Stretchable alternating current electroluminescent device and preparation method thereof
By covering the surface of zinc sulfide with a coating structure of small molecule fluorescent dyes and a combination of elastic polymers, the problem of color and flexibility limitations of AC electroluminescent devices is solved, and the preparation of stretchable AC electroluminescent devices with adjustable The characteristics of luminous color and high mechanical strength are suitable for wearable electronic products.
Patent Information
- Application Number
- CN202410932847.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-25
AI Technical Summary
Existing AC electroluminescent devices have limitations in color capabilities and driving voltage, making it difficult to achieve high flexibility and color display, and the preparation process is complex, which limits their application in wearable electronic products.
Using a coating structure in which the surface of zinc sulfide (ZnS) is covered with a small molecule fluorescent dye, combined with an elastic polymer and a polar solvent, the coating of the phosphor and the preparation of the electrode layer are achieved through a simple solution method to form a stretchable AC electroluminescent device. .
It achieves the adjustability of the luminescent color from green to red, improves the stretchability and mechanical strength of the device, simplifies the preparation process, reduces the cost, and is suitable for large-scale industrial production.
Smart Images

Figure CN118843221A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of light-emitting devices, and in particular to a stretchable alternating current electroluminescent device and a preparation method thereof. Background Art
[0002] Wearable electronics with mechanical deformability and multifaceted intelligent capabilities have experienced rapid development and have had a wide impact on our daily lives. Visual displays, as a core component of information dissemination, have become the main medium for information dissemination. Wearable displays have obvious advantages such as elasticity, even stretchability, portability, deformability, and skin adaptability, thereby improving convenience and comfort. Various display technologies have been developed, including liquid crystal displays (LCDs), organic light-emitting diodes (OLEDs), quantum dot light-emitting diodes (QLEDs), perovskite light-emitting diodes (PeLEDs), and alternating current electroluminescent devices (ACELs). Non-self-emissive liquid crystal displays are the main force of contemporary display technology due to their advantages such as long life, high resolution, high cost performance, and high brightness. However, the rigidity of color filters and backlight sources severely limits the flexibility of LCDs. In recent years, self-emissive displays have made considerable progress, especially in terms of wider color gamut, more vivid colors, and better flexibility. However, their intrinsic instability of emitting materials requires strict environmental control, such as inert gas atmosphere, low humidity, and low temperature. In addition, these devices impose strict requirements on the working function of electrodes to achieve balanced charge injection. This high dependence on equipment and materials significantly increases manufacturing costs and complexity.
[0003] In contrast, AC electroluminescent devices have been explored as viable contenders for evolving wearable displays due to their simple fabrication, superior deformation performance, low power consumption, and long lifetime. However, limited color capabilities and high driving AC voltages have significantly hampered their development. The full width at half maximum (FWHM) of the excitation light of the phosphors in commercial AC electroluminescent devices is greater than 50 nm, and the color region is limited from blue to orange, which means the color gamut is limited. In addition, the electroluminescent performance of orange phosphors is significantly inferior to that of blue and green phosphors, thus hindering the overall integration of full-color displays.
[0004] Small molecule fluorescent dyes are considered as promising color conversion layers for flexible pure color AC electroluminescent devices due to their high absorption coefficient, high photoluminescence quantum yield, and narrow full width at half maximum. Nevertheless, challenges still exist in realizing ultrathin, stretchable, large-area, and color displays for wearable electronics due to the complex multi-layer phosphor encapsulation structure. Summary of the invention
[0005] The purpose of the present invention is to design a stretchable AC electroluminescent device and a preparation method thereof in order to solve the above problems.
[0006] The present invention achieves the above-mentioned purpose through the following technical solutions: The stretchable AC electroluminescence is characterized in that it includes an upper electrode layer, an electroluminescent layer and a lower electrode layer from top to bottom, and the electroluminescent layer is a coating structure in which the surface of zinc sulfide ZnS is covered with a small molecule fluorescent dye.
