Repair method of impact-wear-resistant high-manganese steel
By removing the metal fatigue layer of the Mn13 matrix of high manganese steel and using laser cladding to form an optimized transition layer and wear-resistant layer, the problem of insufficient impact resistance in wear repair of high manganese steel in the existing technology is solved, achieving a performance comparable to that of the original material. Or better than the impact wear resistance effect.
Patent Information
- Application Number
- CN202410896059.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-25
AI Technical Summary
In the existing technology, the repair of high manganese steel Mn13 after wear is difficult to meet the impact wear resistance requirements required by the equipment, and the impact wear resistance of the repaired area is lower than that of the original material.
By removing the metal fatigue layer in the pits of the Mn13 matrix of high manganese steel, laser cladding is used to form a transition layer and a wear-resistant layer in the repair area. The chemical composition of the transition layer and wear-resistant layer is optimized to improve toughness and work hardening ability.
It achieves impact wear resistance that is equivalent to or better than that of the high manganese steel Mn13 matrix, prolongs the service life of the repaired structural layer, and significantly improves the resistance to impact wear.
Smart Images

Figure CN118835239A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of repairing impact-wear resistant high manganese steel, and in particular, relates to a method for repairing impact-wear resistant high manganese steel. Background Art
[0002] When subjected to impact load, high manganese steel Mn13 with a Mn content of up to 11wt.% to 14wt.% will show obvious work hardening effect and has good resistance to impact wear. Figure 1 As shown in the figure, high manganese steel Mn13 is often used on the surface of the impact part of the equipment to resist impact wear. High manganese steel Mn13 steel plates are usually attached to the surface of equipment that is subject to external impact and needs protection by welding, bolting, etc. Figure 2 As shown in the figure, after the equipment has been used for a period of time, pits caused by impact will inevitably appear on the high manganese steel Mn13 base layer. In the prior art, arc welding, gas shielded welding and other methods are generally used to repair the high manganese steel Mn13 after wear. However, due to the composition of the welding material or the welding method, the impact wear resistance of the repaired area is far lower than that of the high manganese steel Mn13, and it is difficult to meet the impact wear resistance requirements required by the equipment.
[0003] Therefore, there is an urgent need to provide a new repair method for impact wear resistant high manganese steel. Summary of the invention
[0004] The embodiment of the present application provides a method for repairing impact-wear resistant high manganese steel, which can obtain impact-wear resistance equivalent to or better than that of a high manganese steel Mn13 matrix.
[0005] In a first aspect, the present application provides a method for repairing impact-wear resistant high manganese steel, comprising:
[0006] The metal fatigue layer at the pit of the high manganese steel Mn13 substrate is removed, and a repair area is formed at the position corresponding to the pit of the high manganese steel Mn13 substrate;
[0007] The transition layer alloy powder is prepared, and the transition layer alloy powder includes the following chemical components by mass percentage: C 0.015% to 0.03%; Si 0.35% to 0.6%; Mn 1% to 3%; P ≤ 0.02%; S ≤ 0.02%; Cr ≤ 22%; Ni 9% to 11%; Mo ≤ 0.5%; V ≤ 0.2%; Nb ≤ 0.02%; the balance is Fe and unavoidable impurities;
[0008] Laser cladding is used to clad the transition layer alloy powder on the high manganese steel Mn13 substrate in the repair area to obtain a cladding repair transition layer;
[0009] Prepare wear-resistant layer alloy powder, which includes the following chemical components by mass percentage: C1.0%-1.4%; Si 0.3%-0.5%; Mn 12.5%-13.5%; P≤0.02%; S≤0.005%; Cr 0.1%-0.3%; Ni≤0.5%; Mo≤0.5%; Ti≤0.1%; V≤0.2%; Nb≤0.02%; the balance is Fe and unavoidable impurities;
[0010] The wear-resistant layer alloy powder is clad on the cladding repair transition layer by laser cladding to form a wear-resistant layer.
[0011] According to an embodiment of the first aspect of the present application, the removal of the metal fatigue layer at the pits of the high manganese steel Mn13 substrate is performed by friction.
[0012] According to the embodiment of the first aspect of the present application, the removal of the metal fatigue layer at the pits of the high manganese steel Mn13 substrate is carried out by friction with a sanding machine.
[0013] According to an embodiment of the first aspect of the present application, the thickness of the cladding repair transition layer is 2 mm to 3 mm.
[0014] According to the embodiment of the first aspect of the present application, the repair method of impact-wear resistant high manganese steel also includes: grinding and polishing the cladding repair transition layer.
