Preparation method and application of nano-composite adhesive hydrogel based on radix astragali seu hedysari extract

The nanocomposite hydrogel of astragalus polyphenol nanoparticles and astragalus polysaccharide prepared through amidation and borate ester reaction solves the problem of multifunctionality and biocompatibility of nanocomposite hydrogel in the treatment of brain diseases in the existing technology. It solves the problem of insufficient adhesion and achieves excellent adhesion and antioxidant properties, significantly improving the repair effect of brain hematoma damage.

CN118845618AActive Publication Date: 2024-10-29SICHUAN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410845207.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Existing nanocomposite hydrogels lack versatility and excellent biocompatibility when dealing with complex environments and clinical applications, such as cardiovascular, liver and brain diseases, and are difficult to effectively repair brain hematoma damage.

Method used

Triaminophenylboronic acid monohydrate was grafted to bexarotene drug through amidation reaction, and then reacted with astragalus polyphenol for borate ester to form astragalus polyphenol nanoparticles, which were mixed with astragalus polysaccharide through hydrogen bonding to prepare Nanocomposite adhesive hydrogel based on astragalus extract was developed. This method combines the antioxidant and anti-inflammatory effects of astragalus polyphenols with the selective activation of retinoid X receptors by bexarotene for the treatment of brain diseases.

Benefits of technology

The prepared nanocomposite hydrogel shows excellent adhesion, antioxidant properties and biocompatibility, can significantly improve the repair effect of brain hematoma damage, and enhances the therapeutic potential for brain diseases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118845618A_ABST
    Figure CN118845618A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of nano-composite adhesive hydrogel based on radix astragali seu hedysari extract.The preparation method comprises the steps that 1, triaminophenylboronic acid monohydrate is grafted to a bexarotene medicine through amidation reaction, and the bexarotene medicine grafted with phenylboronic acid is obtained; step 2, mixing the phenylboronic acid grafted bexarotene medicine with astragalus membranaceus polyphenol, and carrying out boric acid ester reaction to obtain astragalus membranaceus polyphenol nanoparticles; and step 3, mixing the astragalus polyphenol nanoparticles with astragalus polysaccharide, and performing hydrogen-bond interaction to obtain the nano composite adhesive hydrogel. The nano-composite adhesive hydrogel prepared by the invention can be used for repairing brain hematoma injury by cooperating with the effects of the astragalus extract and the bexarotene medicine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of biomedical materials, and specifically relates to a preparation method and application of a nanocomposite adhesive hydrogel based on astragalus extract. Background Art

[0002] Polymer nanoparticle hydrogels have attracted extensive attention due to their unique advantages, such as strong adhesion, low cost, and safety. This multifunctional, tunable, dynamic nanocomposite material is formed by reversible interactions between polymer chains and nanoparticles, and has attracted widespread attention in tissue adhesion, wound healing, organ repair, and other biomedical applications. Scientific researchers have widely reported a variety of nanoparticles and nanosheets combined with polymer chains to prepare nanocomposite hydrogels that can achieve rapid wound repair in special environments. However, these materials generally lack versatility and excellent biocompatibility, and therefore still face severe challenges in coping with complex environments and special diseases in clinical applications, such as cardiovascular, liver, and brain diseases.

[0003] As a traditional Chinese herbal medicine, the root of Astragalus has a long history of medicinal use. Pharmacological studies have shown that Astragalus contains a variety of elements such as folic acid, amino acids, betaine, carbohydrates and proteins. In general, Astragalus and its extracts have the effects of replenishing qi and raising yang, strengthening the exterior and stopping sweating, promoting diuresis and reducing swelling, promoting fluid and nourishing blood, relieving stagnation and relieving arthritis, expelling toxins and draining pus, and healing sores and promoting tissue regeneration. Astragalus polyphenols are a natural extract containing multiple catechols and have biological effects such as antioxidant, anti-inflammatory and antibacterial. Astragalus polysaccharides are an extract with multiple hydrogen bonding groups that can be prepared into hydrogels with excellent adhesion. Therefore, it is a feasible strategy to combine Astragalus polyphenols and Astragalus polysaccharide extracts to prepare a new type of antioxidant and anti-inflammatory nanocomposite hydrogel. Summary of the invention

[0004] The purpose of the present application is to provide a preparation method and application of a nanocomposite adhesive hydrogel based on astragalus extract.

