Catalyst as well as preparation method and application thereof
By loading hollow-structured elemental copper and single-atom palladium metal nanowires on the foam copper catalyst carrier, the problem of low efficiency of the copper catalyst in the reduction of NO3-NH3 is solved, and efficient and selective reduction of NO3- to NH3 is achieved. , extending the service life of the catalyst.
Patent Information
- Application Number
- CN202410859970.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
AI Technical Summary
Existing copper catalysts have low efficiency in reducing nitrate (NO3-) to ammonia (NH3), making it difficult to effectively reduce the toxic intermediate product nitrite (NO2-) to NH3.
Copper foam is used as a catalyst carrier to load hollow-structured elemental copper and single-atom palladium metal nanowires. The catalyst is prepared through electrochemical oxidation, ion replacement reaction, calcination and electrochemical reduction treatment to improve catalytic sites and reaction channels and promote activity. Hydrogen generation and ammonia reduction.
It improves the efficiency and stability of the catalyst, enhances the ability of NO3- to efficiently reduce to NH3 at a lower potential, reduces the accumulation of toxic by-product NO2-, and improves ammonia production efficiency and electrocatalytic reduction performance.
Smart Images

Figure CN118847149A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst preparation, and in particular to a catalyst and a preparation method and application thereof. Background Art
[0002] Nitrate in water (NO3 - ) When the concentration is too high, the water body is prone to eutrophication, causing a large number of algae to reproduce and cause water body deterioration, seriously affecting the aquatic ecosystem and human life and health. - It has high solubility and N presents the highest valence state of +5, which can stably exist in water. Conventional treatment methods are difficult to effectively remove and effectively utilize NO3 in water. - .
[0003] Electrocatalytic reduction of NO3 - The technology is an environmentally friendly wastewater treatment method and resource recovery method based on electrochemical methods. It mainly uses green electrons and protons in water to achieve NO3 - The product ammonia (NH3) produced in the process can be used as an important chemical product, improving the economic competitiveness of the technology.
[0004] The commonly used copper (Cu) catalyst is used to reduce NO3 - Nitrite (NO2 - ) is excellent, which is due to the highest occupied d orbital energy level of transition metal Cu and NO3 - The lowest unoccupied molecular π* orbital energy level of NO3 - Efficient reduction to NO2 - However, Cu catalyzes NO2 - The conversion to NH3 is inefficient, resulting in the production of toxic intermediate NO2 - It is difficult to effectively reduce to NH3. Summary of the invention
[0005] The main purpose of the present invention is to provide a catalyst and its preparation method and application, aiming to solve the problem that Cu catalyst is difficult to effectively reduce NO3 - It's a question of NH3.
[0006] To achieve the above object, the present invention provides a catalyst, comprising a catalyst carrier and metal nanowires loaded on the surface of the catalyst carrier;
[0007] Wherein, the catalyst carrier comprises copper foam;
[0008] The metal nanowire is a hollow structure and includes single-element copper and single-atom palladium.
[0009] In one embodiment, the mass ratio of elemental copper to monatomic palladium in the catalyst is 100:(0.1-2).
[0010] In one embodiment, the average diameter of the metal nanowires is 100 to 400 nm; and / or,
[0011] The average diameter of the hollow structure is 80-300 nm.
[0012] The present invention also provides a method for preparing a catalyst, comprising the following steps:
[0013] S10, obtaining a base copper foam, wherein the base copper foam includes a copper foam having first nanowires grown on the surface thereof, wherein the first nanowires include an insoluble copper compound;
[0014] S20, mixing the base copper foam and the palladium solution to cause an ion replacement reaction, so that the copper ions in a part of the insoluble copper salt are replaced by palladium ions, and a palladium-loaded base copper foam is obtained;
[0015] S30, calcining the palladium-loaded copper foam substrate under an inert gas;
[0016] S40, performing reduction treatment on the palladium-loaded substrate foam copper that has completed the calcination treatment to obtain a catalyst.
[0017] In one embodiment, step S10 includes:
[0018] The base copper foam is prepared by electrochemical oxidation method.
[0019] In one embodiment, the constant current density of the electrochemical oxidation method is 15-25 mA / cm 2 and / or,
[0020] The oxidation time of the electrochemical oxidation method is 10 to 30 minutes.
[0021] In one embodiment, in step S20:
[0022] The palladium ion concentration in the palladium solution is 1 to 100 mM; and / or,
[0023] The ion exchange reaction time is 10 to 40 minutes; and / or,
[0024] Mixing the base copper foam and the palladium solution includes: adding 114 g of the base copper foam to each liter of the palladium solution.
[0025] In one embodiment, in step S30:
[0026] The inert gas includes at least one of argon and nitrogen; and / or,
[0027] The calcination temperature is 180-220°C; and / or,
[0028] The heating rate of the calcination is 4-10°C / min; and / or,
[0029] The calcination time is 1.5 to 2.5 hours.