[0015] According to an embodiment of the first aspect of the present application, the thickness of the wear-resistant layer is 3 mm to 5 mm.
[0016] According to an embodiment of the first aspect of the present application, the method for repairing impact-wear resistant high manganese steel further includes:
[0017] The wear-resistant layer is polished so that the wear-resistant layer has a flat surface.
[0018] According to an embodiment of the first aspect of the present application, the depth of the pit is equal to the sum of the thicknesses of the cladding repair transition layer and the wear-resistant layer.
[0019] According to an embodiment of the first aspect of the present application, the method for repairing impact-wear resistant high manganese steel further includes:
[0020] The wear-resistant layer is pre-impacted to form a work-hardened layer.
[0021] According to the embodiment of the first aspect of the present application, the impact force used for the pre-impact treatment of the cladding repair transition layer is 100N / mm 2 ~500N / mm 2 The frequency of the pre-impact treatment is 1200 times / minute to 3600 times / minute, and the duration of the pre-impact treatment is 30 minutes to 90 minutes.
[0022] The repair method of the impact-wear resistant high manganese steel in the embodiment of the present application first removes the metal fatigue layer at the pit of the high manganese steel Mn13 substrate, and forms a repair area at the position corresponding to the pit of the high manganese steel Mn13 substrate to prevent the metal fatigue layer of the high manganese steel Mn13 substrate from affecting the combination of the subsequent repair layer and the high manganese steel Mn13 substrate; then, a cladding repair transition layer with good toughness is obtained by laser cladding transition layer alloy powder on the repair area, so as to effectively hinder the expansion of cracks extending from the wear-resistant layer during service; finally, wear-resistant layer alloy powder is clad on the cladding repair transition layer to form a wear-resistant layer. The wear-resistant layer formed by the wear-resistant layer alloy powder has good work-hardening ability, and can form a work-hardening layer as soon as it is impacted during service, thereby showing good impact wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solution of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0024] Figure 1 This is a schematic diagram of the structure of providing a high manganese steel Mn13 wear-resistant layer on the surface of equipment that needs wear-resistant or impact-resistant protection.
[0025] Figure 2 It is a schematic diagram of the structure of the surface of the wear-resistant layer of high manganese steel Mn13 being impacted with pits.
[0026] Figure 3 It is a flow chart of the repair method of impact wear resistant high manganese steel provided in the embodiment of the present application.
[0027] Figure 4 It is a schematic diagram of the effect after repair using the repair method for impact-wear resistant high manganese steel provided in an embodiment of the present application.
[0028] Description of reference numerals:
[0029] 1. Equipment that needs wear-resistant protection; 2. High manganese steel Mn13 wear-resistant layer; 3. Pits; 31. Cladding repair transition layer; 32. Wear-resistant layer. DETAILED DESCRIPTION
[0030] The features and exemplary embodiments of various aspects of the present application will be described in detail below. In order to make the purpose, technical solutions and advantages of the present application clearer, the present application will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only intended to explain the present application, rather than to limit the present application. For those skilled in the art, the present application can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present application by illustrating the examples of the present application.
[0031] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "include..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0032] In order to solve the problems of the prior art, the embodiment of the present application provides a method for repairing impact-wear-resistant high manganese steel. The method for repairing impact-wear-resistant high manganese steel provided by the embodiment of the present application is introduced below.
[0033] In general, a piece of wear-resistant material is provided as a protective layer in the parts of the equipment (such as shot blasting machines) that require a wear-resistant layer or impact protection (such as the inner wall of the shot blasting machine), with a thickness of about 5 to 25 mm. When this protective layer is worn through, it will wear out the metal of the equipment itself. Therefore, in order to extend the service life of this protective layer, the protective layer needs to be repaired. The present application provides a method for repairing high manganese steel that is resistant to impact and wear, for equipment that uses high manganese steel Mn13 as a protective layer and needs to repair the wear of the protective layer. The metallographic structure of high manganese steel Mn13 is an austenitic structure. Under the action of external impact (such as the shot of a shot blasting machine), it will be transformed into a martensitic structure, thereby producing a hardened layer. The hardened layer will produce wear, fatigue cracks, and even large pieces of peeling due to the long-term impact of external materials (such as the shot of a shot blasting machine), and pits will be formed at the worn or peeled parts.
[0034] The present application is intended to repair the pits after wear and spalling and the metal fatigue layer of high manganese steel Mn13.