[0005] The present application provides a method for preparing a nanocomposite adhesive hydrogel based on an astragalus extract, comprising:

[0006] Step 1, grafting triaminophenylboronic acid monohydrate onto bexarotene drug through amidation reaction to obtain bexarotene drug grafted with phenylboronic acid;

[0007] Step 2: mixing the bexarotene drug grafted with phenylboronic acid with astragalus polyphenol to carry out a borate ester reaction to obtain astragalus polyphenol nanoparticles;

[0008] Step 3: Mix the astragalus polyphenol nanoparticles and astragalus polysaccharide and obtain a nanocomposite adhesive hydrogel through hydrogen bonding.

[0009] The structural formula of bexarotene is shown in the following formula (I):

[0010]

[0011] The structural formula of the bexarotene drug grafted with phenylboronic acid is shown in the following formula (II):

[0012]

[0013] The structural formula of astragalus polyphenols is shown in the following formula (III):

[0014]

[0015] The structural formula of Astragalus polyphenols is shown in the following formula (IV):

[0016]

[0017] In some specific implementations, step one is specifically:

[0018] 1-2 mole parts of triaminophenylboronic acid monohydrate, 1.5-3 mole parts of amidation catalyst and 1-2 mole parts of bexarotene drug are mixed and dissolved in dimethyl sulfoxide or dimethylformamide, and reacted for 12-24 hours to obtain bexarotene drug grafted with phenylboronic acid.

[0019] Furthermore, the amidation catalyst includes 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide, wherein the molar ratio of 1-ethyl-(3-dimethylaminopropyl)carbodiimide to N-hydroxysuccinimide is 1:1.

[0020] In some specific implementations, step 2 is specifically:

[0021] The bexarotene drug grafted with phenylboronic acid and astragalus polyphenol are taken at a mass ratio of 4-8:10-30 respectively, a dimethyl sulfoxide or dimethylformamide solution of the bexarotene drug grafted with phenylboronic acid is prepared, and an astragalus polyphenol aqueous solution is prepared. The dimethyl sulfoxide or dimethylformamide solution of the bexarotene drug grafted with phenylboronic acid is added dropwise to the astragalus polyphenol aqueous solution, and the astragalus polyphenol nanoparticles are obtained after stirring and reacting for 2-24 hours.

[0022] In some specific embodiments, the concentration of the dimethyl sulfoxide or dimethylformamide solution of the bexarotene drug grafted with phenylboronic acid is 10-30 mg / mL, and the concentration of the astragalus polyphenol aqueous solution is 4-8 mg / mL.

[0023] In some specific implementations, step three is specifically:

[0024] 0.5-5 parts by weight of astragalus polyphenol nanoparticles are dispersed in water, 50-100 parts by weight of astragalus polysaccharide are taken to prepare an astragalus polysaccharide aqueous solution, the astragalus polysaccharide aqueous solution is dissolved in the dispersed solution, and the mixture is stirred for 5-12 hours to obtain a nanocomposite adhesive hydrogel.

[0025] In some specific embodiments, the concentration of astragalus polyphenol nanoparticles in the reaction solution is 0.5-5 mg / mL, and the concentration of astragalus polysaccharide aqueous solution is 50-100 mg / mL.

[0026] Astragalus extract has excellent antioxidant capacity and adhesion, and bexarotene, as a receptor selective agent, can bind to brain-related receptors and selectively activate retinoid X receptor (RXR) agonists, thereby being used to treat brain diseases. The prepared nanocomposite adhesive hydrogel based on astragalus extract, synergistically combining the effects of astragalus extract and bexarotene, can be used to repair brain hematoma damage. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the nuclear magnetic resonance hydrogen spectrum of the bexarotene drug grafted with phenylboronic acid in the examples of the present application;

[0028] Figure 2 This is the mass spectrum of the bexarotene drug grafted with phenylboronic acid in the examples of this application;

