MoS2 Moire superlattice electrocatalyst as well as preparation method and application thereof
By preparing the MoS2 Mohr superlattice electrocatalyst on a SiO2/Si substrate and using the PVA transfer method to form a double-layer structure, the problem of high cost of noble metal catalysts and activity concentrated at the edges of grain boundaries is solved, significantly improving the electrocatalytic activity and The electrochemical performance achieves efficient electrocatalytic hydrogen evolution effect.
Patent Information
- Application Number
- CN202411082107.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-25
AI Technical Summary
Existing precious metal catalysts are expensive and scarce in the process of electrolyzing water to produce hydrogen. The catalytic activity of the two-dimensional transition metal sulfide MoS2 is mainly concentrated on the edges of grain boundaries, which limits the improvement of its catalytic performance.
MoS2 Mohr superlattice electrocatalyst was prepared on SiO2/Si substrate by chemical vapor deposition method, and the rotational dislocation or lattice dislocation of the double-layer structure was achieved through PVA transfer method, which significantly increased the active sites and reduced the interlayer barrier. , improve electrocatalytic activity.
It improves the electrochemical activity of the MoS2 electrocatalyst, simplifies the preparation process, reduces the Gibbs free energy of hydrogen adsorption, and has good electrocatalytic hydrogen evolution performance and large-scale production potential.
Smart Images

Figure CN118835261A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of functional materials and relates to an electrocatalyst, and in particular to a MoS2 moiré superlattice electrocatalyst and a preparation method and application thereof. Background Art
[0002] The extensive use of fossil fuels has not only led to energy shortages, but also caused serious environmental problems. Therefore, the development of a new energy source that is widely available, environmentally friendly and low-cost has become the focus of scientific researchers. Hydrogen, as a clean energy source, has great potential, and the development of hydrogen energy technology is of great significance for promoting sustainable development. Traditional hydrogen production methods are often accompanied by carbon emissions, while water electrolysis, as a carbon-free hydrogen production technology, has the potential to replace non-renewable energy. At present, precious metal materials such as platinum (Pt), rhodium (Rh) and iridium (Ir) and their oxides (RhO2, IrO2) are the most effective catalysts in the process of water electrolysis, but their high cost and scarcity limit their widespread application.
[0003] In recent years, two-dimensional transition metal sulfides (TMDs) have shown great potential as non-precious metal catalysts in the field of water electrolysis. In particular, molybdenum disulfide (MoS2), whose theoretical hydrogen adsorption free energy is close to zero, is very suitable for catalysis of hydrogen evolution reaction (HER). However, for 2H-MoS2 with semiconductor properties, its catalytic activity is mainly concentrated at the edges of grain boundaries, which to some extent limits the further improvement of its catalytic performance. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a MoS2 moiré superlattice electrocatalyst and its preparation method and application. The preparation method is simple and controllable, and the prepared MoS2 moiré superlattice electrocatalyst has high charge transfer efficiency and has high electrocatalytic performance when applied to the catalytic reaction of hydrogen production by electrolysis of water.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] Step 1: Use a pipette to pipette 2-3 μl of 2.5-10 mg / ml (NH4)2MoO4 solution and 1 μl of 5 mg / ml NaCl solution onto the bottom film, place it in an oven to dry, then place the bottom film in a quartz boat, then turn the top film upside down on the boat, and place the quartz boat in the center of the tube furnace; the bottom film and the top film are SiO2 / Si substrates;
[0007] Take excess sulfur powder and pile it in a quartz tile, place it upstream of the tube furnace, place the SiO2 / Si substrate downstream of the tube furnace, use argon as carrier gas, and prepare MoS2 on the surface of the SiO2 / Si substrate by chemical vapor deposition. The temperature of the tube furnace is raised to 700℃-900℃ at a heating rate of 30-50℃ / min, and ventilation and heat preservation are continued for 5-20min. After completion, it is naturally cooled to room temperature and the sample is taken out;
[0008] Two groups of MoS2 grown on SiO2 / Si substrates were prepared in parallel;
[0009] Step 2: Use the PVA transfer method to transfer the MoS2 grown on one of the SiO2 / Si substrates prepared in step 1 to another SiO2 / Si substrate with MoS2, and anneal at 300°C for 0.5-1h to obtain a MoS2 moiré superlattice.
[0010] The present invention also has the following technical features:
[0011] Preferably, the SiO2 / Si substrate is ultrasonically cleaned in acetone, isopropanol, anhydrous ethanol and deionized water respectively before use and then dried.
[0012] Preferably, the quartz boat and quartz tile are ultrasonically cleaned in acetone, isopropanol, anhydrous ethanol and deionized water respectively before use and then dried.
[0013] Preferably, the drying in step 1 is performed by placing the product in an oven at 50° C. for 3-5 minutes.