[0035] like Figure 3As shown, the embodiment of the present application provides a method for repairing impact wear resistant high manganese steel, comprising:
[0036] S1. removing the metal fatigue layer at the pit of the high manganese steel Mn13 substrate, and forming a repair area at the position corresponding to the pit of the high manganese steel Mn13 substrate;
[0037] S2. Prepare transition layer alloy powder, which includes the following chemical components by mass percentage: C 0.015% to 0.03%; Si 0.35% to 0.6%; Mn 1% to 3%; P ≤ 0.02%; S ≤ 0.02%; Cr ≤ 22%; Ni 9% to 11%; Mo ≤ 0.5%; V ≤ 0.2%; Nb ≤ 0.02%; the balance is Fe and unavoidable impurities;
[0038] S3, using laser cladding to clad the transition layer alloy powder on the high manganese steel Mn13 substrate in the repair area to obtain a cladding repair transition layer;
[0039] S4. Prepare wear-resistant layer alloy powder, which includes the following chemical components by mass percentage: C 1.0% to 1.4%; Si 0.3% to 0.5%; Mn 12.5% to 13.5%; P ≤ 0.02%; S ≤ 0.005%; Cr 0.1% to 0.3%; Ni ≤ 0.5%; Mo ≤ 0.5%; Ti ≤ 0.1%; V ≤ 0.2%; Nb ≤ 0.02%; the balance is Fe and unavoidable impurities;
[0040] S5. A wear-resistant layer alloy powder is clad on the cladding repair transition layer by laser cladding to form a wear-resistant layer.
[0041] The repair method of the impact-wear resistant high manganese steel in the embodiment of the present application first removes the metal fatigue layer at the pit of the high manganese steel Mn13 substrate, and forms a repair area at the position corresponding to the pit of the high manganese steel Mn13 substrate to prevent the metal fatigue layer of the high manganese steel Mn13 substrate from affecting the combination of the subsequent repair layer and the high manganese steel Mn13 substrate; then, a cladding repair transition layer with good toughness is obtained by laser cladding transition layer alloy powder on the repair area, so as to effectively hinder the expansion of cracks extending from the wear-resistant layer during service; finally, wear-resistant layer alloy powder is clad on the cladding repair transition layer to form a wear-resistant layer. The wear-resistant layer formed by the wear-resistant layer alloy powder has good work-hardening ability, and can form a work-hardening layer when it is impacted during service, thereby showing good impact and wear resistance.
[0042] In the embodiments of the present application, the position corresponding to the pit in the high manganese steel Mn13 matrix refers to the area where the pit itself is located, or the area including the pit and extending from the pit to the outside of the pit in the high manganese steel Mn13 matrix that is impact-worn and needs to be repaired.
[0043] In an embodiment of the present application, the wear-resistant layer is formed by laser cladding of wear-resistant layer alloy powder, so that the composition of the wear-resistant layer is close to the matrix of high manganese steel Mn13. The impact effect during the impact process can be utilized to form a work-hardening layer on the surface of the wear-resistant layer to resist the impact wear during the impact process, thereby improving the impact wear resistance of the repair structure layer.
[0044] In the embodiments of the present application, since there is a certain thickness of metal fatigue layer at the pit, there are fatigue cracks inside the metal layer. If it is not polished and removed, it will affect the bonding effect between the subsequent repair structure layer metal and the high manganese steel Mn13 substrate, and may even peel off under the stress generated during the laser cladding process. Therefore, removing the metal fatigue layer at the pit of the high manganese steel Mn13 substrate and forming a repair area at the position corresponding to the pit of the high manganese steel Mn13 substrate can prevent the metal fatigue layer of the high manganese steel Mn13 substrate from affecting the bonding between the subsequent repair layer metal and the high manganese steel Mn13 substrate.
[0045] It is understandable that the thickness of the metal fatigue layer of high manganese steel Mn13 will vary depending on factors such as service time and external impact load. Therefore, the removal thickness / depth of the metal fatigue layer is not a fixed value. The removal thickness / depth is generally based on the absence of fatigue cracks after grinding. Whether fatigue cracks exist can be determined by penetrant testing, and the applicant will not elaborate on this.
[0046] In some embodiments of the present application, the removal of the metal fatigue layer at the pits of the high manganese steel Mn13 substrate is performed by friction.
[0047] In some embodiments of the present application, the removal of the metal fatigue layer at the pits of the high manganese steel Mn13 substrate is performed by friction with a sanding machine.
[0048] In the embodiments of the present application, handheld or automated equipment such as a belt sander, a polisher, and an angle grinder are used to remove the metal fatigue layer on the surface of the pits in the high manganese steel Mn13 by friction, avoiding the use of impact to remove the metal fatigue layer, thereby avoiding the formation of a work hardening layer in the high manganese steel Mn13 matrix and affecting the toughness of the high manganese steel Mn13 matrix.