[0029] Figure 3 This is a scanning electron microscope image of the astragalus polyphenol nanoparticles prepared in the examples of the present application;

[0030] Figure 4 The modulus curves of different samples in the examples of this application;

[0031] Figure 5 : is the viscosity curve of different samples in the examples of this application;

[0032] Figure 6 The adhesion strength of different samples on different substrates in the examples of this application;

[0033] Figure 7 The antioxidant properties of different samples in the examples of this application;

[0034] Figure 8 The biocompatibility cell test results of the nanoparticles in the examples of this application;

[0035] Fig. 9 This is the brain hematoma clearance rate of different samples in the examples of this application. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and beneficial effects of the present application more clearly understood, the present application is further described in detail below in conjunction with embodiments.

[0037] In order to make the purpose, technical solutions and beneficial effects of the present application more clearly understood, the present application is further described in detail below in conjunction with embodiments.

[0038] Example

[0039] The specific steps of this embodiment are as follows:

[0040] Step 1: Dissolve 1 mol of triaminophenylboronic acid monohydrate, 3 mol of amidation catalyst and 1.5 mol of bexarotene drug in dimethyl sulfoxide, stir and react for 12 hours to obtain bexarotene drug grafted with phenylboronic acid; wherein the amidation catalyst includes 1.5 mol of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 1.5 mol of N-hydroxysuccinimide.

[0041] The product of this step was subjected to nuclear magnetic resonance detection. The hydrogen spectrum and mass spectrum were respectively shown in Figures 1-2 ,from Figures 1-2 It can be seen that the grafting of phenylboronic acid was successful.

[0042] Step 2: prepare a dimethyl sulfoxide solution of bexarotene grafted with phenylboronic acid at a concentration of 20 mg / mL; prepare an astragalus polyphenol aqueous solution at a concentration of 5 mg / mL; take 200 microliters of the dimethyl sulfoxide solution of bexarotene grafted with phenylboronic acid, add it dropwise to 5 milliliters of the astragalus polyphenol aqueous solution, stir and react for 5 hours, and obtain astragalus polyphenol nanoparticles.

[0043] The scanning electron photo of the product of this step is shown in Figure 3 It can be seen that nano-scale Astragalus polyphenol extract has been successfully prepared.

[0044] Step 3: Disperse the astragalus polyphenol nanoparticles in an aqueous solution to obtain a dispersion with a concentration of 1 mg / mL; prepare an astragalus polysaccharide aqueous solution with a concentration of 60 mg / mL; take 500 microliters of the dispersion, and then take 500 microliters of the astragalus polysaccharide aqueous solution and dissolve it in the dispersion. After 12 hours of hydrogen bonding physical action, a nanocomposite adhesive hydrogel based on astragalus extract is obtained.

[0045] The product of this step was subjected to rheological testing under the following conditions: 1% strain, 25°C, 10 rad / s. The test results are shown in Figures 4-5 , Figure 4 and Figure 5 They are modulus curve and viscosity curve respectively, where “nanogel” is the nanocomposite adhesive hydrogel in this embodiment. Figures 4-5 It can be seen that the nanocomposite adhesive hydrogel based on Astragalus extract has been successfully prepared.

[0046] In order to verify the performance advantages of the nanocomposite adhesive hydrogel based on astragalus extract of the present application, the performance of different samples will be evaluated separately below, among which the "nanogel" sample is the product of step three of the embodiment, that is, the nanocomposite adhesive hydrogel based on astragalus extract; the "nanoparticle" sample is the product of step two of the embodiment, that is, astragalus polyphenol nanoparticles; the "gel" sample is an astragalus polysaccharide gel without astragalus polyphenol nanoparticles, and its preparation method is:

[0047] Astragalus polyphenol is dispersed in an aqueous solution to obtain a dispersion with a concentration of 5 mg / mL; an astragalus polysaccharide aqueous solution is prepared with a concentration of 60 mg / mL; 1000 microliters of the dispersion and the astragalus polysaccharide aqueous solution are taken respectively, and the astragalus polysaccharide aqueous solution is dissolved in the dispersion, and a gel based on the astragalus extract is obtained through the physical action of hydrogen bonds.

