Composite catalyst with adjustable atomic distance as well as preparation method and application of composite catalyst
By growing nickel hydroxide on the surface of nickel foam and etching ZIF-67 with ferrous iron ions to prepare amorphous cobalt iron hydroxide, combined with Nafion solution to form a porous film layer, and adjusting the catalyst spacing, solving the problem of catalyst spacing in the existing technology Problems that are difficult to control, high reactivity and stability are achieved, and are suitable for electrocatalysis and new material development.
Patent Information
- Application Number
- CN202410613467.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-17
- Publication Date
- 2024-10-25
AI Technical Summary
It is difficult to effectively construct catalysts with different atomic spacings with existing technology, which limits the development and industrial-scale application of oxygen evolution reaction catalysts. Especially in nickel iron hydroxide catalysts, the Ni-O-Fe structure inhibits the formation of nickel hydroxide. active.
By growing nickel hydroxide on the surface of nickel foam and etching ZIF-67 with ferrous iron ions, amorphous cobalt iron hydroxide is prepared, combined with Nafion solution to form a porous film layer, and the amorphous cobalt iron hydroxide and hydroxide are adjusted. The spacing of nickel can construct a composite catalyst with adjustable atomic spacing.
It achieves high reactivity and stability of the catalyst, significantly reduces the overpotential of the oxygen evolution reaction of electrolyzed water, is suitable for electrocatalysis and new material development, and has industrial application potential.
Smart Images

Figure CN118835265A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a composite catalyst with adjustable atomic spacing, a preparation method and application thereof. Background Art
[0002] The over-exploitation and use of traditional fossil energy has caused problems such as climate deterioration and environmental pollution. Therefore, improving energy conversion efficiency and developing new energy sources are of great significance to alleviating environmental problems. Hydrogen energy is green and pollution-free, with high energy density (about 120MJ kg -1 ) and renewable characteristics have attracted widespread attention. Electrochemical technology has the characteristics of mild reaction conditions, pollution-free reaction process and high product purity, and is an ideal way to produce hydrogen. However, the efficiency of water electrolysis is affected by the hydrogen evolution reaction on the cathode side and the oxygen evolution reaction on the anode side. Therefore, reducing the theoretical overpotential of the reactions on both sides is of great significance to improving the overall water splitting efficiency. The multi-step proton-electron transfer process causes the overpotential of the oxygen evolution reaction to be much larger than the overpotential of the hydrogen evolution reaction. Therefore, reducing the overpotential of the oxygen evolution reaction is of great significance to improving the overall water splitting efficiency. The hydroxide composed of 3d group transition metals nickel (Ni) and iron (Fe) exhibits excellent oxygen evolution reaction performance due to its high metal element tunability and ultra-high specific surface area. The source of its activity is that under an applied voltage, nickel hydroxide and iron hydroxide are converted into active substances of nickel oxyhydroxide and iron oxyhydroxide. However, there are still some controversies in the study of the oxygen evolution reaction mechanism of nickel-iron hydroxide. Under the action of continuous oxidizing voltage, the oxygen in the electrocatalyst was replaced by oxygen isotope labeling, and it was found that the 16 / 18 O can react with 18 / 16 O exchange occurs, while NiFe hydroxide does not 18 / 16 O exchange, which indicates that the formation of Ni-O-Fe structure will inhibit the participation of lattice oxygen in the reaction of nickel hydroxide and reduce the intrinsic activity of nickel hydroxide.
[0003] Studies have shown that it is of great significance to reduce the overpotential of the oxygen evolution reaction by constructing catalysts with different atomic spacings and utilizing the synergistic effects between different sites to reduce the reaction energy barrier of the deprotonation step during the reaction. However, the controllable construction of catalysts with different atomic spacings is difficult, which is not conducive to the development of oxygen evolution reaction catalysts for industrial-scale application.
[0004] In view of this, the object of the present invention is to provide a new process for constructing a composite catalyst with adjustable atomic spacing to solve the above technical problems. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for constructing a composite catalyst with adjustable atomic spacing. By changing the spacing between amorphous cobalt iron hydroxide and nickel hydroxide, the prepared catalyst has the characteristics of high reaction activity and good stability; and the construction method is simple and can be applied on a large scale.