[0049] In an embodiment of the present application, laser cladding is used to clad the transition layer alloy powder in the repair area to form a cladding repair transition layer with good toughness, which can effectively hinder the expansion of cracks extending from the wear-resistant layer during service and improve the impact wear resistance of the repair structural layer.
[0050] In the embodiment of the present application, the thickness of the cladding repair transition layer can be clad according to the depth of the pit. For a location with a deeper pit, the thickness of the cladding repair transition layer can be appropriately thicker; for a location with a shallower pit, the thickness of the cladding repair transition layer can be appropriately thinner.
[0051] In some embodiments of the present application, the thickness of the cladding repair transition layer is 2 mm to 3 mm.
[0052] In some embodiments of the present application, the method for repairing impact-wear resistant high manganese steel further includes: grinding and polishing the cladding repair transition layer.
[0053] In an embodiment of the present application, handheld or automated equipment such as a wire brush, a grinder, and a polishing machine can be used to grind and polish the cladding repair transition layer in the previous step to remove impurities, unfused alloy powder, etc. on the metal surface of the cladding repair transition layer, so as to facilitate the subsequent cladding of the wear-resistant layer and reduce interlayer defects, thereby improving the interlayer bonding strength between the cladding repair transition layer and the wear-resistant layer.
[0054] In the embodiments of the present application, laser cladding is used to clad the wear-resistant layer alloy powder on the cladding repair transition layer, so that a wear-resistant layer resistant to impact wear can be formed, which has good work hardening ability and can form a work hardening layer as soon as it is impacted during service, thereby exhibiting good impact wear resistance.
[0055] In some embodiments of the present application, the method for repairing impact-wear resistant high manganese steel further includes: grinding the wear-resistant layer so that the wear-resistant layer has a smooth surface.
[0056] In the embodiment of the present application, the laser-clad wear-resistant layer is subjected to residual height grinding to obtain a flat surface so that the wear-resistant layer as a whole is evenly impacted to avoid aggravated wear in local areas due to uneven surface.
[0057] In some embodiments of the present application, the thickness of the wear-resistant layer is 3 mm to 5 mm.
[0058] In some embodiments of the present application, the method for repairing impact-wear resistant high manganese steel further includes: performing a pre-impact treatment on the wear-resistant layer to form a work-hardening layer.
[0059] In the embodiments of the present application, the wear-resistant layer is subjected to a pre-impact treatment to form a work-hardening layer of a certain thickness on the surface of the wear-resistant layer, thereby improving the impact wear resistance of the repaired area.
[0060] In some embodiments of the present application, the thickness of the work-hardened layer is 100 μm to 500 μm.
[0061] In the embodiment of the present application, the wear-resistant layer is subjected to a pre-impact treatment, so that the structure of the surface metal is transformed from austenite to martensite, which can promote the formation of a work hardening layer of a certain thickness on the surface of the wear-resistant layer, thereby improving the impact wear resistance of the repaired area. The pre-impact treatment can be performed by hammering.
[0062] In some embodiments of the present application, the impact force used in the pre-impact treatment of the wear-resistant layer is such that the structure of the surface metal of the wear-resistant layer is transformed from austenite to martensite. For example, the impact force is 100N / mm 2 ~500N / mm 2 The frequency of the pre-impact treatment is 1200 times / minute to 3600 times / minute / second, and the duration of the pre-impact treatment is 30 minutes to 90 minutes.
[0063] In the embodiments of the present application, within the parameter range defined in the present application, the greater the pre-impact force, the higher the pre-impact treatment frequency, and the longer the pre-impact treatment time, the thicker the work-hardened layer thickness is, and the better the impact and wear resistance is.
[0064] like Figure 4 As shown, after grinding the pits on the surface of the steel plate body of the worn high manganese steel Mn13, laser cladding transition layer alloy powder and wear-resistant layer alloy powder are used to form a repair transition layer and wear-resistant layer. The wear-resistant layer metal formed after cladding the wear-resistant layer alloy powder may be higher than the surface of the high manganese steel Mn13 substrate, so it is also necessary to make the wear-resistant layer flush with the substrate surface after grinding. Finally, by hammering the surface of the wear-resistant layer after laser cladding, that is, pre-impact treatment is performed, so that martensitic transformation occurs, thereby producing a work-hardening layer, and the surface becomes more wear-resistant. In addition, considering that the substrate of the high manganese steel Mn13 steel plate near the pit has been in service for a period of time, there is also a partial work-hardening layer on the surface. In order to reduce the wear resistance difference between the laser cladding repaired area and the nearby area, hammering the wear-resistant layer after cladding can also produce a work-hardening layer, which is consistent with the wear resistance of the high manganese steel Mn13 substrate in the area around the pit, and improves the impact wear resistance of the repaired structural layer.