[0007] A method for preparing a stretchable AC electroluminescent device, comprising: S1. Soak the ZnS particles in a mixed solution of concentrated sulfuric acid and hydrogen peroxide, wash them with deionized water, and store them in a constant temperature drying oven; S2, placing ZnS in an anhydrous ethanol solution containing a silane coupling agent and stirring, washing it with anhydrous ethanol and then drying it with nitrogen; S3, adding ZnS to a polar solvent containing a small molecule fluorescent dye, stirring, washing with an anhydrous ethanol solution, and storing in a constant temperature drying oven to obtain a phosphor with a ZnS / small molecule fluorescent dye coating structure; S4, cleaning the three Si / SiO2 wafers with deionized water, isopropyl alcohol, and acetone solution, drying them with nitrogen gas, and storing them in a constant temperature drying oven; S5, after UVO treatment of the surfaces of two Si / SiO2 wafers, any one of PDMS, SEBS, and TPU is spin-coated, printed, or sprayed on the surface of the Si / SiO2 wafer, and thermally annealed to form a stretchable substrate; S6, after the stretchable substrate is subjected to UVO treatment, PEDOT:PSS or silver nanowire solution is spin-coated, printed or sprayed on the surface of the stretchable substrate, and then peeled off from the surface of the Si / SiO2 wafer after secondary annealing to form an upper electrode layer and a lower electrode layer; S7, mixing the phosphor of the ZnS / small molecule fluorescent dye encapsulated structure with the elastic polymer, spin coating, printing or spraying on the surface of another Si / SiO2 wafer, and peeling off from the surface of the Si / SiO2 wafer after annealing to obtain an electroluminescent layer; S8. After the electroluminescent layer, the upper electrode layer and the lower electrode layer are subjected to plasma surface treatment, the upper electrode layer and the lower electrode layer are attached to the upper and lower surfaces of the electroluminescent layer respectively, and after being pressed by a press, the stretchable AC electroluminescent device as described above is obtained.
[0008] The beneficial effects of the present invention are as follows: an innovative and simple solution method is used to achieve efficient coating of ZnS with small molecule fluorescent dyes, the preparation steps are simple and convenient, and large-scale industrial production can be realized, which brings great convenience to practical applications; by cleverly regulating the concentration of small molecule fluorescent dyes in polar solutions, precise adjustment of the surface thickness of ZnS is achieved, thereby precisely controlling the photon reabsorption and fluorescence resonance energy transfer efficiency, and achieving adjustable luminescent color from green to red; an elastic polymer is uniquely used as a substrate material to tightly combine the upper and lower electrode layers with the electroluminescent layer, thereby achieving the stretchability of the device while maintaining excellent mechanical strength, which is a perfect combination of practicality and stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 is a schematic structural diagram of a stretchable AC electroluminescent device of the present invention; Figure 2 is an experimental mechanism diagram of steps (1)-(3) in Example 2; Figure 3 The AC electroluminescence of the ZnS phosphor and the absorption and emission spectra of the small molecule fluorescent dye DCJTB in Example 2; Figure 4 is a CIE coordinate change diagram of the stretchable AC electroluminescent device in Examples 1-4; The corresponding figures are as follows: 1-transparent stretchable upper thin film electrode, 2-stretchable electroluminescent layer, 3-transparent stretchable lower thin film electrode. DETAILED DESCRIPTION
[0010] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0011] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0012] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0013] In the description of the present invention, it should be understood that the terms "upper", "lower", "inside", "outside", "left", "right", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, or are directions or positional relationships in which the product of the invention is usually placed when in use, or are directions or positional relationships commonly understood by those skilled in the art. These directions or positional relationships are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present invention.
[0014] Furthermore, the terms “first”, “second”, etc. are merely used for distinguishing descriptions and are not to be understood as indicating or implying relative importance.
[0015] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms such as "setting" and "connection" should be understood in a broad sense. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0016] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings.
[0017] The stretchable AC electroluminescent device comprises an upper electrode layer, an electroluminescent layer and a lower electrode layer from top to bottom. The electroluminescent layer is a coating structure in which the surface of zinc sulfide ZnS is covered with a small molecule fluorescent dye.
[0018] The zinc sulfide ZnS is a 50-micron particle surface-treated with a silane coupling agent. The methoxy group and cyano group in the small molecule fluorescent dye are paired with the amino group in the silane coupling agent to be wrapped and fixed on the surface of the zinc sulfide ZnS.
[0019] The upper electrode layer and the lower electrode layer are transparent stretchable thin film electrodes formed by PEDOT:PSS or silver nanowires coated on elastic polymers, with a thickness ranging from 0.05-1 mm.