[0030] In one embodiment, step S40 includes:
[0031] The palladium-loaded copper foam substrate that has undergone calcination is subjected to electrochemical reduction treatment to obtain a catalyst;
[0032] Wherein, the electrochemical reduction includes a first reduction treatment and a second reduction treatment;
[0033] The constant current density of the first reduction treatment is 80-120 mA / cm 2 and / or,
[0034] The reduction time of the first reduction treatment is 1.5 to 2.5 hours; and / or,
[0035] The constant current density of the second reduction treatment is 650-750 mA / cm 2 and / or,
[0036] The reduction time of the second reduction treatment is 0.8 to 1.2 hours.
[0037] The present invention also provides an application of a catalyst in treating wastewater, wherein the catalyst comprises a catalyst carrier and metal nanowires loaded on the surface of the catalyst carrier;
[0038] Wherein, the catalyst carrier comprises copper foam;
[0039] The metal nanowire is a hollow structure and includes single-element copper and single-atom palladium.
[0040] The present invention proposes a catalyst and its preparation method and application, wherein the copper foam presents a three-dimensional self-supporting structure, has a high porosity and a large specific surface area, and can provide more attachment points for copper metal nanowires. The hollow structure of the copper metal nanowire provides more surface area, and its inner and outer surfaces can be used as active catalytic sites, thereby increasing the catalytic sites, greatly increasing the chance of contact with reactants, and improving the catalytic efficiency; the cavity inside the hollow structure can be used as a channel, making it easier for reactants to penetrate into the inner surface of the nanowire, and also facilitating the diffusion of products from the inside, which is beneficial to the diffusion of catalytic substrates and products, reducing mass transfer resistance, and accelerating the reaction rate; the hollow nanowire can promote internal convection, improve mass transfer efficiency, and enable molecules in the reaction medium to contact the catalyst surface more quickly and evenly, thereby enhancing the kinetics of the catalytic process; the hollow structure also improves the stability of the catalyst and prolongs its service life. The elemental copper on the copper metal nanowire can catalyze NO3 - To NO2 - The single-atom palladium in the copper metal nanowires reduces the energy barrier of water generating active hydrogen, promotes the generation of active hydrogen at a lower potential, and can dissociate gaseous H2 into H atoms, inhibiting the hydrogen evolution reaction; due to the hydrogen overflow phenomenon between single-atom palladium and elemental copper, single-atom palladium in the elemental copper environment can easily transfer the generated active hydrogen to the copper atoms around it, so that the NO2 generated on the copper site - The active hydrogen is absorbed more quickly and reduced to ammonia, thus improving the efficiency of ammonia production. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0042] Figure 1a This is a scanning electron microscope image of the foam copper material used in Example 4 provided by the present invention;
[0043] Figure 1b This is another scanning electron microscope image of the foam copper material used in Example 4 provided by the present invention;
[0044] Figure 1c This is a scanning electron microscope image of the catalyst prepared in Example 4 provided by the present invention;
[0045] Figure 1d This is a scanning electron microscope image of the hollow nanoarray on the surface of the catalyst prepared in Example 4 provided by the present invention;
[0046] Figure 1e This is a transmission electron microscopy image of the hollow structure on the surface of the catalyst prepared in Example 4 provided by the present invention;
[0047] Figure 1f This is a distribution diagram of palladium elements in the hollow structure on the surface of the catalyst prepared in Example 4 provided by the present invention;
[0048] Figure 1g This is a distribution diagram of copper elements in the hollow structure on the surface of the catalyst prepared in Example 4 provided by the present invention;
[0049] Figure 1h This is a common distribution diagram of palladium and copper elements in the hollow structure on the surface of the catalyst prepared in Example 4 provided by the present invention;
[0050] Figure 1i This is an X-ray diffraction analysis diagram of the material after electrochemical oxidation treatment, calcination treatment and electrochemical reduction in Example 4 provided by the present invention;
[0051] Figure 1j This is an extended X-ray absorption fine structure analysis diagram of the catalyst prepared in Example 4 provided by the present invention;
[0052] Figure 2a Polarization curves of the catalysts prepared in Example 4 and Comparative Example 1 provided by the present invention with and without nitrate;
[0053] Figure 2b This is a test chart of the nitrate removal ability of the catalysts prepared in Example 4 and Comparative Example 1 provided by the present invention;
[0054] Figure 2c This is a test chart of the ammonia production capacity of the catalyst prepared in Example 4 and Comparative Example 1 provided by the present invention;
[0055] Figure 2d The product distribution diagram of the catalyst prepared in Example 4 and Comparative Example 1 provided by the present invention when electro-reducing nitrate at -1.1V vs.Hg / HgO;
[0056] Figure 2e The NH3 selectivity and NH3 Faraday efficiency of the catalyst prepared in Example 4 provided by the present invention during the electroreduction nitrate cycle test at -1.1V vs.Hg / HgO;
[0057] Figure 2f For the purpose of comparing the NH3 production rate of the catalyst prepared in Example 4 provided by the present invention with the data reported in the literature under similar reaction conditions.