[0065] The technical method of the present application will be further illustrated by means of specific embodiments and comparative examples.
[0066] Embodiment 1 A method for repairing impact-wear resistant high manganese steel comprises:
[0067] S1. Use a sanding machine to remove the metal fatigue layer at the pit of the high manganese steel Mn13 substrate. The removal thickness is based on the absence of fatigue cracks. A repair area is formed at the position corresponding to the pit of the high manganese steel Mn13 substrate. The pit depth is 7mm.
[0068] S2. Prepare transition layer alloy powder, which includes the following chemical components by mass percentage: C 0.02%; Si 0.4%; Mn 2.2%; P 0.01%; S 0.05%; Cr 18%; Ni 9.2%; Mo 0.42%; V 0.12%; Nb 0.01%; the balance is Fe and unavoidable impurities.
[0069] S3, using laser cladding to clad the transition layer alloy powder on the high manganese steel Mn13 substrate in the repair area to obtain a cladding repair transition layer with a thickness of 3 mm; using an angle grinder to grind and polish the cladding repair transition layer to obtain a cladding repair transition layer with a smooth surface;
[0070] S4. Prepare wear-resistant layer alloy powder, which includes the following chemical components by mass percentage: C 1.1%; Si 0.35%; Mn 13.5%; P 0.01%; S 0.001%; Cr 0.22%; Ni 0.45%; Mo 0.38%; Ti 0.08%; V 0.12%; Nb 0.015%; the balance is Fe and unavoidable impurities;
[0071] S5. Use laser cladding to clad the wear-resistant layer alloy powder on the cladding repair transition layer to form a wear-resistant layer with a thickness of 5 mm; use an angle grinder to grind the wear-resistant layer to obtain a wear-resistant layer with a smooth surface. The total thickness of the repair structure layer is 7 mm.
[0072] Embodiment 2 A method for repairing impact-wear resistant high manganese steel comprises:
[0073] S1. Use a sanding machine to remove the metal fatigue layer at the pit of the high manganese steel Mn13 substrate. The removal thickness is based on the absence of fatigue cracks. A repair area is formed at the position corresponding to the pit of the high manganese steel Mn13 substrate. The pit depth is 7mm.
[0074] S2. Prepare transition layer alloy powder, which includes the following chemical components by mass percentage: C 0.02%; Si 0.4%; Mn 2.2%; P 0.01%; S 0.05%; Cr 18%; Ni 9.2%; Mo 0.42%; V 0.12%; Nb 0.01%; the balance is Fe and unavoidable impurities;
[0075] S3, using laser cladding to clad the transition layer alloy powder on the high manganese steel Mn13 substrate in the repair area to obtain a cladding repair transition layer with a thickness of 3 mm; using an angle grinder to grind and polish the cladding repair transition layer to obtain a cladding repair transition layer with a smooth surface;
[0076] S4. Prepare wear-resistant layer alloy powder, which includes the following chemical components by mass percentage: C 1.1%; Si 0.35%; Mn 13.5%; P 0.01%; S 0.001%; Cr 0.22%; Ni 0.45%; Mo 0.38%; Ti 0.08%; V 0.12%; Nb 0.015%; the balance is Fe and unavoidable impurities;
[0077] S5. Using laser cladding to clad the wear-resistant layer alloy powder on the cladding repair transition layer to form a wear-resistant layer with a thickness of 5 mm; using an angle grinder to grind the wear-resistant layer to obtain a wear-resistant layer with a smooth surface; the total thickness of the repaired structural layer is 7 mm;
[0078] S6, 100N / mm for the wear-resistant layer 2 The frequency of the pre-impact treatment is 1200 times / minute, and the time of the pre-impact treatment is 30 minutes to form a work-hardened layer with a thickness of 100 μm.
[0079] Embodiment 3 A method for repairing impact-wear resistant high manganese steel comprises:
[0080] S1. Use a sanding machine to remove the metal fatigue layer at the pit of the high manganese steel Mn13 substrate. The removal thickness is based on the absence of fatigue cracks. A repair area is formed at the position corresponding to the pit of the high manganese steel Mn13 substrate. The pit depth is 7mm.