[0006] The first aspect of the present invention is to provide a method for preparing a composite catalyst with adjustable atomic spacing, and the technical scheme thereof is as follows:
[0007] A method for preparing a composite catalyst with adjustable atomic spacing comprises the following steps:
[0008] Step S1, using nickel foam as a substrate, and growing crystalline nickel hydroxide with a lamellar structure on the surface of the nickel foam by a hydrothermal method to obtain nickel foam-loaded nickel hydroxide;
[0009] Step S2, etching ZIF-67 with divalent iron ions to obtain amorphous cobalt iron hydroxide;
[0010] Step S3, dispersing an appropriate amount of Nafion solution on the surface of the nickel hydroxide supported by the nickel foam in step S1, and forming a Nafion membrane layer after drying;
[0011] Step S4, dispersing the amorphous cobalt iron hydroxide of step S2 in a Nafion solution, and then dispersing it on the surface of the nickel hydroxide supported by the nickel foam of step S3 to obtain the nickel hydroxide supported amorphous cobalt iron hydroxide;
[0012] The amorphous cobalt iron hydroxide and the nickel hydroxide maintain a non-bonded state and have a certain distance therebetween, and the distance between the amorphous cobalt iron hydroxide and the nickel hydroxide is adjusted by controlling the amount of Nafion.
[0013] Further, in step S1, the reaction temperature of the hydrothermal method is 90-110°C, and the reaction time is 9-11h. Specifically, the reaction temperature can be 90°C, 95°C, 100°C, 105°C or 110°C, or other values within the range; the reaction time can be 9h, 10h or 11h, or other values within the range.
[0014] Furthermore, step S1 includes the following steps:
[0015] Step S11, cutting the nickel foam into a suitable size and performing pretreatment;
[0016] Step S12, dissolving an appropriate amount of hexamethylenetetramine and nickel nitrate hexahydrate in an aqueous solution, wherein the mass concentration of the solution is 0.02-0.04 g mL -1 , the mass ratio of hexamethylenetetramine to nickel nitrate hexahydrate is 0.7-1.3:1;
[0017] Specifically, the mass concentration of the solution can be 0.02 g mL -1 , 0.03g mL -1 or 0.04 g mL -1 , or other values within this range; the mass ratio of hexamethylenetetramine to nickel nitrate hexahydrate may be 0.7:1, 0.8:1, 0.9:1, 1.0:1, 1.2:1 or 1.3:1, or other values within this range.
[0018] Step S13, placing the nickel foam obtained in step S11 and the mixed solution obtained in step S12 into a reaction container for hydrothermal reaction to obtain nickel foam loaded with nickel hydroxide.
[0019] Furthermore, the method for preparing amorphous cobalt iron hydroxide in step S2 is as follows:
[0020] Appropriate amounts of ferrous chloride tetrahydrate and ZIF-67 are dispersed in methanol solution and mixed, and reacted at room temperature for 1-5 hours.
[0021] Furthermore, the mass ratio of ferrous chloride tetrahydrate to ZIF-67 is 1-4:1, and the concentration of the mixed solution is 0.001-0.02 g mL -1 Specifically, the mass ratio of ferrous chloride tetrahydrate to ZIF-67 can be 1:1, 2:1, 3:1 or 4:1, or other values within the range; the concentration of the mixed solution is 0.001 g mL -1 , 0.002gmL -1 , 0.005g mL -1 , 0.01g mL -1 , 0.015g mL -1 or 0.02 g mL -1 , or other values within this range.
[0022] Furthermore, in step S3, a Nafion solution with a mass concentration of 5%, ultrapure water and anhydrous ethanol are first mixed, and then the mixed solution is dispersed in trace amounts on the surface of the nickel hydroxide supported by the nickel foam multiple times;
[0023] The amount of Nafion solution with a mass concentration of 5% is calculated based on the area of nickel foam and is 0-100 μL cm -2 , and is not 0.
