Rust conversion agent for water-based acrylic resin coating in mine and water-based acrylic resin coating

By using a combination of rust-reversing agents of phosphoric acid, gallic acid and phytic acid and graphene-modified hydroxyacrylic resin coatings in mines, the adhesion and anti-corrosion problems of traditional coatings in high-humidity environments have been solved, and efficient steel materials have been achieved. Protect and expand the scope of application.

CN118835232APending Publication Date: 2024-10-25SHAANXI COAL & CHEM TECH INST

Patent Information

Application Number
CN202410887287.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

In mines, the adhesion and anti-corrosion protection of traditional coatings are insufficient, and problems such as oil, water and rust seriously affect the coating quality, leading to peeling off of the coating and failure of protection. The existing rust-converting agents are difficult to react effectively in high-humidity environments. And the addition amount requires high accuracy, which affects the scope of application.

Method used

Using a rust-removing agent mixed with phosphoric acid, gallic acid and phytic acid in a certain proportion, the phosphoric acid converts deep rust into iron ions, and reacts with gallic acid to form a chelate, blocking the passage of oxygen and water molecules, combined with graphene-modified hydroxyl groups Components such as acrylic resin and zinc powder improve the penetration and corrosion resistance of the paint.

Benefits of technology

It achieves effective protection of steel materials in high-humidity environments, improves the reaction bonding strength and durability of the rust-converting agent, reduces the accuracy requirements for the addition amount, expands the scope of application, and enhances the anti-static and anti-corrosion capabilities of the coating. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004926393600000141
    Figure BDA0004926393600000141
  • Figure BDA0004926393600000151
    Figure BDA0004926393600000151
Patent Text Reader

Abstract

The invention discloses a rust conversion agent for a water-based acrylic resin coating in a mine and the water-based acrylic resin coating, and belongs to the technical field of rust treatment. Gallic acid; phytic acid; the mass ratio of the phosphoric acid to the gallic acid to the phytic acid is 1: (0.5-1.5): (3-5). By designing the rust conversion agent, the requirement for reacting rust of rusted steel and iron materials in a mine can be met, the application range of the coating is widened, meanwhile, too large or too small adding amount of the rust conversion agent has little influence on the corrosion resisting effect, the precision requirement for the adding amount of the rust conversion agent is lowered, and the application range is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rust treatment, and in particular relates to a rust-removing agent for water-based acrylic resin coating in mines and a water-based acrylic resin coating. Background Art

[0002] In chemical plants, power plants, food factories, mines and other environments, the corrosion problem of steel is particularly serious, which brings great challenges to surface treatment. Although traditional coatings are widely used, their effects are not ideal. Traditional topcoats and primers are insufficient in adhesion and anti-corrosion protection, and problems such as oil, water and rust seriously affect the quality of coating, and ultimately lead to coating film shedding and protection failure.

[0003] In view of the above problems, the prior art adds a rust-reducing agent to the coating, and the rust-reducing agent reacts with the rust to convert the rust into an inert substance, which not only seals the rust but also isolates it from the outside world, thereby eliminating the need for high-intensity treatment of the rust and reducing the burden on operators. For example, the Chinese invention patent with the announcement number CN114672795B discloses a water-based rust-reducing agent, including tea polyphenols and gallic acid, wherein the mass ratio of the tea polyphenols to the gallic acid is 2-7:4-10, and the water-based rust-reducing agent also includes a conversion aid, which includes at least one of sodium tripolyphosphate, sodium aminomethylenephosphonate or triethanolamine phosphate. However, this technology cannot be applied in mines. The humidity in mines is relatively high, generally above 80%, and the cold inner walls of the mines and steel supports cause the moist airflow to condense on the inner walls of the mines or on the steel supports, resulting in a high moisture content in the rust. It is necessary to ensure that after the rust remover reacts with the rust, the moisture is discharged before an inert substance is formed; secondly, the rust remover needs to have strong penetrability to solidify the deep rust as much as possible. Summary of the invention

[0004] In order to solve the above problems, the purpose of the present invention is to provide a rust-removing agent and a water-based acrylic resin coating for use in mines. The rust-removing agent can react with the rust of corroded steel materials in mines. At the same time, the addition of too much or too little rust-removing agent has little effect on the anti-corrosion effect, thereby reducing the precision requirement on the addition amount of the rust-removing agent, improving the scope of application, and the coating based on the rust-removing agent has a wide scope of application.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] A rust-removing agent for water-based acrylic resin coating in mines, comprising:

[0007] Phosphoric acid;

[0008] gallic acid;

[0009] Phytic acid;

[0010] The mass ratio of the phosphoric acid, gallic acid and phytic acid is 1:0.5-1.5:3-5.