[0081] S2. Prepare transition layer alloy powder, which includes the following chemical components by mass percentage: C 0.02%; Si 0.4%; Mn 2.2%; P 0.01%; S 0.05%; Cr 18%; Ni 9.2%; Mo 0.42%; V 0.12%; Nb 0.01%; the balance is Fe and unavoidable impurities;
[0082] S3, using laser cladding to clad the transition layer alloy powder on the high manganese steel Mn13 substrate in the repair area to obtain a cladding repair transition layer with a thickness of 2 mm; using an angle grinder to grind and polish the cladding repair transition layer to obtain a cladding repair transition layer with a smooth surface;
[0083] S4. Prepare wear-resistant layer alloy powder, which includes the following chemical components by mass percentage: C 1.1%; Si 0.35%; Mn 13.5%; P 0.01%; S 0.001%; Cr 0.22%; Ni 0.45%; Mo 0.38%; Ti 0.08%; V 0.12%; Nb 0.015%; the balance is Fe and unavoidable impurities;
[0084] S5. Using laser cladding to clad the wear-resistant layer alloy powder on the cladding repair transition layer to form a wear-resistant layer with a thickness of 6.5 mm; using an angle grinder to grind the wear-resistant layer to obtain a wear-resistant layer with a smooth surface; the total thickness of the repaired structural layer is 7 mm;
[0085] S6, 200N / mm for wear-resistant layer 2 The frequency of the pre-impact treatment is 1200 times / minute, and the pre-impact treatment time is 30 minutes to form a work-hardened layer with a thickness of 130 μm.
[0086] Embodiment 4 A method for repairing impact-wear resistant high manganese steel comprises:
[0087] S1. Use a sanding machine to remove the metal fatigue layer at the pit of the high manganese steel Mn13 substrate. The removal thickness is based on the absence of fatigue cracks. A repair area is formed at the position corresponding to the pit of the high manganese steel Mn13 substrate. The pit depth is 7mm.
[0088] S2. Prepare transition layer alloy powder, which includes the following chemical components by mass percentage: C 0.025%; Si 0.5%; Mn 2.2%; P 0.02%; S 0.01%; Cr 18%; Ni 10%; Mo 0.4%; V 0.12%; Nb 0.01%; the balance is Fe and unavoidable impurities;
[0089] S3, using laser cladding to clad the transition layer alloy powder on the high manganese steel Mn13 substrate in the repair area to obtain a cladding repair transition layer with a thickness of 3.5 mm; using an angle grinder to grind and polish the cladding repair transition layer to obtain a cladding repair transition layer with a smooth surface;
[0090] S4. Prepare wear-resistant layer alloy powder, which includes the following chemical components by mass percentage: C 1.2%; Si 0.5%; Mn 12.5%; P 0.01%; S 0.002%; Cr 0.25%; Ni 0.45%; Mo 0.38%; Ti 0.08%; V 0.12%; Nb 0.015%; the balance is Fe and unavoidable impurities;
[0091] S5. Using laser cladding to clad the wear-resistant layer alloy powder on the cladding repair transition layer to form a wear-resistant layer with a thickness of 4 mm; using an angle grinder to grind the wear-resistant layer to obtain a wear-resistant layer with a smooth surface. The total thickness of the repaired structural layer is 7 mm;
[0092] S6, 200N / mm for wear-resistant layer 2The frequency of the pre-impact treatment is 1500 times / minute, and the pre-treatment time is 60 minutes to form a work-hardened layer with a thickness of 170 μm.
[0093] Comparative Example 1 uses a high manganese steel Mn13 steel plate with a thickness of 7 mm as a comparison benchmark.
[0094] In Comparative Example 2, a 7 mm deep pit was repaired by arc welding to form a repaired structural layer. The composition of the welding rod used in the transition layer of Comparative Example 2 was the same as the alloy powder composition of the transition layer of Example 1, and the composition of the welding rod used in the wear-resistant layer of Comparative Example 2 was the same as the alloy powder composition of the wear-resistant layer of Example 1.
[0095] In Comparative Example 3, a 7 mm deep pit was repaired by metal active gas welding to form a repaired structural layer. The composition of the welding rod used in the transition layer of Comparative Example 3 was the same as the alloy powder composition of the transition layer of Example 1, and the composition of the welding rod used in the wear-resistant layer of Comparative Example 3 was the same as the alloy powder composition of the wear-resistant layer of Example 1.