[0014] Preferably, the flow rate of the carrier gas is 50-200 sccm.
[0015] Preferably, the specific operation of the PVA transfer method is: take 5g of PVA particles and 1g of glycerol and add them to 100mL of deionized water, stir thoroughly with a glass rod until the PVA is completely dissolved in the deionized water to form a solution; drop the PVA solution on a SiO2 / Si substrate with MoS2, heat and cure the PVA on a heating table, and the heating time is 8-10min; after curing, transfer the film to another SiO2 / Si substrate with MoS2 to obtain a MoS2 moiré superlattice, and finally soak it in deionized water for 20-30min to remove the PVA.
[0016] The present invention also protects a MoS2 moiré superlattice electrocatalyst prepared by the method as described above and its application in hydrogen production by electrolysis of water.
[0017] Compared with the prior art, the present invention has the following technical effects:
[0018] The present invention firstly uses ammonium molybdate and sulfur powder as precursors, and prepares MoS2 crystal domains of different sizes, different densities and different shapes on a SiO2 / Si substrate by chemical vapor deposition; then, the grown MoS2 is transferred to another SiO2 / Si substrate with MoS2 by PVA transfer method, and the rotational dislocation or lattice dislocation of the double-layer structure obtains a nano-scale MoS2 moiré superlattice, which significantly increases the number of active sites, reduces the interlayer potential barrier, and reduces the hydrogen adsorption Gibbs free energy, thereby improving the electrochemical activity of the electrocatalyst;
[0019] This method has a simple preparation process and is easy to operate. The PVA transfer method can artificially control the interlayer rotation angle of the heterojunction, which is conducive to large-scale production and promotion. The prepared MoS2 moiré superlattice electrocatalytic hydrogen production catalyst has good application prospects in the fields of electrocatalytic hydrogen evolution. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 OM image of the MoS2 moiré superlattice prepared in Example 1;
[0021] Figure 2 LSV diagram of the MoS2 moiré superlattice electrocatalyst prepared in Example 1;
[0022] Figure 3 The Tafel slope diagram of the MoS2 moiré superlattice catalyst prepared in Example 1;
[0023] Figure 4 This is the impedance diagram of the MoS2 moiré superlattice electrocatalyst prepared in Example 1. DETAILED DESCRIPTION
[0024] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.
[0025] Example 1
[0026] A method for preparing a MoS2 moiré superlattice electrocatalyst comprises the following steps:
[0027] Step 1, Si / SiO2 substrate pretreatment: a bottom sheet with a size of 1 cm × 0.7 cm and a top sheet with a size of 1 cm × 1.8 cm were ultrasonically cleaned in acetone, isopropanol and anhydrous ethanol for 10 min respectively, and then dried with nitrogen;
[0028] Step 2, use a pipette to draw 2 μl of 2.5 mg / ml (NH4)2MoO4 solution and 1 μl of 5 mg / ml NaCl solution onto the bottom film, place it in an oven at 50°C for 3 min, then place the bottom film in a quartz boat, turn the top film upside down on the boat, and place the quartz boat in the center of the tube furnace;
[0029] 180 mg of sulfur powder was piled on a quartz tile, and the quartz tile was placed in a sleeve. The sleeve was then placed in a tube furnace and argon gas with a flow rate of 100 sccm was introduced for 30 minutes. The tube furnace was then heated to 750°C at a heating rate of 30°C / min. After growing for 20 minutes, it was naturally cooled to room temperature, and MoS2 was deposited on the top sheet.
[0030] Two groups of MoS2 grown on SiO2 / Si substrates were prepared in parallel;
[0031] Step 3, take 5g PVA particles and 1g glycerol, add them to 100mL deionized water, stir thoroughly with a glass rod until PVA is completely dissolved in the deionized water to obtain a PVA solution; drop the PVA solution onto the SiO2 / Si substrate grown with MoS2, place it on a heating table to cure for 10 minutes, wait for the PVA to dry, tear it off along the edge and stick it to another SiO2 / Si substrate grown with MoS2, soak the transferred SiO2 / Si in water for 30 minutes to remove the PVA, and anneal it at 300°C for 1 hour to obtain the MoS2 moiré superlattice.
[0032] Wet the polishing flannel with deionized water, pour in an appropriate amount of polishing powder with a particle size of 0.3μm, continue to add water to form a suspension, and polish the glassy carbon electrode in an "8" motion for ten minutes; then rinse the glassy carbon electrode with deionized water, replace it with another polishing powder with a particle size of 50nm and repeat the above steps, and finally blow the glassy carbon electrode dry with nitrogen for later use. Similarly, the prepared MoS2 moiré superlattice is transferred to the treated glassy carbon electrode using the PVA transfer method to obtain the MoS2 moiré superlattice electrocatalytic hydrogen production catalyst, which can be used for subsequent electrochemical tests.