[0011] Furthermore, the mass ratio of the phosphoric acid, gallic acid and phytic acid is 1:1:4.

[0012] A water-based acrylic resin coating comprises the following components in parts by weight:

[0013] 40-50 parts of graphene-modified hydroxy acrylic resin;

[0014] 5-7 parts of the rust-removing agent according to claim 1 or 2;

[0015] 20-30 parts of rust inhibitor;

[0016] Curing agent, add curing agent according to the NCO / OH molar ratio of 1.2 to 1.6:1;

[0017] 20-30 parts of filler.

[0018] Furthermore, the preparation method of the graphene-modified hydroxy acrylic resin comprises:

[0019] Under the action of an initiator, the copolymer monomer and the modified graphene are polymerized in an organic solvent to obtain an intermediate solution;

[0020] The intermediate liquid is neutralized, mixed with water, and stirred to obtain the graphene-modified hydroxy acrylic resin.

[0021] Furthermore, the amount of the modified graphene added is 1 to 3 parts;

[0022] The comonomers include, by weight:

[0023] 20-30 parts of methyl methacrylate;

[0024] 5-10 parts of butyl methacrylate;

[0025] 10-20 parts of acrylic acid;

[0026] 15-30 parts of hydroxypropyl acrylate;

[0027] 20-25 parts of isobornyl methacrylate;

[0028] 3 to 8 parts of crotonic acid.

[0029] Furthermore, the preparation process of the modified graphene includes:

[0030] Reduced graphene oxide and dopamine are added in a mass ratio of 1:0.5-0.8, stirred at 120°C and a rotation speed of 200-300 rpm for 5-10 minutes, and then dried.

[0031] Furthermore, the reduced graphene oxide includes a single-layer reduced graphene oxide and a few-layer reduced graphene oxide, and the mass ratio of the single-layer reduced graphene oxide to the few-layer reduced graphene oxide is 1:0.6-0.8.

[0032] Furthermore, the rust inhibitor is zinc powder, the average particle size of the zinc powder is 3-4 μm, and the sphericity of the zinc powder is not less than 0.6.

[0033] Furthermore, the curing agent is aromatic isocyanate.

[0034] Furthermore, it also includes:

[0035] The additive comprises at least one of a leveling agent, a dispersant, a defoaming agent or a thickener.

[0036] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0037] The invention mixes phosphoric acid, gallic acid and phytic acid in a certain proportion, wherein the rust on the surface of the substrate reacts with a relatively large amount of phytic acid to generate an inert and insoluble mixture, and the deep rust is converted into iron ions by the action of phosphoric acid, and the iron ions react with gallic acid with strong permeability to generate a chelate, thereby overcoming the problem in the prior art that the deep rust provides a channel for oxygen and water, resulting in low bonding strength between the inert substance generated by the reaction of the rust and the rust-converting agent and the substrate, and poor durability.

[0038] In the coating of the present invention, a rust-removing agent is prepared by mixing phosphoric acid, gallic acid and phytic acid in a certain proportion. Phosphoric acid has the highest water solubility, gallic acid is slightly soluble, and phytic acid has a certain solubility. When the amount of the rust-removing agent added is relatively small, the phytic acid with higher solubility reacts with the surface layer of rust to generate an inert chelate, which can block the passage of oxygen and water molecules. When the amount of the rust-removing agent added is relatively large, the chelate generated by the iron ions converted by phosphoric acid and the gallic acid mainly blocks the passage of oxygen and water molecules. Even if there are pores between the chelate generated by the surface layer of phytic acid and the rust, it will not affect the rust-removing agent and the rust to generate inert substances, which blocks the passage of oxygen and water molecules and the iron matrix. The problem that some components of the rust-removing agent in the prior art are easily soluble in water, if the amount added is too large, the excess components are hydrolyzed to generate a path for oxygen or water to flow, so that the protective ability of the coating for the substrate is weakened; and if the amount added is small, it cannot react with all the rust, and the rust removal ability is relatively weak. DETAILED DESCRIPTION

[0039] The present invention is further described in detail below by specific embodiments. However, it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If specific techniques or conditions are not specified in the examples, they are carried out according to the techniques or conditions described in the literature in this area or according to the product instructions. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0040] As used herein, the words "comprises," "including," "having," or any other variations thereof, are intended to cover a non-exclusive inclusion. For example, a process, method, article, or apparatus that includes listed elements is not necessarily limited to those elements but may include other elements not expressly listed or inherent to such process, method, article, or apparatus. The singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.

[0041] The invention provides a rust-removing agent for water-based acrylic resin coating in mines, comprising phosphoric acid, gallic acid and phytic acid; the mass ratio of the phosphoric acid, gallic acid and phytic acid is 1:0.5-1.5:3-5.

