.002 Pa; S3: The stainless steel sheath with a vacuum degree of 0.002Pa is sealed and welded, and then placed in a hot isostatic pressing device for curing and molding. The heating rate is 5℃~10℃ / min, the molding temperature is 1150℃, the insulation time is 3h, and the molding pressure is 150MPa. After cooling to room temperature with the furnace, a martensitic steel with a twin substructure is obtained.
2. The method for preparing a martensitic steel having a twin substructure according to claim 1, characterized in that: In step S1: the raw material of the pre-alloyed powder also includes Ti, and the mass percentage of Ti is 0.05% to 0.2%.
3. The method for preparing a martensitic steel having a twin substructure according to claim 1, characterized in that: In step S1: the raw material of the pre-alloyed powder also includes C, and the mass percentage of C is 0% to 0.1%.
4. A martensitic steel having a twin substructure, wherein the martensitic steel is obtained based on the preparation method of the martensitic steel having a twin substructure as claimed in any one of claims 1 to 3.