Preparation process of aluminum-iron alloy special for aerospace-grade titanium alloy
By using a specific ratio of small particles of high-purity aluminum and high-purity iron in titanium alloy smelting and a medium-frequency induction furnace smelting process, the AlFe60 composite is formed, which solves the problems of iron segregation and aluminum burning loss, and improves the quality of titanium alloy ingots. Ingredient uniformity and stability.
Patent Information
- Application Number
- CN202410910744.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-25
AI Technical Summary
During the smelting process of titanium alloys, the addition of iron elements can easily lead to segregation, and the burning rate of aluminum elements is high, making it difficult to smelt, affecting the quality and stability of titanium alloy ingots.
Small particles of high-purity aluminum and high-purity iron are mixed according to a specific ratio. After being pressed into specification blocks by a hydraulic press, they are vacuum melted in a medium frequency induction furnace. The process parameters are controlled to form an AlFe60 composite and reduce iron segregation and aluminum burning loss.
It achieves uniform distribution of iron elements and low burning loss rate of aluminum elements, improves the composition uniformity and melting point proximity of finished titanium alloy products, and enhances the quality and stability of titanium alloy ingots.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of titanium alloys, and in particular relates to a preparation process of an aluminum-iron alloy special for aerospace-grade titanium alloys. Background Art
[0002] Titanium alloy materials are mainly used in aerospace, national defense and military industries. In the development of titanium alloy materials and in the preparation of titanium alloys, different grades of titanium alloys are produced due to different performance requirements. The formation of different titanium alloy grades depends on the alloy as an added element called the master alloy. Master alloys are an important additive in the titanium alloy smelting industry and are known as the "vitamin of titanium alloys." The preparation of titanium alloy ingots is made by smelting sponge titanium and master alloys together. Therefore, the quality and stability of the master alloy directly affect the quality of titanium alloy ingots.
[0003] At present, the preparation of a certain grade of titanium alloy ingots often requires the addition of multiple different types of intermediate alloys or elements to meet the requirements of the element grade. The role of the intermediate alloy is to make the melting point and density of the added alloy close to that of the titanium matrix when smelting alloy components with very different melting points. At present, in the titanium alloy smelting industry, iron elements are mostly added directly in the form of iron nails or other pure elements. Because their density and melting point are quite different from those of the titanium matrix, the smelted titanium alloys often have the problem of iron segregation. The titanium-iron alloys used by a very small number of titanium alloy ingot manufacturers are prone to iron enrichment problems, so the quality and stability of titanium alloy ingots are difficult to guarantee.
[0004] The present invention aims at the problems of segregation occurring in the process of adding iron element in titanium alloy smelting and high burning loss rate and difficulty in smelting in the process of adding aluminum element, and provides an intermediate alloy meeting the smelting requirements. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a preparation process of aluminum-iron alloy specially used for aerospace-grade titanium alloy.
[0006] The technical solution adopted by the present invention is: a preparation process of aluminum-iron alloy for aerospace grade titanium alloy, comprising the following steps: Step 1: Prepare the ingredients Small particles of high-purity aluminum and high-purity iron are used as raw materials, and the purity of high-purity aluminum and high-purity iron is greater than 99%; Step 2: Mixing High-purity aluminum and high-purity iron particles are mixed evenly according to the element ratio of Al:Fe=40-45:55-60 to form an aluminum-iron mixture; Step 3: Pressing The aluminum-iron mixture is placed in a hydraulic press mold to press out a raw material block with a diameter of φ260 mm×320 mm; Step 4: Melting The raw materials are put into a medium frequency induction furnace, and the process parameters of the medium frequency furnace smelting process are: vacuum degree ≥15Pa, smelting power: 50kw-80kw, smelting temperature: 1550℃-1700℃, refining time: 8-10min, cooling time ≥1h, the temperature is below 400℃ and taken out of the furnace to form aluminum iron ingots, and the surface interlayer is removed by sandblasting; Step 5: Qualified entry into the warehouse The finished aluminum-iron ingots are then crushed and screened to obtain aluminum-iron alloy for aerospace-grade titanium alloy.
[0007] The aluminum-iron alloy prepared by the invention changes the melting point and density of a single component, and finally forms an AlFe60 complex.
[0008] The particle size of the small-particle high-purity aluminum is 3×3 mm, and such a particle size reduces the burning loss of aluminum.
[0009] The high-purity iron is carbonyl iron powder with a particle size of 10 microns. The carbonyl iron powder has a smaller specific surface area and lower thermal stability, thereby overcoming the segregation of iron elements in the smelting of aluminum-iron alloy.