[0042] The present invention prepares the rust-removing agent by uniformly mixing phosphoric acid, gallic acid and phytic acid in a certain proportion. When the chelate completely covers the steel material matrix, a certain gap is left between gallic acid and phytic acid molecules to discharge water and gas, thereby preventing the residual liquid and oxygen from continuing to oxidize the iron matrix to generate iron oxide, thereby reducing the bonding strength between the complex generated by the reaction and the matrix. Secondly, when the water and gas are completely discharged, the gallic acid and phytic acid molecules are hydrogen-bonded to block the gaps, thereby preventing external water and gas from entering the matrix. Especially for the use environment in mines, the matrix can be completely coated in a high-humidity state to avoid secondary oxidation, and the composition of the rust-removing agent takes into account the technical requirements of subsequent coatings meeting antistatic requirements, that is, the surface resistance of the coating is less than 1×10 6 Ω.m.

[0043] As an inorganic acid, phosphoric acid is stronger than gallic acid and weaker than phytic acid. Phosphoric acid has strong permeability and can convert deep rust into iron ions so that the iron ions can undergo chelation reaction with gallic acid and phytic acid to generate inert substances. However, due to its strong acidity, it is easy to corrode the matrix. Gallic acid is an organic acid with a relative molecular mass between phosphoric acid and phytic acid. Its acidity is weaker than those of phosphoric acid and phytic acid and has certain permeability. Phytic acid has a larger relative molecular weight and stronger acidity. Its hydroxyl group is a chelating group, which can chelate with iron ions to generate inert phytic acid iron complex salts, which adhere to the metal surface and can effectively inhibit corrosion. The present invention mixes the above three acids in a certain proportion, wherein the rust on the surface of the substrate reacts with a relatively large amount of phytic acid to generate an inert and insoluble mixture, and the deep rust is converted into iron ions through the action of phosphoric acid, and the iron ions react with gallic acid with strong permeability to generate a chelate. In the prior art, the deep rust provides a channel for oxygen and water, resulting in a low bonding strength between the inert substance generated by the reaction of the rust and the rust-removing agent and the substrate, and poor durability. Secondly, in the prior art, due to the different oxidation degrees of the substrate, the thickness of the rust varies, resulting in a specific amount of rust-removing agent being difficult to react exactly with the generated rust, and thus the rust-removing agent has the problem of being added in too much or too little amount, and a large amount of addition will cause certain corrosion to the substrate, and some components in the rust-removing agent are easily soluble in water. If the amount added is too large, the excess components will be hydrolyzed. A path for oxygen or water to flow is generated, which weakens the protective ability of the coating for the substrate; and if the amount added is small, it cannot react with all the rust, and the rust removal ability is weak. The present invention, taking the above situation into consideration, proposes a scheme of mixing phosphoric acid, gallic acid and phytic acid in a certain proportion. In this scheme, phosphoric acid has the highest water solubility, gallic acid is slightly soluble, and phytic acid has a certain solubility. When the amount of rust remover added is small, the phytic acid with higher solubility reacts with the surface of rust to form an inert chelate, which can block the passage of oxygen and water molecules. When the amount of rust remover added is large, the chelate generated by the iron ions converted from phosphoric acid and the gallic acid mainly blocks the passage of oxygen and water molecules. Even if there are pores between the chelate generated by the surface phytic acid and the rust, it will not affect the rust remover and the rust to generate inert substances, blocking the passage of oxygen and water molecules to the iron matrix.

[0044] The reaction of phosphoric acid, gallic acid and phytic acid with iron ions is common knowledge, and phosphoric acid, gallic acid and phytic acid can be analytically pure or chemically pure. Unless otherwise specified in the present invention, phosphoric acid, gallic acid and phytic acid are commercially available.

[0045] Preferably, the mass ratio of the phosphoric acid, gallic acid and phytic acid is 1:1:4.

[0046] It should be noted that a certain amount of deionized water can be added to the rust remover provided by the present invention so that it can be used alone. The amount of deionized water added is 10-20 times the total mass of phosphoric acid, gallic acid and phytic acid. When used in combination with a coating, it can be directly added to the coating.

[0047] On the other hand, the present invention provides a water-based acrylic resin coating, comprising the following components in parts by weight: 40 to 50 parts of graphene-modified hydroxy acrylic resin; 5 to 7 parts of the above-mentioned rust-removing agent; 20 to 30 parts of rust inhibitor; a curing agent, the curing agent being added according to an NCO / OH molar ratio of 1.2 to 1.6:1; and 20 to 30 parts of filler.

[0048] The above components in parts by weight are mixed and stirred for at least 20 minutes before use.