[0048] The performance evaluation of the above three samples is carried out as follows.

[0049] 1. Evaluation of Adhesion

[0050] Evaluate the adhesion of gel and nanogel to different substrates. Apply the gel sample evenly on the surface of a substrate of 25mm*25mm size. When the substrate is pig skin, apply the gel sample on the inner epidermis of pig skin. Use a universal testing machine to measure the lap shear stress of the PDL gel sample adhering to the substrate. Fix the ends of the tissue sample on a single clamp and stretch it at a tensile rate of 10mm / min using a 500N load cell. Calculate the adhesion strength by dividing the maximum stress by the contact area between the gel sample and the substrate. For adhesion strength data, see Figure 6 .from Figure 6 It can be seen that the adhesion of the nanogel is significantly better.

[0051] 2. Antioxidant Capacity Assessment

[0052] The antioxidant capacity of nanoparticles, gels and nanogels was evaluated. The antioxidant capacity of different samples in aqueous solution was evaluated by scavenging 2,2'-azido-bis(3-ethylbenzothiazoline-6-sulfonic acid) radicals (ABTS). ABTS solution was reacted with 2.45 mM potassium persulfate at room temperature in the dark for 12 h to generate ABTS cation radicals. Sample solution and 7 mM ABTS aqueous solution were prepared. Sample solution and 100 μL ABTS solution were added to meet the test requirement of a total of 3 mL and the absorbance of the test sample at 734 nm was recorded for 30 minutes. The above test was repeated three times for each group of samples. For test results, see Figure 7 , used to evaluate the antioxidant capacity of nanoparticles and nanocomposite hydrogels. Figure 7 It can be seen that both nanoparticles and nanogels have relatively excellent antioxidant properties.

[0053] 3. Biocompatibility Cell Testing

[0054] NIH 3T3 cells were cultured (5% CO 2 and 37°C) were used for cellular evaluation of nanoparticles, and the in vitro cell activity of each sample was evaluated by the Alamar blue method. NIH 3T3 cells were plated on 96-well plates (2000 cells per well) and cultured for 24 hours. Then, the cells were treated with different concentrations of nanoparticle solutions and incubated for 24 hours, and then the corresponding cell viability of each sample was evaluated using the standard Alamar blue method. The test results are shown in Figure 8 .

[0055] 4. Animal experiment on brain hematoma repair in rats

[0056] (1) Establishment of brain hematoma injury model:

[0057] Mice weighing 25-30 g were used. Anesthesia was performed by intraperitoneal injection of tribromoethanol before surgery. After the righting reflex disappeared, the anesthesia was successful and the breathing was stable. The mice were fixed in a prone position on a stereotaxic instrument. The head was prepared and disinfected. A midline incision was made. Blunt separation was performed until the anterior fontanelle was exposed. Positioning was performed 0.2 mm in front of the anterior fontanelle and 2.25 mm to the right of the sagittal suture. A bone hole with a diameter of about 1 mm was drilled with a grinding drill and used for standby after completion. The right femoral artery and vein were exposed by anatomical separation. The proximal end was temporarily blocked, and the distal end was blocked by ligation. The femoral artery and vein were straightened and maintained with a certain tension. A small incision was made with microscissors near the ligation at the distal end of the femoral artery. The femoral artery was cannulated with a plastic catheter. After cannulation, about 40 μL of femoral arterial blood was collected and placed in a 1 mL syringe. Then, 30 μl of autologous blood was injected into the right basal ganglia area (3.7 mm deep) of the mouse through a microinjection pump. The injection speed was set to 3 μL / min. After the injection, the needle was withdrawn after 10 minutes to see if there was any blood reflux. If no reflux was observed, the skull hole was sealed with bone wax and the skin of the head and thigh was sutured.

[0058] (2) Experimental grouping and sampling method:

[0059] Eighteen rats with cerebral hematoma injury model were randomly divided into three groups according to body weight, including a control group of 6 rats (no treatment), a Gel group and a Gel-NPs group of 6 rats (bioadhesive hydrogel loaded with nanoparticles). The drugs were injected through the tail vein at a dose of 1.0 mg / Kg / Day, and the drugs were continuously administered for 1-7 days after modeling.