[0024] Furthermore, in step S4, appropriate amounts of amorphous cobalt iron hydroxide, Nafion solution, ultrapure water and anhydrous ethanol solution are first mixed, and then the mixed solution is dispersed on the surface of the nickel hydroxide supported by the nickel foam.
[0025] Furthermore, the loading amount of amorphous cobalt iron hydroxide is 0.2-5 mg cm-3 based on the area of nickel foam. -2 .
[0026] The second aspect of the present invention is to provide a composite catalyst with adjustable atomic spacing, comprising nickel hydroxide supported on nickel foam, a Nafion film layer formed on the surface of the nickel hydroxide supported on nickel foam, and amorphous cobalt iron hydroxide dispersed on the surface of the nickel hydroxide supported on nickel foam, wherein the amorphous cobalt iron hydroxide and the nickel hydroxide are kept in a non-bonded state and have a certain spacing, and the spacing between the amorphous cobalt iron hydroxide and the nickel hydroxide is adjusted by controlling the amount of Nafion used.
[0027] The third aspect of the present invention is to provide an application of the composite catalyst with adjustable atomic spacing as described in the second aspect in an electrocatalytic reaction.
[0028] Compared with the prior art, the composite catalyst with adjustable atomic spacing provided by the present invention and its preparation method and application have the following beneficial effects:
[0029] 1. The composite catalyst with adjustable atomic spacing provided by the present invention uses Nafion solution as a diaphragm and adhesive, and while inhibiting the bonding of amorphous cobalt iron hydroxide and nickel hydroxide, a porous Nafion membrane layer of different thicknesses is formed by adjusting the amount of Nafion solution added, thereby changing the spacing between amorphous cobalt iron hydroxide and nickel hydroxide. The composite material nickel hydroxide loaded with amorphous cobalt iron hydroxide has the characteristics of high reactivity and good stability. It is used as an oxygen evolution reaction catalyst, and under alkaline conditions, the overpotential of the oxygen evolution reaction in electrolysis of water can be significantly reduced.
[0030] 2. The composite catalyst with adjustable atomic distance provided by the present invention has a simple construction method and can be applied on a large scale.
[0031] 3. The composite catalyst with adjustable atomic spacing provided by the present invention has good catalytic performance and can be widely used in the development and application of new materials such as electrocatalysis and air batteries. It is an efficient and stable catalytic material. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0033] Figure 1 X-ray diffraction patterns of amorphous cobalt iron hydroxide and nickel hydroxide supported by nickel foam prepared in Example 1 of the present invention;
[0034] Figure 2 The scanning electron microscope images of the amorphous cobalt iron hydroxide and the nickel hydroxide supported by nickel foam prepared in Example 1 of the present invention;
[0035] Figure 3 A schematic diagram of the composite structure of the nickel hydroxide supported amorphous cobalt iron hydroxide catalyst prepared in Example 1 of the present invention;
[0036] Figure 4 The X-ray photoelectron spectrum of the nickel hydroxide-supported amorphous cobalt iron hydroxide catalyst prepared in Example 1 of the present invention before and after oxygen evolution reaction;
[0037] Figure 5 This is a polarization curve diagram of the nickel hydroxide-supported amorphous cobalt iron hydroxide catalyst prepared in Example 1 of the present invention in a 1M potassium hydroxide aqueous solution;
[0038] Figure 6 The nickel hydroxide supported amorphous cobalt iron hydroxide catalyst prepared in Example 1 of the present invention is 10mAcm -2 and 1A cm -2 Oxygen evolution reaction stability test diagram under
[0039] Figure 7 The actual gas production of the nickel hydroxide-supported amorphous cobalt iron hydroxide catalyst prepared in Example 1 of the present invention when the solar panel is used as the driving energy source;
[0040] Figure 8 Polarization curves of the nickel hydroxide-supported amorphous cobalt iron hydroxide catalyst prepared in Example 1 of the present invention at different spacings (different Nafion amounts). DETAILED DESCRIPTION
[0041] In order to enable those skilled in the art to better understand the technical solutions in the embodiments of the present invention and to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation modes of the present invention are further described below.