[0033] Figure 1 This is the OM image of the MoS2 moiré superlattice prepared in Example 1. Figure 2 LSV diagram of the MoS2 moiré superlattice electrocatalyst prepared in Example 1 at 10 mA / cm 2 The potential corresponding to the current density is 420 mV (Vs RHE). Figure 3 This is the Tafel slope diagram of the MoS2 moiré superlattice catalyst prepared in Example 1. It can be seen from the figure that the slope is 158.2 mV dec -1 . Figure 4 This is the impedance diagram of the MoS2 moiré superlattice electrocatalyst prepared in Example 1. The charge transfer resistance (Rct) value is 119.7Ω obtained by fitting the equivalent Randles circuit model in Zview software; the prepared MoS2 moiré superlattice electrocatalyst has good catalytic hydrogen evolution performance.
[0034] Example 2
[0035] A method for preparing a MoS2 moiré superlattice electrocatalyst comprises the following steps:
[0036] Step 1, SiO2 / Si substrate pretreatment: a bottom sheet with a size of 1 cm×0.7 cm and a top sheet with a size of 1 cm×1.8 cm were ultrasonically cleaned in acetone, isopropanol and anhydrous ethanol for 10 min respectively, and then dried with nitrogen;
[0037] Step 2, use a pipette to draw 3 μl of 2.5 mg / ml (NH4)2MoO4 solution and 1 μl of 5 mg / ml NaCl solution onto the bottom film, place it in an oven at 50°C for 5 min, then place the bottom film in a quartz boat, turn the top film upside down on the boat, and place the quartz boat in the center of the tube furnace;
[0038] 270 mg of sulfur powder was piled on a quartz tile, and the quartz tile was placed in a sleeve. The sleeve was then placed in a tube furnace and argon gas with a flow rate of 50 sccm was introduced for 30 minutes. The tube furnace was then heated to 900°C at a heating rate of 50°C / min. After growing for 5 minutes, it was naturally cooled to room temperature, and MoS2 was deposited on the top sheet.
[0039] Two groups of MoS2 grown on SiO2 / Si substrates were prepared in parallel;
[0040] Step 3, take 5g PVA particles and 1g glycerol, add them to 100mL deionized water, stir thoroughly with a glass rod until PVA is completely dissolved in the deionized water to obtain a PVA solution; drop the PVA solution onto the SiO2 / Si substrate grown with MoS2, place it on a heating table to cure for 8 minutes, wait for the PVA to dry, tear it off along the edge and stick it to another SiO2 / Si substrate grown with MoS2, soak the transferred SiO2 / Si in water for 20 minutes to remove the PVA, and anneal it at 300°C for 0.5h to obtain the MoS2 moiré superlattice.
[0041] Example 3
[0042] A method for preparing a MoS2 moiré superlattice electrocatalyst comprises the following steps:
[0043] Step 1, SiO2 / Si substrate pretreatment: a bottom sheet with a size of 1 cm×0.7 cm and a top sheet with a size of 1 cm×1.8 cm were ultrasonically cleaned in acetone, isopropanol and anhydrous ethanol for 10 min respectively, and then dried with nitrogen;
[0044] Step 2, use a pipette to draw 2.5 μl of 10 mg / ml (NH4)2MoO4 solution and 1 μl of 5 mg / ml NaCl solution onto the bottom film, place it in an oven at 50°C for 4 min, then place the bottom film in a quartz boat, turn the top film upside down on the boat, and place the quartz boat in the center of the tube furnace;
[0045] 900 mg of sulfur powder was piled on a quartz tile, and the quartz tile was placed in a sleeve. The sleeve was then placed in a tube furnace and argon gas with a flow rate of 200 sccm was introduced for 30 minutes. The tube furnace was then heated to 700°C at a heating rate of 40°C / min. After growing for 15 minutes, it was naturally cooled to room temperature, and MoS2 was deposited on the top sheet.
[0046] Two groups of MoS2 grown on SiO2 / Si substrates were prepared in parallel;
[0047] Step 3, take 5g PVA particles and 1g glycerol, add them to 100mL deionized water, stir thoroughly with a glass rod until PVA is completely dissolved in the deionized water to obtain a PVA solution; drop the PVA solution onto the SiO2 / Si substrate grown with MoS2, place it on a heating table to cure for 9 minutes, wait for the PVA to dry, tear it off along the edge and stick it to another SiO2 / Si substrate grown with MoS2, soak the transferred SiO2 / Si in water for 25 minutes to remove the PVA, and anneal it at 300°C for 0.8h to obtain the MoS2 moiré superlattice.