[0096] The repaired structural layer formed by the repair method of the impact wear resistant high manganese steel in Examples 1-4 and the repaired structural layer formed by the repair method of the high manganese steel Mn13 steel plate in Comparative Example 1 and Comparative Examples 2-3 were tested for impact wear resistance, and the test data were recorded in the following Table 1 for performance comparison. The test method is:
[0097] Shots with a diameter of 0.8 mm are selected for shot blasting machines, and are ejected from the shot outlet of the shot blasting machine at a speed of 50 m / s. The height from the shot outlet to the shot impact position is set to 1000 mm. The repaired structural layer of Examples 1-4 and the high manganese steel plate of Comparative Example 1 and the repaired structural layer formed by the repair method of Comparative Example 2-3 are placed at the shot impact position for impact testing, and the maximum wear depth is recorded as a detection index for impact wear resistance. The wear depth of the repaired structural layer and the high manganese steel Mn13 steel plate in the above-mentioned embodiments and comparative examples after 30 minutes of impact by shot blasting machines is used as the test result of impact wear resistance. Among them, the greater the wear depth, the worse the impact wear resistance; conversely, the better the impact wear resistance.
[0098] Table 1
[0099]
[0100] By comparing the test data in Table 1, it can be concluded that the wear depth of the surface of a 7mm thick high manganese steel plate after 30 minutes of impact is 10μm as a comparison benchmark;
[0101] Compared with the high manganese steel Mn13 steel plate in comparative example 1, the repaired structural layer obtained by the repair method of embodiment 1 of the present application has a wear depth of 12 μm after 30 minutes of impact, indicating that the repaired structural layer formed by the repair method of impact-wear resistant high manganese steel in embodiment 1 of the present application has an impact wear resistance close to that of the high manganese steel Mn13 steel plate, and the wear depth is only 2 μm higher than that of the high manganese steel Mn13 steel plate, but is still significantly less than the wear depths of 16 μm and 18 μm of comparative examples 2 and 3, respectively. This also indicates that the repair method of embodiment 1 of the present application can obtain a relatively good repair effect equivalent to that of the high manganese steel Mn13 steel plate.
[0102] Compared with the high manganese steel Mn13 steel plate in comparative example 1, the repaired structural layer obtained by the repair method of Example 2 of the present application also includes a work-hardening layer with a thickness of 100 μm. The wear depth of the repaired structural layer after 30 minutes of impact is only 3 μm, indicating that the repaired structural layer with a work-hardening layer formed by the repair method of impact-wear resistant high manganese steel in Example 2 of the present application has an impact wear resistance that is significantly higher than that of the high manganese steel Mn13 steel plate.
[0103] Compared with the high manganese steel Mn13 steel plate in comparative example 1, the repaired structural layer obtained by the repair method of Example 3 of the present application also includes a work-hardening layer with a thickness of 130 μm. The wear depth of the repaired structural layer after 30 minutes of impact is only 2 μm, indicating that the repaired structural layer with a work-hardening layer formed by the repair method of the impact-wear resistant high manganese steel in Example 3 of the present application has significantly higher impact wear resistance than that of the high manganese steel Mn13 steel plate.
[0104] Compared with the high manganese steel Mn13 steel plate in comparative example 1, the repaired structural layer obtained by the repair method of Example 4 of the present application also includes a work-hardening layer with a thickness of 170 μm. The wear depth of the repaired structural layer after 30 minutes of impact is only 2 μm, indicating that the repaired structural layer with a work-hardening layer formed by the repair method of the impact-wear resistant high manganese steel in Example 4 of the present application has an impact wear resistance that is significantly better than that of the high manganese steel Mn13 steel plate.
[0105] Through the above comparison, it can be concluded that the repaired structural layer obtained by the repair method of Examples 1 to 4 of the present application has a wear depth under the impact of shot blasting machine pellets that is less than the wear depth of the repaired structural layer obtained by the repair method of Comparative Examples 2 to 3 under the impact of shot blasting machine pellets; and the repaired structural layer obtained by the repair method of Example 1 for the impact wear resistant high manganese steel has a slightly weaker impact wear resistance than the high manganese steel Mn13 steel plate, and is similar to the impact wear resistance of the high manganese steel Mn13 steel plate, but is still better than the impact wear resistance of the repaired structural layer of Comparative Examples 2 to 3. This shows that the repaired structural layer obtained by the repair method of the impact wear resistant high manganese steel of the present application has good impact wear resistance.