[0058] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0059] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0060] Nitrate in water (NO3 - ) When the concentration is too high, the water body is prone to eutrophication, causing a large number of algae to reproduce and cause water body deterioration, seriously affecting the aquatic ecosystem and human life and health. High concentrations of NO3 - It is toxic and carcinogenic. When the human body ingests high concentrations of NO3 - When NO3 - It is easily converted into NO2 in the human body - , NO2 - It is easy to induce hemoglobinemia in the blood, leading to hypoxia, suffocation and even death. - With NO2 - Combined with the carcinogenic N-nitroso compounds, this substance is very likely to induce cancer and cause great harm to human health. Take appropriate measures to remove NO3 in water - Or convert it into substances useful for human production, which is not only beneficial to environmental protection and pollution control, but also can protect humans from environmental NO2 to the greatest extent. - of harm.
[0061] NO3 - It has high solubility and N presents the highest valence state of +5, which can stably exist in water. Conventional treatment methods are difficult to effectively remove and effectively utilize NO3 in water. - .
[0062] Electrocatalytic reduction of nitrate is an environmentally friendly wastewater treatment and resource recovery method based on electrochemical methods. It mainly uses green electrons and protons in water to reduce NO3 - The ammonia (NH3) produced in the process can be used as an important chemical product, which improves the economic competitiveness of the technology. In addition, the technology has strong resistance to water quality fluctuations, is suitable for normal temperature and pressure operation, is easy to scale up, has no secondary pollution, and takes into account pollution reduction and carbon reduction. Therefore, it is an environmentally friendly, low-carbon and resource-saving process.
[0063] Commonly used copper (Cu) catalysts in the reduction of NO3 - This is due to the high occupied d orbital energy level of transition metal Cu and NO3 - The lowest unoccupied molecular π* orbital energy level of NO3 - Efficient reduction to NO2 - However, Cu catalyzes NO2 - The conversion to NH3 is inefficient, resulting in the production of toxic intermediate NO2 - It is difficult to effectively reduce to NH3, which is mainly due to the weak ability of Cu to produce strongly reducing atomic hydrogen (H*) through the Volmer process. The Volmer process usually refers to the process in which water molecules are reduced on the electrode surface to generate adsorbed hydrogen atoms (H*).
[0064] In view of this, the present invention provides a catalyst, comprising a catalyst carrier and metal nanowires supported on the surface of the catalyst carrier;
[0065] Wherein, the catalyst carrier comprises copper foam;
[0066] The metal nanowire is a hollow structure and includes single-element copper and single-atom palladium.
[0067] In the technical solution of the present invention, the hollow structure of copper metal nanowires provides more surface area, and its inner and outer surfaces can be used as active catalytic sites, thereby increasing the catalytic sites, greatly increasing the chance of contact with reactants, and improving the catalytic efficiency; the cavity inside the hollow structure can be used as a channel, making it easier for reactants to penetrate into the inner surface of the nanowires, while also facilitating the diffusion of products from the inside, which is beneficial to the diffusion of catalytic substrates and products, reducing mass transfer resistance and accelerating the reaction rate; the hollow nanowires can promote internal convection, improve mass transfer efficiency, and enable molecules in the reaction medium to contact the catalyst surface more quickly and evenly, thereby enhancing the kinetics of the catalytic process. The elemental copper on the copper metal nanowires can catalyze NO3 - To NO2 -The single-atom palladium in the copper metal nanowires reduces the energy barrier for water to generate active hydrogen, promotes the generation and retention of active hydrogen at a lower potential, and thus promotes NO x Species deep hydrogenation reduction; Due to the hydrogen overflow phenomenon between single-atom palladium and elemental copper, single-atom palladium is dispersed in the environment of elemental copper nanowires with a hollow structure, which facilitates the transfer of the generated active hydrogen to the copper atoms around it, making the NO2 generated on the copper site - The active hydrogen is quickly absorbed and reduced to ammonia, which not only improves the utilization rate of palladium, but also avoids the toxic byproduct NO2 - The accumulation of NO3 at the catalyst interface and poisoning of the catalyst increases the efficiency of ammonia production. The structure of the monolithic catalyst is also beneficial to improve the conductivity of the electrode and improve the electrocatalytic reduction of NO3 - Therefore, the catalyst of the present invention simultaneously couples the ability of palladium to efficiently produce H* and copper to efficiently convert NO3 - Reduction to NO2 - The ability of NO3 - It can be reduced to ammonia more efficiently and selectively at a lower potential, which improves the efficiency of Cu catalyst in reducing NO3 - Efficiency of reduction to NH3.