[0049] The water-based acrylic resin coating provided by the present invention can be applied in mines to provide reliable protection for steel. In addition to water vapor, mines also contain corrosive gases such as hydrogen sulfide (H2S), sulfur dioxide (SO2), nitrogen dioxide (NO2), and ammonia (NH3). These substances have high corrosiveness and accelerate the aging of the coating. The present invention adopts water-based acrylic resin coating. During the drying and curing process of the water-based acrylic resin coating, water evaporates and certain small-sized pores will exist. How to block the pores is particularly important. The technical solution of the present invention adopts graphene-modified hydroxy acrylic resin and performs special treatment on the structure of graphene. On the one hand, the problem of uneven distribution of graphene is solved, and the treated graphene has strong resistance to the above-mentioned corrosive gases; on the other hand, the graphene is combined with a rust inhibitor to form a primary battery, which increases the corrosion resistance of the coating.

[0050] It should be pointed out that the curing agent in the present invention is isocyanate, which can be aromatic, aliphatic or alicyclic. In order to achieve a better reaction effect, the aromatic curing agent, toluene diisocyanate (TDI), is used so that the prepared paint film has higher hardness and chemical resistance.

[0051] The filler is calcium carbonate, talcum powder, titanium dioxide or silicon dioxide, and preferably nano-scale filler powder is used.

[0052] The preparation method of the graphene-modified hydroxy acrylic resin comprises:

[0053] S1. Under the action of an initiator, the copolymer monomer and the modified graphene are polymerized in an organic solvent to obtain an intermediate solution.

[0054] In the embodiment of the present invention, the organic solvent is propylene glycol butyl ether and ethylene glycol butyl ether, wherein the mass ratio of propylene glycol butyl ether to ethylene glycol butyl ether is 1.8-2.2:1, and the sum of the masses of the propylene glycol butyl ether and the ethylene glycol butyl ether is 7-8wt% of the total mass of the intermediate liquid; the initiator is an azo compound or a peroxide compound. The present invention prepares a water-based acrylic resin coating, selects tert-butyl perbenzoate as an initiator, and the addition amount is 3.1-3.8wt% of the total mass of the graphene-modified hydroxy acrylic resin, wherein the half-life of tert-butyl perbenzoate is 2h (120°C), and a one-time addition method is adopted.

[0055] The modified graphene is added in an amount of 1 to 3 parts; the comonomers are calculated by weight and include: 20 to 30 parts of methyl methacrylate; 5 to 10 parts of butyl methacrylate; 10 to 20 parts of acrylic acid; 15 to 30 parts of hydroxypropyl acrylate; 20 to 25 parts of isobornyl methacrylate; and 3 to 8 parts of crotonic acid. The preparation process of the comonomer is: uniformly mix the components by weight.

[0056] The preparation process of the modified graphene includes:

[0057] Add reduced graphene oxide and dopamine to the container at a mass ratio of 1:0.5-0.8, stir at 120°C, 200-300rpm for 5-10min, and then dry. Preferably, the oxygen content of the reduced graphene oxide is 6-10at%. It should be pointed out that the value of the oxygen content indicates the number of sites that can react with dopamine. If there are many reaction sites, the interaction between the reduced graphene oxide and the hydroxy acrylic resin will be greater, and the resistance value itself will increase; secondly, it is difficult to overlap the subsequent reduced graphene oxide, which increases the coating resistance and weakens the ability to prevent harmful gases and moisture. More importantly, the rust inhibitor cannot be effectively connected to form a primary battery to protect the substrate. If there are few reaction sites, the interaction between the prepared graphene and the hydroxy acrylic resin is small, and the graphene is easy to agglomerate, resulting in poor overall effect. In addition, the graphene overlap in the present invention improves the overall strength and impact resistance.

[0058] Furthermore, the reduced graphene oxide includes a single-layer reduced graphene oxide and / or a few-layer reduced graphene oxide, and the mass ratio of the single-layer reduced graphene oxide to the few-layer reduced graphene oxide is 1:0.6-0.8.

[0059] The present invention increases the probability of overlapping between the single layer and the few layers of reduced graphene oxide by arranging a single layer and a few layers of reduced graphene oxide, which, on the one hand, improves the connection effect with the rust inhibitor particles and has a good primary cell protection effect; on the other hand, it can effectively block the micropores of the water-based acrylic resin coating after drying.