[0010] Step 4: Aluminum-iron alloy is generated during the smelting process.
[0011] The crushing in step 4 includes air hammer, coarse crushing and fine crushing, and the screening includes 0.25mm or less, 0.25-6.2mm, and 6.2mm or more. Such a particle size is for the convenience of smelting. The smelting requires a particle size of 0.25-6.2mm in order to match the materials of general titanium master alloys. The particle size of 0.25-6.2mm can be fully mixed with other master alloys for smelting.
[0012] High-purity aluminum and high-purity iron particles are evenly mixed into an aluminum-iron mixture according to the element ratio of Al:Fe=40-45:55-60, so that the aluminum-iron alloy after smelting can meet the design component requirements and make the later titanium alloy finished product have higher component uniformity, thereby overcoming the segregation caused by the iron element addition process in the titanium alloy smelting in the prior art; Since Al has a low melting point and is partially ablated, the AlFe60 complex finally obtained by the present invention ensures that the Fe content is between 55-60, with Al as the remainder; when the Fe content of the AlFe60 complex is 60, the best state and the best technical effect are achieved.
[0013] Since the melting point of aluminum itself is 660°C and the melting point of iron itself is 1538°C, the aluminum-iron alloy of the present invention, as an intermediate alloy, has a melting point of 1300°C-1400°C, which lowers the melting point of iron in the preparation of titanium alloy ingots, making it easier to melt into titanium liquid; the melting point of aluminum is increased, and the burnout rate of aluminum element is reduced; the burnout rate can be reduced by 1-2%.
[0014] During the preparation process, the invention simultaneously completes the addition of aluminum and iron; the aluminum-iron alloy can make the addition of aluminum and iron elements in the titanium alloy smelting process simpler and improve the composition uniformity of the titanium alloy material. DETAILED DESCRIPTION
[0015] The following examples illustrate the implementation and features of the present invention, but the present invention is not limited to the following embodiments.
[0016] Embodiment 1:
[0017] A preparation process of aluminum-iron alloy for aerospace grade titanium alloy, comprising the following steps: Step 1: Prepare the ingredients Small particles of high-purity aluminum and carbonyl iron powder are used as raw materials, wherein the purity of high-purity aluminum and carbonyl iron is greater than 99%; the particle size of high-purity aluminum is 3×3mm; the particle size of carbonyl iron powder is 10 microns; Step 2: Mixing The high purity aluminum and carbonyl iron particles are uniformly mixed in an element ratio of Al:Fe=40:60 to form an aluminum-iron mixture; Step 3: Pressing The aluminum-iron mixture is placed in a hydraulic press mold to press out a raw material block with a diameter of φ260 mm×320 mm; Step 4: Melting The raw materials are put into a medium frequency induction furnace, and the process parameters of the medium frequency furnace smelting process are: vacuum degree ≥15Pa, smelting power: 50kw-80kw, smelting temperature: 1550℃-1700℃, refining time: 8-10min, cooling time ≥1h, the temperature is below 400℃ and taken out of the furnace to form aluminum iron ingots, and the surface interlayer is removed by sandblasting; Step 5: Qualified entry into the warehouse The finished aluminum-iron ingots are then crushed and screened to obtain aluminum-iron alloy for aerospace-grade titanium alloy.
[0018] The AlFe60 composite obtained in this embodiment has an iron content of 61% and aluminum as the balance; the aluminum-iron alloy is used as an intermediate alloy with a melting point of 1350°C.
[0019] Embodiment 2:
[0020] A preparation process of aluminum-iron alloy for aerospace grade titanium alloy, comprising the following steps: Step 1: Prepare the ingredients Small particles of high-purity aluminum and carbonyl iron powder are used as raw materials, wherein the purity of high-purity aluminum and carbonyl iron is greater than 99%; the particle size of high-purity aluminum is 3×3mm; the particle size of carbonyl iron powder is 10 microns; Step 2: Mixing High-purity aluminum and carbonyl iron particles are uniformly mixed in an element ratio of Al:Fe=43:57 to form an aluminum-iron mixture; Step 3: Pressing The aluminum-iron mixture is placed in a hydraulic press mold to press out a raw material block with a diameter of φ260 mm×320 mm; Step 4: Melting The raw materials are put into a medium frequency induction furnace, and the process parameters of the medium frequency furnace smelting process are: vacuum degree ≥15Pa, smelting power: 50kw-80kw, smelting temperature: 1550℃-1700℃, refining time: 8-10min, cooling time ≥1h, the temperature is below 400℃ and taken out of the furnace to form aluminum iron ingots, and the surface interlayer is removed by sandblasting; Step 5: Qualified entry into the warehouse The finished aluminum-iron ingots are then crushed and screened to obtain aluminum-iron alloy for aerospace-grade titanium alloy.