[0060] (3) The wound healing was observed every day and imaging analysis was performed. The edema and hematoma of the mice were observed by MRI T2 and T2* sequences on the day of modeling and on the 3rd, 7th, and 14th days respectively. The degree of edema and hematoma volume were calculated by ImageJ, and magnetic resonance imaging analysis was performed.

[0061] The results of the rat brain hematoma clearance test are shown in Fig. 9 , shows the hematoma clearance rate calculated based on the wound healing status on the 7th day.

[0062] The above embodiments are only for the purpose of clearly illustrating the embodiments, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, so the obvious changes or modifications derived are still within the protection scope of the invention.

Claims

1. A method for preparing a nanocomposite adhesive hydrogel based on astragalus extract, comprising: Step 1, grafting triaminophenylboronic acid monohydrate onto bexarotene drug through amidation reaction to obtain bexarotene drug grafted with phenylboronic acid; Step 2: mixing the bexarotene drug grafted with phenylboronic acid with astragalus polyphenol to carry out a borate ester reaction to obtain astragalus polyphenol nanoparticles; Step 3: Mix the astragalus polyphenol nanoparticles and astragalus polysaccharide and obtain a nanocomposite adhesive hydrogel through hydrogen bonding.

2. The method for preparing the nanocomposite adhesive hydrogel based on Astragalus extract according to claim 1, characterized in that: Step 1 is as follows: 1-2 mole parts of triaminophenylboronic acid monohydrate, 1.5-3 mole parts of amidation catalyst and 1-2 mole parts of bexarotene drug are mixed and dissolved in dimethyl sulfoxide or dimethylformamide, and reacted for 12-24 hours to obtain bexarotene drug grafted with phenylboronic acid.

3. The method for preparing the nanocomposite adhesive hydrogel based on Astragalus extract according to claim 2, characterized in that: The amidation catalyst comprises 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide, wherein the molar ratio of 1-ethyl-(3-dimethylaminopropyl)carbodiimide to N-hydroxysuccinimide is 1:

1.

4. The method for preparing the nanocomposite adhesive hydrogel based on astragalus extract according to claim 1, characterized in that: Step 2 is as follows: The bexarotene drug grafted with phenylboronic acid and astragalus polyphenol are taken at a mass ratio of 4-8:10-30 respectively, a dimethyl sulfoxide or dimethylformamide solution of the bexarotene drug grafted with phenylboronic acid is prepared, and an astragalus polyphenol aqueous solution is prepared. The dimethyl sulfoxide or dimethylformamide solution of the bexarotene drug grafted with phenylboronic acid is added dropwise to the astragalus polyphenol aqueous solution, and the astragalus polyphenol nanoparticles are obtained after stirring and reacting for 2-24 hours.

5. The method for preparing the nanocomposite adhesive hydrogel based on astragalus extract according to claim 1, characterized in that: Step three is as follows: 0.5-5 parts by weight of astragalus polyphenol nanoparticles are dispersed in water, 50-100 parts by weight of astragalus polysaccharide are taken to prepare an astragalus polysaccharide aqueous solution, the astragalus polysaccharide aqueous solution is dissolved in the dispersed solution, and the mixture is stirred for 5-12 hours to obtain a nanocomposite adhesive hydrogel.

6. Use of the nanocomposite adhesive hydrogel prepared by the preparation method according to any one of claims 1 to 5 in preparing a drug for repairing brain hematoma injury.

7. Use of the nanocomposite adhesive hydrogel prepared by the preparation method according to any one of claims 1 to 5 in preparing drugs for treating brain diseases.

Citation Information

Patent Citations

  • Preparation method of injectable self-adaptive natural hydrogel adhesive

    CN113248732A

  • Injectable heart failure treatment hydrogel based on recombinant humanized collagen and preparation method of injectable heart failure treatment hydrogel

    CN115068594A

  • Polyphenol cross-linked natural polysaccharide-based hydrogel dressing as well as preparation method and application thereof

    CN115212345A

  • Self-repairing injectable hydrogel dressing and preparation method thereof

    CN116603097A