[0060] The comonomer and the modified graphene are polymerized in an organic solvent to obtain an intermediate solution. Specifically, an organic solvent is added to a reaction vessel, and then the corresponding mass parts of the comonomer, initiator and modified graphene (1 / 3 of the total mass of the modified graphene) are weighed into the reaction vessel, stirred evenly, and nitrogen is added to the system. When the temperature rises to 120°C, it is kept warm for 30-60 minutes, and then the remaining modified graphene (2 / 3 of the total mass of the modified graphene) is added. After keeping warm for 30-50 minutes, the system temperature is lowered to 50°C to obtain the intermediate solution. The use of this process mainly takes into account the polymer nucleation process and growth process. Adding an appropriate amount of modified graphene during the nucleation process can ensure that there is a certain amount of modified graphene inside the core, and the modified graphene added later can make the surface of the formed polymer evenly attached with modified graphene, thereby improving the effectiveness of the primary cell and the corrosion resistance of the steel matrix.

[0061] S2. neutralizing the intermediate liquid, mixing it with water, and stirring it to obtain graphene-modified hydroxy acrylic resin.

[0062] The present invention uses N,N-dimethylethanolamine as a neutralizer with a neutralization degree of 91-93%. When the mass fraction of the modified graphene is 1-3 parts, the mass fraction of the added water is 80-140 parts. The stirring speed is 200-300 rpm, and the stirring time is at least 5 minutes.

[0063] The rust inhibitor is zinc powder, the average particle size of the zinc powder is 3-4 μm, and the sphericity of the zinc powder is not less than 0.6. In the prior art, flaky zinc powder is used, but there are some problems with the use of flaky zinc powder, that is, the water-based acrylic resin coating generates certain stress during the drying process, and due to its weak bonding strength with the flaky zinc powder, more microporous structures will appear, and the appearance of micropores will aggravate the entry of corrosive gases and water molecules into the protected substrate to cause corrosion. Based on the above considerations, the present invention uses quasi-spherical zinc powder to alleviate the above problems, and the present invention uses reduced graphene oxide to replace part of the zinc powder to form a steric effect. On the other hand, the present invention proposes the use of a few layers and a single layer of reduced graphene oxide, and combines with zinc powder to form an effectively connected primary battery to protect the substrate.

[0064] The water-based acrylic resin coating further comprises: an additive, wherein the additive comprises at least one of a leveling agent, a dispersant, a defoamer or a thickener. It should be noted that the above-mentioned additive can be commercially available without any special restrictions, and the additive amount can be 0.2-1.0wt% of the total mass of the water-based acrylic resin coating.

[0065] Example 1

[0066] The present embodiment provides a water-based acrylic resin coating, comprising the following components in parts by weight: 40 parts of graphene-modified hydroxy acrylic resin; 5 parts of rust remover; 20 parts of zinc powder; toluene diisocyanate, added at an NCO / OH molar ratio of 1.2:1; and 20 parts of silicon dioxide. The above components in parts by weight are mixed and stirred for 20 minutes before use.

[0067] The preparation method of the graphene-modified acrylic resin is:

[0068] S1. Under the action of tert-butyl perbenzoate, 20 parts of methyl methacrylate, 5 parts of butyl methacrylate, 10 parts of acrylic acid, 15 parts of hydroxypropyl acrylate, 20 parts of isobornyl methacrylate, 3 parts of crotonic acid and 1 part of modified graphene are polymerized in an organic solvent at 120°C for 30 minutes to obtain an intermediate solution.

[0069] The organic solvent is a mixture of propylene glycol butyl ether and ethylene glycol butyl ether in a mass ratio of 1.8:1, wherein the mass of the organic solvent is 7wt% of the total mass of the intermediate liquid;

[0070] The preparation process of the modified graphene includes:

[0071] Reduced graphene oxide and dopamine are stirred at 120° C. and 200 rpm for 5 minutes in a mass ratio of 1:0.5. The reduced graphene oxide includes a single-layer reduced graphene oxide and a few-layer reduced graphene oxide. The mass ratio of the single-layer reduced graphene oxide to the few-layer reduced graphene oxide is 1:0.6.

[0072] S2. neutralizing the intermediate liquid, mixing it with water, and stirring it to obtain graphene-modified hydroxy acrylic resin.

[0073] N,N-dimethylethanolamine is used as a neutralizing agent with a neutralization degree of 91%. The mass fraction of water added is 80 parts. The stirring speed is 200 rpm and the stirring time is 5 minutes.

[0074] The preparation method of the rust-removing agent is:

[0075] Add phosphoric acid, gallic acid and phytic acid into a container, wherein the mass ratio of the phosphoric acid, gallic acid and phytic acid is 1:0.5:3, and stir for 5 minutes.

[0076] Example 2

[0077] The present embodiment provides a water-based acrylic resin coating, comprising the following components in parts by weight: 45 parts of graphene-modified hydroxyl acrylic resin; 6 parts of rust remover; 25 parts of zinc powder; toluene diisocyanate, added at an NCO / OH molar ratio of 1.4:1; and 25 parts of silicon dioxide. The above components in parts by weight are mixed and stirred for 30 minutes before use.