[0068] It should be noted that the copper foam was purchased from Kunshan Guangjiayuan New Materials Co., Ltd., product model GJYCU001, and the size of the copper foam catalyst was 10mm×10mm×1.5mm, the porosity was 75% to 98%, and the through-porosity was ≥97%. The porous structure of the copper foam helps to improve the diffusion of reactants to the catalyst surface and the removal of products from the surface, reduce mass transfer resistance, avoid mass transfer restrictions caused by excessive local concentration gradients, and maintain the continuity and efficiency of the reaction.
[0069] In some embodiments of the present invention, the mass ratio of elemental copper to monatomic palladium in the catalyst is 100:(0.1-2). The mass ratio of elemental copper to monatomic palladium in the catalyst can be 100:0.1, 100:1 or 100:2. The mass ratio of elemental copper to monatomic palladium in the catalyst within a suitable range can ensure that the catalyst has both the ability to degrade NO3 - Efficient reduction to NO2 - The ability and NO2 - Ability to efficiently reduce NH3.
[0070] In some embodiments of the present invention, the average diameter of the metal nanowires is 100-400 nm. The average diameter of the metal nanowires can be 100 nm, 200 nm, 300 nm or 400 nm. The average diameter of the metal nanowires within a suitable range can ensure that the metal nanowires have good electrical conductivity and catalytic performance.
[0071] In some embodiments of the present invention, the average diameter of the hollow structure is 80 to 300 nm. The average diameter of the hollow structure can be 80 nm, 150 nm or 300 nm. The average diameter of the hollow structure within a suitable range can ensure effective diffusion of reactants and products, reduce mass transfer resistance, avoid local overheating caused by electric field effects, and protect the stability of the catalyst structure.
[0072] The present invention also provides a method for preparing a catalyst, comprising the following steps:
[0073] S10, obtaining a base copper foam, wherein the base copper foam includes a copper foam having first nanowires grown on the surface thereof, wherein the first nanowires include an insoluble copper compound;
[0074] S20, mixing the base copper foam and the palladium solution to cause an ion replacement reaction, so that the copper ions in a part of the insoluble copper salt are replaced by palladium ions, and a palladium-loaded base copper foam is obtained;
[0075] S30, calcining the palladium-loaded copper foam substrate under an inert gas;
[0076] S40, performing reduction treatment on the palladium-loaded substrate foam copper that has completed the calcination treatment to obtain a catalyst.
[0077] In the technical scheme of the present invention, the base copper foam refers to the base copper foam with the first nanowire of the insoluble copper compound grown on the surface, and is not the commercial copper foam directly purchased. The insoluble copper compound includes copper hydroxide. In the ion replacement reaction, the insoluble copper compound provides active divalent copper ions, and the palladium ions in the palladium solution replace part of the divalent copper ions and enter the nanowire structure, so that the first nanowire in the base copper foam is loaded with palladium ions; after calcination with inert gas, the insoluble copper compound on the first nanowire in the base copper foam may lose water and turn into cuprous oxide, and palladium is loaded on the cuprous oxide nanowire. During the calcination process, the volatilization of water causes vacancies to be left on the original nanowire, thereby forming a hollow structure inside or around the cuprous oxide nanowire; after the calcination treatment, a reduction treatment is performed to reduce the monovalent copper in the cuprous oxide nanowire to zero-valent copper element, and at the same time, the divalent palladium loaded on the nanowire is reduced to zero-valent palladium. During the reduction treatment, the zero-valent palladium is evenly dispersed on the copper element nanowire, so that the nanowire on the base copper foam is converted into a copper nanowire uniformly loaded with palladium, that is, a catalyst.
[0078] In step S10, the method of obtaining the base copper foam includes electrochemical oxidation or chemical deposition. The electrochemical oxidation method is an electrochemical anodic oxidation method, that is, an electrochemical reaction is performed by applying a voltage, so that copper hydroxide nanowires are grown in situ on the surface of the copper foam. The nanowires can be regularly arranged nanowires or irregularly arranged nanowires, and the regular nanowires include nanowire arrays.
[0079] In step S20, the palladium solution can be a Pd(NO3)2 solution or a PdCl2 solution, as long as it can provide divalent palladium ions.
[0080] In step S40, the reduction treatment may be an electrochemical reduction treatment. It should be noted that the reduction may be a one-time reduction or a multi-stage reduction, as long as the copper in the final nanowire exists as a zero-valent single substance and the palladium exists as a zero-valent single atom.
[0081] In some embodiments of the present invention, step S10 includes: preparing the base copper foam by electrochemical oxidation. Compared with other methods, the nanowires on the surface of the base copper foam prepared by electrochemical oxidation are regularly arranged nanowire arrays, and compared with individual nanowires, the regularly arranged nanowire array structure has more catalytic active sites and better mechanical properties.
[0082] In addition, the electrochemical oxidation method does not require the addition of binders such as Nafion, and has higher stability and conductivity.