[0106] After analysis, under the condition of the same welding material composition, the laser cladding repair method has high laser energy density, fast cladding speed, small heat input and relatively fast cooling speed, so the corresponding repair structure layer has better impact wear resistance, that is, better wear resistance. Compared with laser cladding, arc welding has lower energy density and larger diameter of welding rod, generally 3.2mm~4.0mm, slow melting speed of welding rod, slow welding speed and large welding heat input, resulting in slow cooling speed, making the weld metal hardness low, and the corresponding repair structure layer has poor impact wear resistance. Compared with the repair methods of laser cladding and arc welding, the heat input of gas shielded welding is between laser cladding and arc welding, that is, the heat input of gas shielded welding is slightly smaller than that of arc welding, but much larger than that of laser cladding. Therefore, the impact wear resistance of the repair structure layer formed by gas shielded welding is slightly better than that of arc welding, but worse than that of the repair structure layer formed by laser cladding repair. That is, since the heat input of arc welding is the largest, the heat input of gas shielded welding is the second, and the heat input of laser cladding is the smallest, the cooling rates of the repaired structural layers formed by the three different repair methods are very slow, relatively slow, and relatively fast, respectively, which causes the hardness of the corresponding wear-resistant layers to be low, relatively low, and relatively high, respectively. Ultimately, the impact wear resistance of the repaired structural layers formed by the repair methods of Examples 1-4 of the present application is better than the impact wear resistance of the wear-resistant layers formed by the repair methods of Comparative Examples 2-3.
[0107] It can be seen that the repaired structural layer obtained by the repair method for impact-wear resistant high manganese steel according to the embodiment of the present application has an impact-wear resistance performance that is significantly higher than or equivalent to the impact-wear resistance performance of high manganese steel Mn13 steel plate.
[0108] The above is only a specific implementation method of the present application. Those skilled in the art can clearly understand that for the convenience and simplicity of description, the specific working process described above can refer to the corresponding process in the aforementioned method embodiment, and will not be repeated here. It should be understood that the protection scope of the present application is not limited to this. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the protection scope of the present application.
Claims
1. A method for repairing impact-wear resistant high manganese steel, characterized in that: include: The metal fatigue layer at the pit of the high manganese steel Mn13 substrate is removed, and a repair area is formed at the position corresponding to the pit of the high manganese steel Mn13 substrate; The transition layer alloy powder is prepared, and the transition layer alloy powder includes the following chemical components by mass percentage: C 0.015% to 0.03%; Si 0.35% to 0.6%; Mn 1% to 3%; P ≤ 0.02%; S ≤ 0.02%; Cr ≤ 22%; Ni 9% to 11%; Mo ≤ 0.5%; V ≤ 0.2%; Nb ≤ 0.02%; the balance is Fe and unavoidable impurities; The transition layer alloy powder is clad on the high manganese steel Mn13 substrate in the repair area by laser cladding to obtain a cladding repair transition layer; Prepare wear-resistant layer alloy powder, which includes the following chemical components by mass percentage: C 1.0%-1.4%; Si 0.3%-0.5%; Mn 12.5%-13.5%; P≤0.02%; S≤0.005%; Cr 0.1%-0.3%; Ni≤0.5%; Mo≤0.5%; Ti≤0.1%; V≤0.2%; Nb≤0.02%; the balance is Fe and unavoidable impurities; The wear-resistant layer alloy powder is clad on the cladding repair transition layer by laser cladding to form a wear-resistant layer.
2. The repair method according to claim 1, characterized in that: Also includes: The wear-resistant layer is subjected to a pre-impact treatment to form a work-hardened layer.
3. The repair method according to claim 1 or 2, characterized in that: The removal of the metal fatigue layer at the pits of the high manganese steel Mn13 substrate is carried out in a friction manner.
4. The repair method according to claim 1, characterized in that: The depth of the pit is equal to the sum of the thickness of the cladding repair transition layer and the wear-resistant layer.
5. The repair method according to claim 1, characterized in that: The thickness of the cladding repair transition layer is 2 mm to 3 mm.
6. The repair method according to claim 1, characterized in that Also includes: The cladding repair transition layer is ground and polished.
7. The repair method according to claim 1, characterized in that: The thickness of the wear-resistant layer is 3 mm to 5 mm.
8. The repair method according to claim 1, characterized in that: Also includes: The wear-resistant layer is polished so that the wear-resistant layer has a flat surface.
9. The repair method according to claim 2, characterized in that: The impact force used for the pre-impact treatment of the wear-resistant layer is 100N / mm 2 ~500N / mm 2 The frequency of the pre-impact treatment is 1200 times / minute to 3600 times / minute, and the duration of the pre-impact treatment is 30 minutes to 90 minutes.
10. The repair method according to claim 2 or 9, characterized in that: The thickness of the work-hardened layer is 100 μm to 500 μm.