[0078] The preparation method of the graphene-modified acrylic resin is:

[0079] S1. Under the action of tert-butyl perbenzoate, 25 parts of methyl methacrylate, 8 parts of butyl methacrylate, 15 parts of acrylic acid, 23 parts of hydroxypropyl acrylate, 22 parts of isobornyl methacrylate, 5 parts of crotonic acid and 2 parts of modified graphene are added to an organic solvent, and a polymerization reaction is carried out at 120°C for 30 minutes to obtain an intermediate solution.

[0080] The organic solvent is a mixture of propylene glycol butyl ether and ethylene glycol butyl ether in a mass ratio of 1.8:1, wherein the mass of the organic solvent is 7wt% of the total mass of the intermediate liquid;

[0081] The preparation process of the modified graphene includes:

[0082] Reduced graphene oxide and dopamine were stirred at 120° C. and 300 rpm for 8 min in a mass ratio of 1:0.7, and the mass ratio of the monolayer reduced graphene oxide to the few-layer reduced graphene oxide was 1:0.7.

[0083] S2. neutralizing the intermediate liquid, mixing it with water, and stirring it to obtain graphene-modified hydroxy acrylic resin.

[0084] N,N-dimethylethanolamine is used as a neutralizing agent with a neutralization degree of 92%. The mass fraction of water added is 100 parts. The stirring speed is 300 rpm and the stirring time is 5 minutes.

[0085] The preparation method of the rust-removing agent is:

[0086] Add phosphoric acid, gallic acid and phytic acid into a container, wherein the mass ratio of the phosphoric acid, gallic acid and phytic acid is 1:1:3, and stir for 5 minutes.

[0087] Example 3

[0088] The present embodiment provides a water-based acrylic resin coating, comprising the following components in parts by weight: 50 parts of graphene-modified hydroxyl acrylic resin; 7 parts of rust remover; 30 parts of zinc powder; toluene diisocyanate, added at an NCO / OH molar ratio of 1.6:1; and 30 parts of silicon dioxide. The above components in parts by weight are mixed and stirred for 20 minutes before use.

[0089] The preparation method of the graphene-modified acrylic resin is:

[0090] S1. Under the action of tert-butyl perbenzoate, 30 parts of methyl methacrylate, 10 parts of butyl methacrylate, 20 parts of acrylic acid, 30 parts of hydroxypropyl acrylate, 25 parts of isobornyl methacrylate, 8 parts of crotonic acid and 3 parts of modified graphene are added in an organic solvent and polymerized at 120°C for 30 minutes to obtain an intermediate solution.

[0091] The organic solvent is a mixture of propylene glycol butyl ether and ethylene glycol butyl ether in a mass ratio of 1.8:1, wherein the mass of the organic solvent is 7wt% of the total mass of the intermediate liquid;

[0092] The preparation process of the modified graphene includes:

[0093] Reduced graphene oxide and dopamine were stirred at 120° C. and 300 rpm for 10 min in a mass ratio of 1:0.8, and the mass ratio of the monolayer reduced graphene oxide to the few-layer reduced graphene oxide was 1:0.8.

[0094] S2. neutralizing the intermediate liquid, mixing it with water, and stirring it to obtain graphene-modified hydroxy acrylic resin.

[0095] N,N-dimethylethanolamine is used as a neutralizing agent with a neutralization degree of 93%. The mass fraction of water added is 140 parts. The stirring speed is 300 rpm and the stirring time is 5 minutes.

[0096] The preparation method of the rust-removing agent is:

[0097] Add phosphoric acid, gallic acid and phytic acid into a container, wherein the mass ratio of the phosphoric acid, gallic acid and phytic acid is 1:1.5:5, and stir for 5 minutes.

[0098] Example 4

[0099] Different from Example 1, in this embodiment, the preparation process of the modified graphene includes:

[0100] Reduced graphene oxide and dopamine were stirred at a mass ratio of 1:0.5 at 120° C. and a rotation speed of 200 rpm for 5 min, and all the reduced graphene oxide was a single-layer reduced graphene oxide. Other raw materials and steps were the same as those in Comparative Example 1 and will not be repeated here.

[0101] Example 5

[0102] Different from Example 1, in this embodiment, the preparation process of the modified graphene includes:

[0103] Reduced graphene oxide and dopamine were added in a mass ratio of 1:0.5, stirred at 120°C and a rotation speed of 200 for 5 minutes, and the reduced graphene oxide was all reduced graphene oxide with few layers. Other raw materials and steps were the same as those in Comparative Example 1, and will not be repeated here.