[0021] The AlFe60 composite obtained in this embodiment has an iron content of 60% and aluminum as the balance; the aluminum-iron alloy is used as an intermediate alloy with a melting point of 1300° C., reaching the optimal state.
[0022] Embodiment 3:
[0023] A preparation process of aluminum-iron alloy for aerospace grade titanium alloy, comprising the following steps: Step 1: Prepare the ingredients Small particles of high-purity aluminum and carbonyl iron powder are used as raw materials, wherein the purity of high-purity aluminum and carbonyl iron is greater than 99%; the particle size of high-purity aluminum is 3×3mm; the particle size of carbonyl iron powder is 10 microns; Step 2: Mixing High purity aluminum and carbonyl iron particles are mixed evenly in an element ratio of Al:Fe=45:55 to form an aluminum-iron mixture; Step 3: Pressing The aluminum-iron mixture is placed in a hydraulic press mold to press out a raw material block with a diameter of φ260 mm×320 mm; Step 4: Melting The raw materials are put into a medium frequency induction furnace, and the process parameters of the medium frequency furnace smelting process are: vacuum degree ≥15Pa, smelting power: 50kw-80kw, smelting temperature: 1550℃-1700℃, refining time: 8-10min, cooling time ≥1h, the temperature is below 400℃ and taken out of the furnace to form aluminum iron ingots, and the surface interlayer is removed by sandblasting; Step 5: Qualified entry into the warehouse The finished aluminum-iron ingots are then crushed and screened to obtain aluminum-iron alloy for aerospace-grade titanium alloy.
[0024] The AlFe60 composite obtained in this embodiment has an iron content of 59% and aluminum as the balance; the aluminum-iron alloy is used as an intermediate alloy with a melting point of 1400°C.
Claims
1. A process for preparing aluminum-iron alloy for aerospace grade titanium alloy, characterized in that: The following steps are involved: Step 1: Prepare the ingredients Small particles of high-purity aluminum and high-purity iron are used as raw materials, and the purity of high-purity aluminum and high-purity iron is greater than 99%; Step 2: Mixing High-purity aluminum and high-purity iron particles are mixed evenly according to the element ratio of Al:Fe=40-45:55-60 to form an aluminum-iron mixture; Step 3: Pressing The aluminum-iron mixture is placed in a hydraulic press mold to press out a raw material block with a diameter of φ260 mm×320 mm; Step 4: Melting The raw materials are put into a medium frequency induction furnace, and the process parameters of the medium frequency furnace smelting process are: vacuum degree ≥15Pa, smelting power: 50kw-80kw, smelting temperature: 1550℃-1700℃, refining time: 8-10min, cooling time ≥1h, the temperature is below 400℃ and taken out of the furnace to form aluminum iron ingots, and the surface interlayer is removed by sandblasting; Step 5: Qualified entry into the warehouse The finished aluminum-iron ingots are then crushed and screened to obtain aluminum-iron alloy for aerospace-grade titanium alloy.
2. The process for preparing an aluminum-iron alloy for aerospace-grade titanium alloy according to claim 1, characterized in that: The particle size of the small particles of high-purity aluminum in step 1 is 3×3 mm.
3. The process for preparing an aluminum-iron alloy for aerospace-grade titanium alloy according to claim 1, characterized in that: High purity iron is carbonyl iron powder.
4. The process for preparing an aluminum-iron alloy for aerospace-grade titanium alloy according to claim 1, characterized in that: The crushing described in step 4 includes air hammer, coarse crushing and fine crushing, and the screening includes below 0.25mm, 0.25-6.2mm, and above 6.2mm.
5. The process for preparing an aluminum-iron alloy for aerospace-grade titanium alloy according to claim 1, characterized in that: The element ratio of high-purity aluminum to high-purity iron particles in step 2 is Al:Fe=43:57, which is optimal.
6. The process for preparing an aluminum-iron alloy for aerospace-grade titanium alloy according to claim 1, characterized in that: The prepared aluminum-iron alloy forms an AlFe60 complex.
7. The process for preparing an aluminum-iron alloy for aerospace-grade titanium alloy according to claim 6, characterized in that: The optimum content of AlFe60 complex is 60%.
8. The process for preparing an aluminum-iron alloy for aerospace-grade titanium alloy according to claim 7, characterized in that: The melting point of AlFe60 complex is 1300℃-1400℃.