[0083] In some embodiments of the present invention, the constant current density of the electrochemical oxidation method is 15-25 mA / cm 2 The constant current density can be 15mA / cm 2 , 20mA / cm 2 or 25mA / cm 2 , constant current density within a suitable range helps to form a nanowire array with good directionality, regular arrangement and compactness.
[0084] In some embodiments of the present invention, the electrochemical oxidation method has an oxidation time of 15 to 25 minutes. The electrochemical oxidation method can have an oxidation time of 15 minutes, 20 minutes or 25 minutes. The oxidation time of the electrochemical oxidation method within a suitable range can ensure the orderly growth of the nanowires and form a nanowire array with uniform diameter and high consistency.
[0085] In some embodiments of the present invention, in step S20: the palladium ion concentration in the palladium solution is 1 to 100 mM. The palladium ion concentration in the palladium solution can be 1 mM, 10 mM, 50 mM or 100 mM. The palladium ion concentration in the palladium solution within a suitable range can ensure that after the copper ion and palladium ion replacement reaction, more palladium is loaded on the nanowire, and at the same time, the palladium is ensured to exist in the form of single atoms.
[0086] In some embodiments of the present invention, in step S20: the time of the ion exchange reaction is 10 to 40 minutes. The time of the ion exchange reaction can be 10 minutes, 25 minutes or 40 minutes. The time of the ion exchange reaction within a suitable range can ensure that the nanowires are loaded with more palladium without replacing all the copper, so that the final catalyst has both the ability of palladium to produce active hydrogen and the ability of copper to reduce nitrate to ammonia.
[0087] In some embodiments of the present invention, in step S20: mixing the base copper foam and the palladium solution comprises: adding 114 g of the base copper foam to each liter of the palladium solution. Such a setting can ensure that the nanowires are loaded with more palladium without replacing all the copper.
[0088] In some embodiments of the present invention, in step S30: the inert gas includes at least one of argon and nitrogen. The main purpose of the inert gas environment is to isolate oxygen and prevent the copper compound and palladium compound on the nanowire from reacting with oxygen at high temperature, which helps to form a more uniform and stable catalyst structure.
[0089] In some embodiments of the present invention, in step S30: the calcination temperature is 180-220° C. The calcination temperature can be 180° C., 200° C. or 220° C. The calcination temperature within a suitable range can ensure a suitable hollow structure, thereby effectively regulating the structural stability and catalytic performance of the catalyst.
[0090] In some embodiments of the present invention, in step S30: the heating rate of the calcination is 4-10°C / min. The heating rate of the calcination can be 4°C, 5°C or 6°C. The heating rate of the calcination can regulate the physical parameters of the hollow nanowire structure and the morphology of the nanowire array within a suitable range.
[0091] In some embodiments of the present invention, in step S30: the calcination time is 1.5 to 2.5 hours. The calcination time can be 1.5 hours, 2 hours or 2.5 hours. The calcination time within a suitable range can ensure that the copper compound and the palladium compound in the nanowire react sufficiently to complete the desired phase change.
[0092] In some embodiments of the present invention, step S40 includes: electrochemically reducing the palladium-loaded substrate copper foam that has completed the calcination treatment to obtain a catalyst; wherein the electrochemical reduction includes a first reduction treatment and a second reduction treatment. The two-stage electrochemical reduction is mainly to more accurately control the structural stability of the catalyst. The potential or conditions of the first reduction treatment are milder than those of the second reduction treatment. The first reduction treatment is intended to partially reduce the oxidation state of palladium and copper to a metallic state and stabilize the hollow nanowire array structure; the second reduction treatment is carried out under more negative potential conditions to promote the complete reduction of the copper nanowires and the substrate to a metallic state.
[0093] Wherein, the constant current density of the first reduction treatment is 80-120 mA / cm 2 The constant current density of the first reduction treatment can be 80 mA / cm 2 , 100mA / cm 2 or 120mA / cm 2 The constant current density of the first reduction treatment can convert at least part of the oxidized state of palladium and copper into the metallic state within a suitable range.
[0094] The reduction time of the first reduction treatment is 1.5 to 2.5 hours. The reduction time of the first reduction treatment can be 1.5 hours, 2 hours or 2.5 hours. The reduction time of the first reduction treatment within a suitable range can ensure sufficient time for preliminary reduction of some palladium and copper oxides.
[0095] Wherein, the constant current density of the second reduction treatment is 650-750 mA / cm 2 The constant current density of the second reduction treatment can be 650 mA / cm 2 , 700mA / cm 2 or 750mA / cm 2 , the constant current density of the second reduction treatment can ensure that the oxidation states of palladium and copper are completely converted into the metallic state to form palladium single atoms within a suitable range.
[0096] The reduction time of the second reduction treatment is 0.8 to 1.2 hours. The reduction time of the second reduction treatment can be 0.8 hours, 1 hour or 1.2 hours. The reduction time of the second reduction treatment within a suitable range can ensure sufficient time for palladium and copper to be converted from an oxidized state to a zero-valent metal state, and ensure the redispersion of palladium single atoms on the copper nanowires.