[0020] A method for preparing a stretchable AC electroluminescent device, comprising: S1. After soaking 50 μm ZnS particles in a mixed solution of concentrated sulfuric acid and 30% hydrogen peroxide in a mass ratio of 7:3 for 2 hours, the particles were washed with deionized water and stored in a constant temperature drying oven; S2, placing ZnS in an anhydrous ethanol solution containing a silane coupling agent with a concentration range of 5-100 mM and stirring for 1-2 hours, washing with anhydrous ethanol and drying with nitrogen, wherein the silane coupling agent is one of APTMS or APTES; S3, adding ZnS to a polar solvent containing a small molecule fluorescent dye with a concentration range of 5-100 mg / ml, stirring, washing with an anhydrous ethanol solution and storing in a constant temperature drying oven to obtain a phosphor with a ZnS / small molecule fluorescent dye coating structure, wherein the small molecule fluorescent dye is DCJTB or rhodamine, and the polar solvent is one of chloroform, ethyl acetate, dichloromethane and DMF; S4, cleaning the three Si / SiO2 wafers with deionized water, isopropyl alcohol, and acetone solution, drying them with nitrogen gas, and storing them in a constant temperature drying oven; S5. After UVO treatment is performed on the surfaces of two Si / SiO2 wafers, any one of PDMS, SEBS, and TPU is spin-coated, printed, or sprayed on the surface of the Si / SiO2 wafer, and thermally annealed to form a stretchable substrate with a thickness of 0.05-1 mm; S6, after the stretchable substrate is subjected to UVO treatment for 15-30 minutes, a PEDOT:PSS solution with a concentration of 0.5-5% wt% or a silver nanowire solution with a concentration of 10-100 mg / ml is spin-coated, printed or sprayed on the surface of the stretchable substrate, and then secondary annealed at 110-150° C. for 5-30 minutes and then peeled off from the surface of the Si / SiO2 wafer to form an upper electrode layer and a lower electrode layer; S7, mixing the phosphor of the ZnS / small molecule fluorescent dye encapsulated structure with the elastic polymer in a ratio of 10-50% wt%, spin coating, printing or spraying on the surface of another Si / SiO2 wafer, annealing at 80-110° C. for 1-2 hours, and then peeling off from the surface of the Si / SiO2 wafer to obtain an electroluminescent layer with a thickness of 0.05-1 mm; S8. After the electroluminescent layer, the upper electrode layer and the lower electrode layer are subjected to plasma surface treatment, the upper electrode layer and the lower electrode layer are attached to the upper and lower surfaces of the electroluminescent layer respectively, and after being pressed by a press, the stretchable AC electroluminescent device as described above is obtained.
[0021] Under the action of high-frequency AC electric field, ZnS particles produce charge polarization, which causes electrons to undergo energy transition and eventually release green light with a wavelength of 510 nm. The absorption peak of small molecule fluorescent dyes such as DCJTB or rhodamine is located at 510 nm. Through the combined action of photon reabsorption and fluorescence resonance energy transfer, the small molecule fluorescent dye absorbs the excitation energy generated in ZnS, realizing the photoluminescence of the small molecule fluorescent dye. By adjusting the ratio of ZnS to the small molecule fluorescent dye, it is finally possible to achieve narrow half-width light emission while showing spectral tunability. This stretchable AC electroluminescent device based on ZnS / small molecule fluorescent dye coated structure phosphor realizes adjustable luminescent color and can be used for interactive skin displays and intelligent soft robots.