[0042] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0043] Example 1
[0044] A method for preparing a composite catalyst with adjustable atomic spacing comprises the following steps:
[0045] Step S1, using nickel foam as a substrate, growing crystalline nickel hydroxide with a lamellar structure on the surface of the nickel foam by a hydrothermal method to obtain nickel foam-loaded nickel hydroxide, the specific method is as follows:
[0046] Step S11, cutting the nickel foam into a size of 1 cm×2 cm, putting it into a beaker, adding an acetone solution that covers the nickel foam, and ultrasonicating overnight; then, cleaning the nickel foam treated with acetone, adding a 1M hydrochloric acid solution that covers the nickel foam, and ultrasonicating for 30 minutes; then, cleaning the nickel foam treated with hydrochloric acid multiple times with ultrapure water and anhydrous ethanol, and putting it into anhydrous ethanol for standby use after cleaning;
[0047] Step S12, dissolving an appropriate amount of hexamethylenetetramine and nickel nitrate hexahydrate in an aqueous solution, specifically weighing 1.5 g of hexamethylenetetramine and 1.6 g of nickel nitrate hexahydrate and dissolving them in 100 mL of ultrapure water;
[0048] Step S13, placing the nickel foam of step S11 and the mixed solution of step S12 into a reaction vessel for hydrothermal reaction to obtain nickel foam loaded with nickel hydroxide. Specifically, the reaction temperature is 110°C and the time is 10 hours. Stirring needs to be turned on during the reaction to ensure that the reaction solution is uniform, and the stirring speed cannot be too fast to prevent the nickel foam from being damaged; after the reaction is completed, the nickel foam is washed and dried with ultrapure water to obtain a nickel foam loaded with nickel hydroxide material.
[0049] Step S2, etching ZIF-67 with divalent iron ions to obtain amorphous cobalt iron hydroxide, the specific method is as follows:
[0050] About 0.2 g of ferrous chloride tetrahydrate and about 0.1 g of ZIF-67 were weighed, and 25 mL of methanol solution was added respectively and dispersed evenly; then, the two dispersed solutions were mixed, stirred and reacted at room temperature for 1 h, 3 h or 5 h. After the reaction was completed, the solution was centrifuged, the solid was collected and dried to obtain amorphous cobalt iron hydroxide.
[0051] Step S3, dispersing an appropriate amount of Nafion solution on the surface of the nickel hydroxide supported by the nickel foam in step S1, and forming a Nafion membrane layer after drying, the specific method is as follows:
[0052] Take a 5% Nafion solution (30 μL cm -2 For example), 300 μL of anhydrous ethanol and 300 μL of ultrapure water were added, and ultrasonic treatment was performed for 1 hour to obtain a uniformly dispersed Nafion solution. The uniformly dispersed Nafion solution was dispersed on the surface of nickel foam loaded with nickel hydroxide in trace amounts multiple times using a pipette to form a Nafion membrane layer with a porous structure;
[0053] In the present invention, the amount of Nafion solution with a mass concentration of 5% is calculated based on the area of the nickel foam and is 0-100 μL cm -2 , and is not 0. Specifically, the amount of Nafion solution added is 5 μL cm -2 , 10 μL cm -2 , 20 μL cm -2 , 30 μL cm -2 , 50 μL cm -2 , or 100 μL cm -2 By adjusting the amount of Nafion added, the construction of Nafion membrane layers of different thicknesses can be achieved.
[0054] Step S4, dispersing the amorphous cobalt iron hydroxide of step S2 in a Nafion solution, and then dispersing it on the surface of the nickel hydroxide supported by the nickel foam of step S3 to obtain the nickel hydroxide supported amorphous cobalt iron hydroxide, the specific method is as follows:
[0055] Weigh 1 mg of the amorphous cobalt iron hydroxide in step S2, add 10 μL of 5% mass concentration Nafion solution, 300 μL of ultrapure water and 300 μL of anhydrous ethanol, and ultrasonically treat for 1 hour to obtain a uniformly dispersed amorphous cobalt iron hydroxide dispersion. Use a pipette to disperse it in trace amounts on the surface of the nickel hydroxide in step S3 multiple times, and obtain nickel hydroxide-loaded amorphous cobalt iron hydroxide after drying.