[0104] Example 6

[0105] Different from Example 1, in this example, the preparation method of the rust-removing agent is as follows: phosphoric acid, gallic acid and phytic acid are added into a container, wherein the mass ratio of phosphoric acid, gallic acid and phytic acid is 1:1:4, and stirred for 5 minutes. Other raw materials and steps are the same as those in Comparative Example 1, and will not be repeated here.

[0106] Example 7

[0107] Different from Example 1, in this embodiment, the reduced graphene oxide includes a single-layer reduced graphene oxide and a few-layer reduced graphene oxide, and the mass ratio of the single-layer reduced graphene oxide to the few-layer reduced graphene oxide is 1:0.5. Other raw materials and steps are the same as those in Comparative Example 1, and are not repeated here.

[0108] Example 8

[0109] Different from Example 1, in this embodiment, the reduced graphene oxide includes a single-layer reduced graphene oxide and a few-layer reduced graphene oxide, and the mass ratio of the single-layer reduced graphene oxide to the few-layer reduced graphene oxide is 1:0.9. Other raw materials and steps are the same as those in Comparative Example 1, and are not repeated here.

[0110] Comparative Example 1

[0111] The difference from Example 1 is that in this comparative example, hydroxy acrylic resin is used without graphite modification. Other raw materials and steps are the same as those in Comparative Example 1, which will not be repeated here.

[0112] Comparative Example 2

[0113] Different from Example 1, in this comparative example, the preparation method of the rust-removing agent is as follows: phosphoric acid, gallic acid and phytic acid are added into a container, wherein the mass ratio of phosphoric acid, gallic acid and phytic acid is 1:0.3:2.5, and stirred for 5 minutes. Other raw materials and steps are the same as those in Comparative Example 1, and will not be repeated here.

[0114] Comparative Example 3

[0115] Different from Example 1, in this comparative example, the preparation method of the rust-removing agent is as follows: phosphoric acid, gallic acid and phytic acid are added into a container, wherein the mass ratio of phosphoric acid, gallic acid and phytic acid is 1:2:5.5, and stirred for 5 minutes. Other raw materials and steps are the same as those in Comparative Example 1, and will not be repeated here.

[0116] Comparative Example 4

[0117] Different from Example 1, in this comparative example, hydroxy acrylic resin is used without graphite modification;

[0118] The preparation method of the rust-removing agent is as follows: add phosphoric acid, gallic acid and phytic acid into a container, wherein the mass ratio of phosphoric acid, gallic acid and phytic acid is 1:0.3:2.5, and stir for 5 minutes. Other raw materials and steps are the same as those in comparative example 1, which will not be repeated here.

[0119] Comparative Example 5

[0120] Different from Example 1, in this comparative example, hydroxy acrylic resin is used without graphite modification;

[0121] The preparation method of the rust-removing agent is as follows: add phosphoric acid, gallic acid and phytic acid into a container, wherein the mass ratio of phosphoric acid, gallic acid and phytic acid is 1:2:5.5, and stir for 5 minutes. Other raw materials and steps are the same as those in comparative example 1, and will not be repeated here.

[0122] Performance Test:

[0123] The water-based acrylic resin coatings provided in Examples 1-8 and the water-based acrylic resin coatings provided in Comparative Examples 1-5 were subjected to performance tests. Specifically, after being stirred evenly, they were applied and dried for seven days under constant temperature and humidity conditions before the performance tests were conducted. The results are shown in Table 1.

[0124] The performance test contents are as follows:

[0125] Appearance test: in accordance with GB1729;

[0126] Adhesion test: Make the board according to the requirements of HG / T 3668, apply the paint, and then test it according to CJ / T 120-2008 to determine the adhesion of the coating;

[0127] Surface resistance test: MT 113-1995, technical index: ≤1×10 6 (Ω.m);

[0128] Wear resistance test: GB / T 1768-1979, technical indicators: 1000g pressure 1000 turns, ≤20g;

[0129] Flattening test: CJ / T 120-2008, flattening rate 4 / 5;

[0130] Bending test: CJ / T 120-2008, technical indicators: no peeling and cracking of the inner coating;

[0131] Alcohol torch flame combustion test: MT 181-88, technical indicators: average value of flame combustion time ≤3s; maximum value of flame combustion time ≤10s; average value of flameless combustion time ≤20s; maximum value of flameless combustion time ≤60s;

[0132] Paint film water resistance test: Make the board according to the requirements of HG / T 3668, apply the paint, and then test the paint film water resistance performance according to the requirements of GB / T 1733;

[0133] Acid resistance test of paint film: Make the board according to the requirements of HG / T 3668, apply the paint, and then test the acid resistance of the paint film according to the requirements of GB / T9274;

[0134] Alkali resistance test of paint film: Make the board according to the requirements of HG / T 3668, apply the paint, and then test the alkali resistance of the paint film according to the requirements of GB / T9265;