[0022] Control group 1: (1) After soaking ZnS particles with a particle size of 50 μm in a solution of concentrated sulfuric acid and 30% hydrogen peroxide in a mass ratio of 7:3 for 1 hour, the particles were washed with deionized water and stored in a constant temperature drying oven; (2) Place ZnS in an anhydrous ethanol solution containing APTMS (5 mM) and stir for 1 hour, wash with anhydrous ethanol and blow dry with nitrogen; (3) Add ZnS to chloroform without small molecule fluorescent dye, stir for 1 hour, wash with anhydrous ethanol solution and store in a constant temperature drying oven; (4) Clean the Si / SiO2 wafer with deionized water, isopropanol, and acetone solution, blow dry with nitrogen, and store in a constant temperature drying oven; (5) After the Si / SiO2 wafer surface is subjected to UVO treatment for 15 minutes, PDMS is spin-coated, printed or sprayed on the Si / SiO2 wafer surface, and then thermally annealed at 80°C for 1 hour to form a stretchable substrate; (6) After the stretchable substrate was UVO treated for 15 minutes, PEDOT:PSS (0.5 wt%, aqueous solution) was spin-coated on the surface of the stretchable substrate at 3000 rpm, and then secondary annealed at 110 °C for 5 minutes and peeled off from the surface of the Si / SiO2 wafer to form a transparent stretchable thin film electrode; (7) ZnS phosphor was mixed with PDMS at 30% wt%, and then spin-coated on the surface of Si / SiO2 wafer at 500 rpm. After annealing at 80 °C for 1 hour, the mixture was peeled off from the surface of Si / SiO2 wafer to obtain a stretchable electroluminescent layer.
[0023] (8) After the stretchable electroluminescent layer and the transparent stretchable thin film electrode are subjected to plasma surface treatment, a transparent stretchable thin film electrode is attached to the upper and lower surfaces of the stretchable electroluminescent layer, and the layers are pressed by a press to obtain a stretchable AC electroluminescent device based on ZnS phosphor.
[0024] Embodiment 1: The difference from control group 1 is that in step (3), ZnS is added to chloroform containing DCJTB (5 mg / ml), stirred for 1 hour, washed with anhydrous ethanol solution and stored in a constant temperature drying oven, and in step (8), a stretchable AC electroluminescent device based on ZnS / DCJTB coated structure phosphor is obtained.
[0025] Embodiment 2: The difference from control group 1 is that in step (3), ZnS is added to chloroform containing DCJTB (10 mg / ml), stirred for 1 hour, washed with anhydrous ethanol solution and stored in a constant temperature drying oven, and in step (8), a stretchable AC electroluminescent device based on ZnS / DCJTB coated structure phosphor is obtained.
[0026] Embodiment 3: The difference from control group 1 is that in step (3), ZnS is added to chloroform containing DCJTB (20 mg / ml), stirred for 1 hour, washed with anhydrous ethanol solution and stored in a constant temperature drying oven, and in step (8), a stretchable AC electroluminescent device based on ZnS / DCJTB coated structure phosphor is obtained.
[0027] Embodiment 4: The difference from control group 1 is that in step (3), ZnS is added to chloroform containing DCJTB (40 mg / ml), stirred for 1 hour, washed with anhydrous ethanol solution and stored in a constant temperature drying oven, and in step (8), a stretchable AC electroluminescent device based on ZnS / DCJTB coated structure phosphor is obtained.
[0028] The test results of the stretchable AC electroluminescent devices of Control Group 1 and Examples 1-4 are shown in Table 1.
[0029] Table 1 Test results of stretchable AC electroluminescent devices sample Thickness (micrometer) Threshold voltage (V) Maximum elastic strain (%) CIE coordinates (x, y) Control group 1 426 53 120 (0.1892, 0.5513) Example 1 431 61 120 (0.2745, 0.5227) Example 2 415 67 120 (0.3368, 0.4965) Example 3 424 72 120 (0.4376, 0.4726) Example 4 438 77 120 (0.5274, 0.4335) It can be seen that: a stretchable AC electroluminescent device based on ZnS / small molecule fluorescent dye coated structured phosphor and its preparation method (ie, Examples 1 to 4) is not significantly improved in stretchability and thickness compared to the stretchable AC electroluminescent device of ZnS phosphor (ie, control group 1), and the threshold voltage is slightly increased. At the same time, by comparing Examples 1 to 4, it can be seen that with the increase of DCJTB concentration, the CIE coordinates of the device change, and the luminescent color gradually changes from green to red, achieving adjustable luminescent color. And the threshold voltage gradually increases, which is because the thickness of DCJTB coated on the ZnS surface increases, resulting in an increase in the energy threshold required for photon reabsorption and fluorescence resonance energy transfer, resulting in an increase in the threshold voltage.
[0030] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.
Claims
1. A stretchable AC electroluminescent device, characterized in that: It includes an upper electrode layer, an electroluminescent layer and a lower electrode layer from top to bottom. The electroluminescent layer is a coating structure in which the surface of zinc sulfide ZnS is covered with a small molecule fluorescent dye.