[0056] The amorphous cobalt iron hydroxide and the nickel hydroxide maintain a non-bonded state and have a certain distance therebetween, and the distance between the amorphous cobalt iron hydroxide and the nickel hydroxide is adjusted by controlling the amount of Nafion.
[0057] Please refer to Figures 1 to 3 ,in Figure 1 X-ray diffraction patterns of amorphous cobalt iron hydroxide and nickel hydroxide supported by nickel foam prepared in Example 1 of the present invention; Figure 2 The scanning electron microscope images of the amorphous cobalt iron hydroxide and the nickel hydroxide supported by nickel foam prepared in Example 1 of the present invention; Figure 3 The composite structure diagram of the nickel hydroxide supported amorphous cobalt iron hydroxide catalyst prepared in Example 1 of the present invention. Figure 1 It can be seen that the amorphous cobalt iron hydroxide-t (t represents time in hours) after etching is an amorphous structure, and the nickel foam loaded with nickel hydroxide shows the characteristic peaks of nickel hydroxide and nickel foam; Figure 2It can be seen that as the etching time increases, the structure of the amorphous cobalt iron hydroxide is gradually destroyed, forming a three-dimensional hollow polyhedron structure, and the nickel foam loaded nickel hydroxide shows a lamellar structure of nickel hydroxide, indicating the successful preparation of amorphous cobalt iron hydroxide and nickel hydroxide. The element content of the amorphous cobalt iron hydroxide was analyzed by inductively coupled plasma emission spectrometry, and the test results are shown in Table 1:
[0058] Table 1: Inductively coupled plasma emission spectroscopy detection results of amorphous cobalt iron hydroxide catalyst
[0059]
[0060]
[0061] It can be seen from the data in Table 1 that with the increase of etching time, the content of cobalt element gradually decreases, and the content of iron element gradually increases.
[0062] Figure 3 Schematic diagram of the composite structure. The amorphous cobalt iron hydroxide and the nickel hydroxide are bonded by a Nafion membrane layer with a porous structure. The thickness of the Nafion membrane layer adjusts the distance between the amorphous cobalt iron hydroxide and the nickel hydroxide.
[0063] Please refer to Figure 4 , is the X-ray photoelectron spectrum of the nickel hydroxide-supported amorphous cobalt iron hydroxide catalyst prepared in Example 1 of the present invention before and after oxygen evolution reaction, wherein the oxygen evolution reaction is tested under a three-electrode system, the nickel hydroxide-supported amorphous cobalt iron hydroxide is used as the working electrode, the platinum sheet electrode and the silver / silver chloride electrode are used as the counter electrode and the reference electrode respectively, the tested solution is a 1M potassium hydroxide aqueous solution, and the test interval is 1.023V-1.723V (relative to the reversible hydrogen electrode). By Figure 4 It can be seen that before and after the reaction of amorphous cobalt iron hydroxide and nickel hydroxide, Fe 2p 3 / 2 and Ni 2p 3 / 2 The peak position of has basically not changed, that is, the electronic structure of Ni and Fe has basically not changed, indicating that no bonding occurs between Ni and Fe during the reaction, proving that Nafion can be used as a membrane to inhibit the bonding between Ni and Fe.
[0064] Please refer to Figure 5 , is a polarization curve of the nickel hydroxide-supported amorphous cobalt iron hydroxide catalyst prepared in Example 1 of the present invention in 1M potassium hydroxide aqueous solution. Figure 5 It can be seen that the electrochemical performance of amorphous cobalt iron hydroxide is optimal after etching for 3 hours, with a current density of 10 mA cm -2 and 100mA cm -2The overpotentials were only 207 mV and 271 mV, indicating that nickel hydroxide-loaded amorphous cobalt iron hydroxide has excellent electrochemical properties under alkaline conditions.