[0135] Paint film salt spray resistance test: Make the board according to the requirements of HG / T 3668, apply the paint, and then test the paint film salt spray resistance according to the requirements of GB / T1771;

[0136] Rust conversion degree test: Select steel plates with rust grades B and C in GB / T 9286, apply the coating to be tested at a coating rate of 4㎡ / kg, and cut the rusted parts with a blade after 24 hours to observe the rust conversion degree by visual inspection;

[0137] Rust conversion time test: Select steel plates with rust grades B and C in GB / T 9286, and apply the paint to be tested at a coating rate of 4㎡ / kg. From the end of painting, use a stopwatch to record the time it takes for the steel plate to change from its original color to completely black, and use visual inspection.

[0138] At present, the testing standards for the coating industry for coal mines are partially obtained by combining the methods of the three standards MT181, MT113, and CJ / T120. First, it must meet the anti-corrosion performance requirements and pass the CJ / T-120-2008 "Plastic-coated Composite Steel Pipe for Water Supply" standard test; second, it must be conductive, and the arithmetic average value of the surface resistance must be ≤1.0×10 6 Ohm; third, it must be flame retardant.

[0139] Table 1 Coating performance test data

[0140]

[0141]

[0142] It can be seen from Table 1 that the coatings prepared in Examples 1-8 of the present invention and Comparative Examples 1-5 have smooth surfaces, uniform colors, and no bubbles, cracks, or shrinkage cavities.

[0143] It can be seen from Table 1 that the water-based acrylic resin coatings of Examples 1-8 of the present invention have good adhesion and effectively prevent the further development of rust, and have excellent impact resistance, water resistance, acid resistance, alkali resistance and salt spray resistance.

[0144] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.

[0145] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

Claims

1. A rust-removing agent for water-based acrylic resin coatings in mines, characterized in that: include: Phosphoric acid; gallic acid; Phytic acid; The mass ratio of the phosphoric acid, gallic acid and phytic acid is 1:0.5-1.5:3-5.

2. The rust-removing agent according to claim 1, characterized in that: The mass ratio of the phosphoric acid, gallic acid and phytic acid is 1:1:

4.

3. A water-based acrylic resin coating, characterized in that: The composition comprises the following components in parts by weight: 40-50 parts of graphene-modified hydroxy acrylic resin; 5-7 parts of the rust-removing agent according to claim 1 or 2; 20-30 parts of rust inhibitor; Curing agent, add curing agent according to the NCO / OH molar ratio of 1.2 to 1.6:1; 20-30 parts of filler.

4. The water-based acrylic resin coating according to claim 3, characterized in that: The preparation method of the graphene-modified hydroxy acrylic resin comprises: Under the action of an initiator, the copolymer monomer and the modified graphene are polymerized in an organic solvent to obtain an intermediate solution; The intermediate liquid is neutralized, mixed with water, and stirred to obtain the graphene-modified hydroxy acrylic resin.

5. The water-based acrylic resin coating according to claim 4, characterized in that: The modified graphene is added in an amount of 1 to 3 parts; The comonomers include, by weight: 20-30 parts of methyl methacrylate; 5-10 parts of butyl methacrylate; 10-20 parts of acrylic acid; 15-30 parts of hydroxypropyl acrylate; 20-25 parts of isobornyl methacrylate; 3-8 parts of crotonic acid.

6. The water-based acrylic resin coating according to claim 5, characterized in that: The preparation process of the modified graphene includes: Reduced graphene oxide and dopamine were added in a mass ratio of 1:0.5-0.8, stirred at 120°C and a rotation speed of 200-300 rpm for 5-10 minutes, and then dried.

7. The water-based acrylic resin coating according to claim 6, characterized in that: The reduced graphene oxide comprises a single-layer reduced graphene oxide and a few-layer reduced graphene oxide, and the mass ratio of the single-layer reduced graphene oxide to the few-layer reduced graphene oxide is 1:0.6-0.

8.

8. The water-based acrylic resin coating according to claim 3, characterized in that: The rust inhibitor is zinc powder, the average particle size of the zinc powder is 3-4 μm, and the sphericity of the zinc powder is not less than 0.

6.

9. The water-based acrylic resin coating according to claim 3, characterized in that: The curing agent is aromatic isocyanate.

10. The water-based acrylic resin coating according to claim 3, characterized in that: Also includes: The additive comprises at least one of a leveling agent, a dispersant, a defoaming agent or a thickener.

Citation Information

Patent Citations

  • Water-based rust-converting agent and water-based rust-converting coating and their preparation methods

    CN114672795B

Cited By

  • Peelable and degradable water-based rust removal coating as well as preparation method and application thereof

    CN121203516A