2. The stretchable AC electroluminescent device according to claim 1, characterized in that: The zinc sulfide ZnS is a 50-micron particle surface-treated with a silane coupling agent. The methoxy group and cyano group in the small molecule fluorescent dye are paired with the amino group in the silane coupling agent to be wrapped and fixed on the surface of the zinc sulfide ZnS.
3. The stretchable AC electroluminescent device according to claim 1, characterized in that: The upper electrode layer and the lower electrode layer are transparent stretchable thin film electrodes formed by PEDOT:PSS or silver nanowires coated on elastic polymers, with a thickness ranging from 0.05-1 mm.
4. A method for preparing a stretchable AC electroluminescent device, characterized in that: include: S1. Soak the ZnS particles in a mixed solution of concentrated sulfuric acid and hydrogen peroxide, wash them with deionized water, and store them in a constant temperature drying oven; S2, placing ZnS in an anhydrous ethanol solution containing a silane coupling agent and stirring, washing it with anhydrous ethanol and then drying it with nitrogen; S3, adding ZnS to a polar solvent containing a small molecule fluorescent dye, stirring, washing with an anhydrous ethanol solution, and storing in a constant temperature drying oven to obtain a phosphor with a ZnS / small molecule fluorescent dye coating structure; S4, cleaning the three Si / SiO2 wafers with deionized water, isopropyl alcohol, and acetone solution, drying them with nitrogen gas, and storing them in a constant temperature drying oven; S5, after UVO treatment of the surfaces of two Si / SiO2 wafers, any one of PDMS, SEBS, and TPU is spin-coated, printed, or sprayed on the surface of the Si / SiO2 wafer, and thermally annealed to form a stretchable substrate; S6, after the stretchable substrate is subjected to UVO treatment, PEDOT:PSS or silver nanowire solution is spin-coated, printed or sprayed on the surface of the stretchable substrate, and then peeled off from the surface of the Si / SiO2 wafer after secondary annealing to form an upper electrode layer and a lower electrode layer; S7, mixing the phosphor of the ZnS / small molecule fluorescent dye encapsulated structure with the elastic polymer, spin coating, printing or spraying on the surface of another Si / SiO2 wafer, and peeling off from the surface of the Si / SiO2 wafer after annealing to obtain an electroluminescent layer; S8. After the electroluminescent layer, the upper electrode layer and the lower electrode layer are subjected to plasma surface treatment, the upper electrode layer and the lower electrode layer are attached to the upper and lower surfaces of the electroluminescent layer respectively, and after being pressed by a press, a stretchable AC electroluminescent device as described in any one of claims 1 to 3 is obtained.
5. The method for preparing a stretchable AC electroluminescent device according to claim 4, characterized in that: In S1, the mass ratio of concentrated sulfuric acid to 30% hydrogen peroxide in the mixed solution was 7:3, and the immersion time was 2 hours.
6. The method for preparing a stretchable AC electroluminescent device according to claim 4, characterized in that: In S2, the silane coupling agent is one of APTMS or APTES, the concentration range is 5-100 mM, and the stirring time is 1-2 hours.
7. The method for preparing a stretchable AC electroluminescent device according to claim 4, characterized in that: In S3, the small molecule fluorescent dye is DCJTB or rhodamine, the polar solvent is one of chloroform, ethyl acetate, dichloromethane and DMF, and the concentration range of the small molecule fluorescent dye is 5-100 mg / ml.
8. The method for preparing a stretchable AC electroluminescent device according to claim 4, characterized in that: In S6, the UVO treatment time is 15-30 minutes, the PEDOT:PSS concentration is 0.5-5% wt%, the silver nanowire concentration is 10-100 mg / ml, the secondary annealing temperature is 110-150°C, and the annealing time is 5-30 minutes.
9. The method for preparing a stretchable AC electroluminescent device according to claim 4, characterized in that: In S7, the ratio of phosphor to elastic polymer in the ZnS / small molecule fluorescent dye encapsulation structure is 10-50 wt%, the annealing temperature is 80-110°C, the annealing time is 1-2 hours, and the thickness of the electroluminescent layer is 0.05-1 mm.