[0097] The present invention also provides a catalyst for treating wastewater, the catalyst comprising a catalyst carrier and a metal nanowire supported on the surface of the catalyst carrier; wherein the catalyst carrier comprises foamed copper; the metal nanowire is a hollow structure, and the metal nanowire comprises elemental copper and single-atom palladium. The catalyst comprises all the technical solutions of the catalyst, and therefore also has all the beneficial effects brought by the above technical solutions, which will not be described one by one here.
[0098] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0099] Example 1
[0100] A catalyst comprises a catalyst carrier and metal nanowires loaded on the surface of the catalyst carrier; wherein the catalyst carrier comprises foamed copper; the metal nanowires are hollow structures and comprise elemental copper and single-atom palladium.
[0101] Among them, the mass ratio of elemental copper and monatomic palladium in the catalyst is 100:0.1; the average diameter of the metal nanowires is 100.3nm; and the average diameter of the hollow structure is 80.9nm.
[0102] Example 2
[0103] The difference between Example 2 and Example 1 is that:
[0104] The mass ratio of elemental copper to monatomic palladium in the catalyst is 100:1; the average diameter of the metal nanowires is 176.3 nm; and the average diameter of the hollow structure is 130.6 nm.
[0105] Example 3
[0106] The difference between Example 3 and Example 1 is that:
[0107] The mass ratio of elemental copper to monatomic palladium in the catalyst is 100:2; the average diameter of the metal nanowires is 387.4 nm; and the average diameter of the hollow structure is 298.1 nm.
[0108] Example 4
[0109] A method for preparing a catalyst comprises the following steps:
[0110] (1) Take two pieces of copper foam (the size of the copper foam is 10 mm × 10 mm × 1.5 mm) purchased from Kunshan Guangjiayuan New Materials Co., Ltd. (product model GJYCU001), clean the copper foam with acetone ultrasonically for 10 min, and then soak the cleaned copper foam in 0.1 M hydrochloric acid solution for 10 min to remove possible oxides on the surface, then clean the copper foam with deionized water, dry it at room temperature for later use, and obtain the pretreated copper foam.
[0111] (2) Electrochemical oxidation was performed in a H2 cell with pretreated copper foam as the working electrode, a platinum (Pt) sheet (10×10×1.5 mm) as the counter electrode, and 1 M NaOH solution as the electrolyte. The anode (i.e., the working electrode) was oxidized at 20 mA / cm 2 The constant current was applied for 20 min to obtain copper hydroxide nanowire array foam (Cu(OH)2NWs), which was rinsed with deionized water and naturally dried for later use.
[0112] (3) The synthesized Cu(OH)2NWs were immersed in 10 mL of 10 mM Pd(NO3)2 solution at room temperature for 30 min to perform a cation exchange process to obtain palladium-loaded copper hydroxide nanowire array foam copper (Pd1@Cu(OH)2NWs). After ion exchange, it was dried at room temperature, and then heated from room temperature to 200°C at a heating rate of 5°C / min in an argon inert atmosphere, and calcined at 200°C for 2 h to obtain palladium-loaded cuprous oxide nanowire array foam copper (Pd1@Cu2ONWs).
[0113] (4) The electrochemical reduction steps are as follows:
[0114] The first reduction treatment was carried out at 100 mA / cm 2 The electrochemical reduction was carried out at a constant current density for 2 h;
[0115] The second reduction treatment was performed at 700 mA / cm 2 The electrochemical reduction was carried out at a constant current density for 1 h to obtain the catalyst (Pd1Cu SAA).
[0116] Example 5
[0117] The difference between Example 5 and Example 4 is that:
[0118] The concentration of palladium ions in the Pd(NO3)2 solution was 1 mM; the cation exchange time was 10 min;
[0119] The constant current density in the electrochemical oxidation method is 15 mA / cm 2 , oxidation time is 15min;
[0120] The calcination temperature is 180°C; the calcination time is 1.5h; the calcination heating rate is 4°C / min;
[0121] The constant current density of the first reduction treatment was 80 mA / cm 2 The reduction time of the first reduction treatment was 1.5 h; the constant current density of the second reduction treatment was 650 mA / cm 2 ; The reduction time of the second reduction treatment is 0.8h.
[0122] Example 6
[0123] The difference between Example 6 and Example 4 is that:
[0124] The concentration of palladium ions in the Pd(NO3)2 solution was 100 mM; the cation exchange time was 40 min;
[0125] The constant current density in the electrochemical oxidation method is 25 mA / cm 2, oxidation time is 25min;
[0126] The calcination temperature is 220°C; the calcination time is 2.5h; the calcination heating rate is 10°C / min;
[0127] The constant current density of the first reduction treatment was 120 mA / cm 2 The reduction time of the first reduction treatment was 2.5 h; the constant current density of the second reduction treatment was 750 mA / cm 2 ; The reduction time of the second reduction treatment is 1.2h.