[0065] Please refer to Figure 6 , is the nickel hydroxide supported amorphous cobalt iron hydroxide catalyst prepared in Example 1 of the present invention at 10 mA cm -2 and 1A cm -2 Oxygen evolution reaction stability test diagram under Figure 6 It can be seen that when the applied voltage is 1.48 V (relative to reversible hydrogen), the current density is basically 10 mA cm -2 It can run stably for about 24 hours. When the applied voltage is 2.43V (relative to reversible hydrogen), the current density is basically 1A cm -2 The results show that the composite catalyst of the present invention can achieve a higher current density at a lower voltage and has a higher stability, indicating that it has excellent prospects for industrial application.
[0066] Please refer to Figure 7 , is the actual gas production of the nickel hydroxide-supported amorphous cobalt iron hydroxide catalyst prepared in Example 1 of the present invention when the solar panel is used as the driving energy source. The actual hydrogen and oxygen production using the solar panel (output voltage of 2.35V) as the driving energy source was evaluated using a two-electrode system. The oxygen production was about 0.42mL min in 60 minutes. -1 , the hydrogen production is about 0.82mL min -1 In the process of electrolyzing water using solar panels directly as energy, the composite catalyst of the present invention can reduce the loss caused by multiple energy conversions and improve the efficiency of energy utilization, further indicating that the composite catalyst of the present invention has practical application prospects.
[0067] Please refer to Figure 8 , are polarization curves of the nickel hydroxide-supported amorphous cobalt iron hydroxide catalyst prepared in Example 1 of the present invention at different spacings (different Nafion amounts). By changing the amount of Nafion dispersed on the nickel hydroxide supported by the foam nickel in step S3 for the first time (0 μL cm -2 , 5 μL cm -2 , 10 μL cm -2 , 20 μL cm -2 , 30 μL cm -2 , 50 μL cm -2 and 100 μL cm -2), forming a porous Nafion membrane structure with different thicknesses, and then the amorphous cobalt iron hydroxide in step S4 is loaded on the nickel hydroxide with different thicknesses of the Nafion membrane layer, so as to achieve the purpose of regulating the distance between the amorphous cobalt iron hydroxide and the nickel hydroxide. Figure 8 It can be seen that the amount of Nafion added is from 0 μL cm -2 to 100 μL cm -2 The oxidation potential and oxygen evolution reaction starting potential of nickel hydroxide show a trend of first decreasing and then increasing. Figure 8 Point A represents the oxidation site of nickel hydroxide, and point B represents the starting site of oxygen evolution reaction. The results show that adjusting the thickness of the Nafion membrane layer can change the electrochemical oxygen evolution characteristics, proving that the Nafion membrane layer formed by the Nafion solution is effective in regulating the atomic spacing. In the present invention, the amount of 5% Nafion solution is calculated as 30 μL cm based on the area of the nickel foam. -2 It should be noted that the Nafion membrane thickness of 0 μL means that no Nafion solution is added to the surface of nickel hydroxide supported by nickel foam.
[0068] The composite catalyst of amorphous cobalt iron hydroxide and nickel foam loaded nickel hydroxide has good electrochemical oxygen evolution performance under alkaline conditions. During the reaction, Fe in the amorphous cobalt iron hydroxide 3+ -O can form intermolecular hydrogen bonds with the reaction intermediates on nickel hydroxide in nickel foam-supported nickel hydroxide (*OOH on nickel hydroxide), accelerating the deprotonation process. However, the construction of intermolecular hydrogen bonds requires the regulation of the intermolecular distance. Too close a distance is not conducive to the construction of intermolecular hydrogen bonds, and too far a distance is not conducive to the function of hydrogen bonds. Therefore, a certain distance is created between amorphous cobalt iron hydroxide and nickel foam-supported nickel hydroxide by using Nafion membrane layers of different thicknesses, thereby improving the electrochemical oxygen evolution performance of the composite material.
[0069] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations made to these embodiments without departing from the principles and spirit of the present invention are still within the protection scope of the present invention.