[0048] Example 4
[0049] A method for preparing a MoS2 moiré superlattice electrocatalyst comprises the following steps:
[0050] Step 1, SiO2 / Si substrate pretreatment: a bottom sheet with a size of 1 cm×0.7 cm and a top sheet with a size of 1 cm×1.8 cm were ultrasonically cleaned in acetone, isopropanol and anhydrous ethanol for 10 min respectively, and then dried with nitrogen;
[0051] Step 2, use a pipette to pipette 2 μl of 5 mg / ml (NH4)2MoO4 solution and 1 μl of 5 mg / ml NaCl solution onto the bottom film, place it in an oven at 50°C for 5 min, then place the bottom film in a quartz boat, turn the top film upside down on the boat, and place the quartz boat in the center of the tube furnace;
[0052] 360 mg of sulfur powder was piled on a quartz tile, and the quartz tile was placed in a sleeve. The sleeve was then placed in a tube furnace and argon gas with a flow rate of 150 sccm was introduced for 30 minutes. The tube furnace was then heated to 800°C at a heating rate of 30°C / min. After growing for 15 minutes, it was naturally cooled to room temperature, and MoS2 was deposited on the top sheet.
[0053] Two groups of MoS2 grown on SiO2 / Si substrates were prepared in parallel;
[0054] Step 3, take 5g PVA particles and 1g glycerol, add them to 100mL deionized water, stir thoroughly with a glass rod until PVA is completely dissolved in the deionized water to obtain a PVA solution; drop the PVA solution onto the SiO2 / Si substrate grown with MoS2, place it on a heating table to cure for 10 minutes, wait for the PVA to dry, tear it off along the edge and stick it to another SiO2 / Si substrate grown with MoS2, soak the transferred SiO2 / Si in water for 30 minutes to remove the PVA, and anneal it at 300°C for 0.5h to obtain the MoS2 moiré superlattice.
[0055] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a MoS2 moiré superlattice electrocatalyst, characterized in that: The following steps are involved: Step 1: Use a pipette to pipette 2-3 μl of 2.5-10 mg / ml (NH4)MoO4 solution and 1 μl of 5 mg / ml NaCl solution onto the bottom film, place it in an oven to dry, then place the bottom film in a quartz boat, then turn the top film upside down on the boat, and place the quartz boat in the center of the tube furnace; the bottom film and the top film are SiO2 / Si substrates; Take excess sulfur powder and pile it in a quartz tile, place it upstream of the tube furnace, place the SiO2 / Si substrate downstream of the tube furnace, use argon as carrier gas, and prepare MoS2 on the surface of the SiO2 / Si substrate by chemical vapor deposition. The temperature of the tube furnace is raised to 700℃-900℃ at a heating rate of 30-50℃ / min, and ventilation and heat preservation are continued for 5-20min. After completion, it is naturally cooled to room temperature and the sample is taken out; Two groups of MoS2 grown on SiO2 / Si substrates were prepared in parallel; Step 2: Use the PVA transfer method to transfer the MoS2 grown on one of the SiO2 / Si substrates prepared in step 1 to another SiO2 / Si substrate with MoS2, and anneal at 300°C for 0.5-1h to obtain a MoS2 moiré superlattice.
2. The method for preparing the MoS2 moiré superlattice electrocatalyst according to claim 1, characterized in that: The SiO2 / Si substrate is ultrasonically cleaned in acetone, isopropanol, anhydrous ethanol and deionized water respectively before use and then dried.
3. The method for preparing the MoS2 moiré superlattice electrocatalyst according to claim 1, characterized in that: The quartz boat and the quartz tile are respectively ultrasonically cleaned in acetone, isopropanol, anhydrous ethanol and deionized water before use and then dried.
4. The method for preparing the MoS2 moiré superlattice electrocatalyst according to claim 1, characterized in that: The drying described in step 1 is to place it in an oven at 50° C. for 3-5 minutes.
5. The method for preparing the MoS2 moiré superlattice electrocatalyst according to claim 1, characterized in that: The flow rate of the carrier gas is 50-200 sccm.
6. The method for preparing the MoS2 moiré superlattice electrocatalyst according to claim 1, characterized in that: The specific operation of the PVA transfer method is as follows: take 5g of PVA particles and 1g of glycerol and add them to 100mL of deionized water, stir thoroughly with a glass rod until PVA is completely dissolved in the deionized water to form a solution; drop the PVA solution on a SiO2 / Si substrate with MoS2, heat and cure the PVA on a heating table, and the heating time is 8-10min; after curing, transfer the film to another SiO2 / Si substrate with MoS2 to obtain a MoS2 moiré superlattice, and finally soak it in deionized water for 20-30min to remove the PVA.
7. A MoS2 moiré superlattice electrocatalyst prepared by the method as described in any one of claims 1 to 6.
8. An application of the MoS2 moiré superlattice electrocatalyst as claimed in claim 7 in hydrogen production by electrolysis of water.