[0128] Comparative Example 1
[0129] Comparative Example 1 is compared with Example 4, except that palladium nitrate solution is not added for ion replacement, and other aspects are the same as Example 4.
[0130] Performance Testing
[0131] The morphology of the copper foam material used in Example 4 was observed by scanning electron microscopy. Figure 1a and Figure 1b As shown, the surface morphology of the catalyst prepared in Example 4 is shown in Figure 1c As shown, the morphology of the hollow nanoarray on the catalyst surface prepared in Example 4 is shown in Figure 1d As shown. Figure 1a and Figure 1b It can be seen that the surface of the foam copper material is relatively smooth; Figure 1c It can be seen that the catalyst surface is relatively rough; Figure 1d It can be seen that the catalyst surface is composed of hollow nanowire arrays.
[0132] The hollow structure of the catalyst surface prepared in Example 4 was observed by transmission electron microscopy. Figure 1e As shown, the palladium element distribution diagram of the hollow structure is as follows Figure 1f As shown, the copper element distribution diagram of the hollow structure is as follows Figure 1g As shown, the distribution diagram of palladium and copper elements in the hollow structure is as follows Figure 1h As shown. Figure 1f The hollow structure of the nanowires on the catalyst surface can be clearly seen. Figure 1f , 1g and 1h, it can be seen that the elemental palladium is evenly distributed on the copper nanowires.
[0133] The materials after electrochemical oxidation, calcination and electrochemical reduction in Example 4 were analyzed by X-ray diffraction. Figure 1i As shown. Figure 1iIt can be seen that the foam copper material (green line) obtained Cu(OH)2NWs (yellow line) after electrochemical oxidation; after calcination, it was converted into Pd1@Cu2O (blue line); after electrochemical reduction, it became the catalyst Pd1CuSAA (red line). No XRD peak of palladium was observed, indicating that palladium exists in a single atomic form.
[0134] The structural spectrum of the catalyst prepared in Example 4 was analyzed by extended X-ray absorption fine structure. Figure 1j As shown. Figure 1j It can be seen that Pd1Cu SAA There is an obvious peak (blue line) that can be attributed to the Pd-Cu bond, but no The peak corresponding to Pd-Pd (black line) is detected, which verifies that Pd exists in a single atomic form.
[0135] Electrochemical polarization analysis was performed on the catalysts prepared in Example 4 and Comparative Example 1. The specific detection method was as follows: using an electrochemical workstation and an H cell to detect the presence or absence of NO3 on different catalysts. - When (50mL 1MKOH±2000ppm NO3 - The polarization curve of electrolyte) was tested with a 1cm*1cm platinum sheet as the counter electrode and Hg / HgO as the reference electrode. The test results are as follows Figure 2a As shown, palladium nanoparticles (Pd NPs) and comparative example 1 are used as the control group. Figure 2a It can be seen that Pd1Cu SAA in the presence of NO3 - The current density increases the most when NO3 is present (red solid line), indicating that it has the highest electrochemical - Restore capability.
[0136] Taking palladium nanoparticles (Pd NPs) and comparative example 1 as the control group, the removal of NO3 by Example 4 and the control group was analyzed. - Ability, the specific detection method is: UV-visible spectrophotometry, the test results are as follows Figure 2b As shown. Figure 2b It can be seen that Pd1Cu SAA can remove almost 100% of NO3 in the applied potential range (-0.9 to -1.3 V vs. Hg / HgO). - , which is significantly higher than that of Pd NPs and Comparative Example 1.
[0137] The ammonia (NH3) production capacity of Example 4 and the control group was analyzed by using palladium nanoparticles (Pd NPs) and comparative example 1 as the control group. The specific detection method was: UV-visible spectrophotometry. The detection results were as follows: Figure 2c As shown. Figure 2cIt can be seen that by comparing the NH3 production capabilities of the three catalysts, it is found that in the entire potential range, the Faradaic efficiency (NH3 FE) of Pd1Cu SAA for NH3 is significantly higher than that of Cu and Pd NPs. At -1.1V, the catalyst Pd1Cu SAA prepared in Example 4 reaches its highest NH3 FE of 95%.