Claims
1. A method for preparing a composite catalyst with adjustable atomic spacing, It is characterized in that The steps include: Step S1, using nickel foam as a substrate, and growing crystalline nickel hydroxide with a lamellar structure on the surface of the nickel foam by a hydrothermal method to obtain nickel foam-loaded nickel hydroxide; Step S2, etching ZIF-67 with divalent iron ions to obtain amorphous cobalt iron hydroxide; Step S3, dispersing an appropriate amount of Nafion solution on the surface of the nickel hydroxide supported by the nickel foam in step S1, and forming a Nafion membrane layer after drying; Step S4, dispersing the amorphous cobalt iron hydroxide of step S2 in a Nafion solution, and then dispersing it on the surface of the nickel hydroxide supported by the nickel foam of step S3 to obtain the nickel hydroxide supported amorphous cobalt iron hydroxide; The amorphous cobalt iron hydroxide and the nickel hydroxide maintain a non-bonded state and have a certain distance therebetween, and the distance between the amorphous cobalt iron hydroxide and the nickel hydroxide is adjusted by controlling the amount of Nafion.
2. The method for preparing the composite catalyst with adjustable atomic spacing according to claim 1, It is characterized in that In step S1, the reaction temperature of the hydrothermal method is 90-110° C., and the reaction time is 9-11 h.
3. The method for preparing the composite catalyst with adjustable atomic spacing according to claim 2, It is characterized in that Step S1 includes the following steps: Step S11, cutting the nickel foam into a suitable size and performing pretreatment; Step S12, dissolving an appropriate amount of hexamethylenetetramine and nickel nitrate hexahydrate in an aqueous solution, wherein the mass concentration of the solution is 0.02-0.04 g mL -1 , the mass ratio of hexamethylenetetramine to nickel nitrate hexahydrate is 0.7-1.3:1; Step S13, placing the nickel foam obtained in step S11 and the mixed solution obtained in step S12 into a reaction container for hydrothermal reaction to obtain nickel foam loaded with nickel hydroxide.
4. The method for preparing the composite catalyst with adjustable atomic spacing according to claim 1, It is characterized in that The method for preparing amorphous cobalt iron hydroxide in step S2 is as follows: Appropriate amounts of ferrous chloride tetrahydrate and ZIF-67 are dispersed in methanol solution and mixed, and reacted at room temperature for 1-5 hours.
5. The method for preparing the composite catalyst with adjustable atomic spacing according to claim 4, It is characterized in that The mass ratio of ferrous chloride tetrahydrate to ZIF-67 is 1-4:1, and the concentration of the mixed solution is 0.001-0.02 g mL based on ZIF-67. -1 .
6. The method for preparing the composite catalyst with adjustable atomic spacing according to claim 1, It is characterized in that In step S3, a Nafion solution with a mass concentration of 5%, ultrapure water and anhydrous ethanol are first mixed, and then the mixed solution is dispersed in trace amounts on the surface of the nickel hydroxide supported by the nickel foam multiple times; The amount of Nafion solution with a mass concentration of 5% is calculated based on the area of nickel foam and is 0-100 μL cm -2 , and is not 0.
7. The method for preparing the composite catalyst with adjustable atomic spacing according to claim 1, It is characterized in that In step S4, appropriate amounts of amorphous cobalt iron hydroxide, Nafion solution, ultrapure water and anhydrous ethanol solution are first mixed, and then the mixed solution is dispersed on the surface of the nickel hydroxide supported by the nickel foam.
8. The method for preparing the composite catalyst with adjustable atomic spacing according to claim 1, It is characterized in that The loading amount of amorphous cobalt iron hydroxide was 0.2–5 mg cm based on the area of nickel foam. -2 .
9. A composite catalyst with adjustable atomic spacing, It is characterized in that The invention comprises nickel hydroxide supported on nickel foam, a Nafion film layer formed on the surface of nickel hydroxide supported on nickel foam, and amorphous cobalt iron hydroxide dispersed on the surface of nickel hydroxide supported on nickel foam. The amorphous cobalt iron hydroxide and nickel hydroxide are kept in a non-bonded state and have a certain distance therebetween, and the distance between the amorphous cobalt iron hydroxide and nickel hydroxide is adjusted by controlling the dosage of Nafion.
10. Use of the composite catalyst with adjustable atomic spacing as claimed in claim 7 in an electrocatalytic reaction.