[0138] The product distribution of the catalysts prepared in Example 4 and Comparative Example 1 when electro-reducing nitrate at -1.1 V vs. Hg / HgO was analyzed. The specific detection method was: UV-visible spectrophotometry. The detection results were as follows: Figure 2d As shown. Figure 2d It can be seen that Pd1Cu SAA electroreduces NO3 - The kinetics of the reaction are the fastest (blue solid line), and the reaction is basically completely converted into NH3 after 2 hours, and no NO2 can be detected. - The presence of NO3-N is lower than the US Environmental Protection Agency's drinking water standard (NO3-N: 10 mg / L; NO2-N: 1 mg / L), while the Cu catalyst still has more than 200 mg / L NO2 after 2 hours of reaction. - -N is retained in the water (yellow dashed line), which indicates that the addition of palladium enhances the ability of Cu to undergo deep hydrodeoxygenation. Figure 2e It can be seen that after 2h of reaction, the selectivity of Pd1Cu SAA for NH3 is close to 100%. Figure 2f It can be seen that after 2h of reaction, the yield of NH3 by Pd1Cu SAA is close to 2.0mM / (h×cm 2 ). The selectivity of NH3 is the amount of NH3 detected after 2 hours of reaction divided by the initial NO3 - The amount of substance. The Faraday efficiency of NH3 can be calculated by the following formula (where: V is the volume of the electrolyte: 50mL; C NH4+ is the concentration of NH4 after 2 hours of reaction: mol / mL, F = 96485C / mol, Q is the total charge involved in the reaction during the electrolysis process):
[0139]
[0140] In summary, in the catalyst provided by the present invention, palladium is anchored on the copper crystal surface in the form of a single atom. The introduction of palladium single atoms can significantly improve the kinetics of copper reduction of nitrate, improve the Faraday efficiency of the product ammonia, and promote the deep reduction of nitrite to ammonia.
[0141] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A catalyst, characterized in that It includes a catalyst carrier and metal nanowires loaded on the surface of the catalyst carrier; Wherein, the catalyst carrier comprises copper foam; The metal nanowire is a hollow structure and includes single-element copper and single-atom palladium.
2. The catalyst according to claim 1, characterized in that The mass ratio of elemental copper to monatomic palladium in the catalyst is 100:(0.1-2).
3. The catalyst according to claim 1, characterized in that The average diameter of the metal nanowires is 100 to 400 nm; and / or, The average diameter of the hollow structure is 80-300 nm.
4. The method for preparing the catalyst according to any one of claims 1 to 3, characterized in that: The following steps are involved: S10, obtaining a base copper foam, wherein the base copper foam includes a copper foam having first nanowires grown on the surface thereof, wherein the first nanowires include an insoluble copper compound; S20, mixing the base copper foam and the palladium solution to cause an ion replacement reaction, so that the copper ions in a part of the insoluble copper salt are replaced by palladium ions, and a palladium-loaded base copper foam is obtained; S30, calcining the palladium-loaded copper foam substrate under an inert gas; S40, performing reduction treatment on the palladium-loaded substrate foam copper that has completed the calcination treatment to obtain a catalyst.
5. The method for preparing the catalyst according to claim 4, characterized in that: Step S10 includes: The base copper foam is prepared by electrochemical oxidation method.
6. The method for preparing the catalyst according to claim 5, characterized in that: The constant current density of the electrochemical oxidation method is 15-25 mA / cm 2 and / or, The oxidation time of the electrochemical oxidation method is 10 to 30 minutes.
7. The method for preparing the catalyst according to claim 4, characterized in that: In step S20: The palladium ion concentration in the palladium solution is 1 to 100 mM; and / or, The ion exchange reaction time is 10 to 40 minutes; and / or, Mixing the base copper foam and the palladium solution includes: adding 114 g of the base copper foam to each liter of the palladium solution.
8. The method for preparing the catalyst according to claim 4, characterized in that: In step S30: The inert gas includes at least one of argon and nitrogen; and / or, The calcination temperature is 180-220°C; and / or, The heating rate of the calcination is 4-10°C / min; and / or, The calcination time is 1.5 to 2.5 hours.
9. The method for preparing a catalyst according to claim 4, characterized in that: Step S40 includes: The palladium-loaded copper foam substrate that has undergone calcination is subjected to electrochemical reduction treatment to obtain a catalyst; Wherein, the electrochemical reduction includes a first reduction treatment and a second reduction treatment; The constant current density of the first reduction treatment is 80-120 mA / cm 2 and / or, The reduction time of the first reduction treatment is 1.5 to 2.5 hours; and / or, The constant current density of the second reduction treatment is 650-750 mA / cm 2 and / or, The reduction time of the second reduction treatment is 0.8 to 1.2 hours.
10. Use of the catalyst according to any one of claims 1 to 3 or the catalyst prepared by the method for preparing the catalyst according to any one of claims 4 to 9 in treating wastewater.
Citation Information
Patent Citations
Preparation method and application of mesoporous palladium-copper nano-catalyst for reducing nitrate to produce ammonia
CN115584527A
Self-supporting CuO loaded Ir monatomic electrocatalyst as well as preparation method and application thereof
CN117026279A
Copper-palladium-loaded mesoporous silicon carbide-based catalyst, preparation method and application thereof
US20210404077A1
Cited By
Metal-loaded three-dimensional copper-based catalyst as well as preparation method and application thereof
CN119352092A
Metal-loaded three-dimensional copper-based catalyst, its preparation method and application