Gas turbine moving blade top rebuilding process capable of repairing welding cladding line cracks

Through the welding protection process, welding cladding process and brazing cladding process, combined with argon gas protection and high-temperature brazing technology, the problem of defects in the repair of the moving blade tip in the traditional welding process is solved, and a repair effect with a high success rate is achieved. .

CN118848422APending Publication Date: 2024-10-29HUARUI (JIANGSU) GAS TURBINE SERVICE CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410971740.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Traditional welding technology is prone to defects such as pores and cracks during the repair process of gas turbine rotor blade tips, resulting in reduced service life of the rotor blades and low repair success rate.

Method used

The welding protection process, welding cladding process and brazing cladding process are adopted, including the use of argon gas shielded welding, fine welding line energy control and high temperature brazing cladding, combined with ultrasonic degreasing, sandblasting cleaning and vacuum brazing technology to ensure There are no cracks in the welding area.

Benefits of technology

The success rate of moving blade tip repair is improved from the original 60% to more than 99%, which avoids the occurrence of welding defects and extends the service life of the moving blade.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118848422A_ABST
    Figure CN118848422A_ABST
Patent Text Reader

Abstract

The invention discloses a gas turbine moving blade top rebuilding process capable of repairing welding cladding line cracks, a blade is rebuilt through a welding protection process, a welding cladding process and a brazing cladding process, and a welding protection box body is arranged, so that a moving blade is completely placed in a uniform argon atmosphere through blade top welding; performance adjustment is achieved by setting optimal welding parameters, and brazing cladding is achieved through the method that gaps of solid components are filled with liquid brazing filler metal to enable metal to be connected and welded. According to the method, the blade tops of the moving blades of different types can be repaired, the repairing process combines an argon arc welding cladding process and a brazing cladding process, is different from a traditional blade repairing process and is particularly suitable for the situation that moving blade materials are degraded and are not prone to welding due to long-time operation, various defects are not generated any more after repairing, and the repairing efficiency is improved. And the repair success rate is increased to 99% or above from the original 60%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a gas turbine rotor blade tip reconstruction process capable of repairing welding cladding line cracks, and belongs to the technical field of gas turbines. Background Art

[0002] The rapid development of the heavy-duty gas turbine industry has put forward higher and higher requirements on the efficiency of gas turbines. However, the gap between the tip of the turbine blade and the casing is one of the important factors that reduce the overall efficiency of the gas turbine and increase the gas consumption. Clearance control is an important technical measure to reduce the fuel consumption rate of the gas turbine, improve reliability and extend the service life by controlling the change of the tip clearance of the turbine components. It also makes a great contribution to reducing the emission of pollutants. For every 0.075mm increase in the radial clearance of the high-pressure turbine components, the fuel loss increases by an average of 1%. During the operation of the gas turbine, grinding occurs between the blade tip and the compound ring, so the repair and reconstruction of the blade tip is an indispensable process in the repair process of the blade.

[0003] Generally, the argon arc welding and nickel-based alloy cladding process is used to repair the blade tips. The traditional welding process is prone to defects such as pores and cracks due to welding parameter mismatch, poor welding protection effect, and heat treatment stress release. This seriously affects the quality of welding cladding and greatly reduces the service life of the blades. This invention combines three major processes to ultimately solve this difficulty and achieve crack-free reconstruction of the blade tip. The three key processes are as follows: 1. Welding protection process; 2. Welding cladding process; 3. Brazing cladding process. Figure 1-Figure 3 As shown in the figure, some typical defects are produced after the blade tip is repaired by cladding welding using traditional welding technology and then subjected to post-weld heat treatment. In the actual production process, due to the excessive operation of the moving blades and the degradation of the material, a large number of cases often occur after post-weld heat treatment, the stress in the welding fusion line area is released, and the material has thermal cracks (such as Figure 3 As shown in the figure, it is necessary to design a process so that no cracks are found in all the moving blade welding areas after flaw detection, slice analysis and other means, so as to effectively achieve repair. Summary of the invention

[0004] In view of the problems existing in the above-mentioned prior art, the present invention provides a gas turbine rotor blade tip reconstruction process that can repair weld cladding line cracks, thereby solving the above-mentioned technical problems.

[0005] In order to achieve the above-mentioned object, the technical solution adopted by the present invention is: a gas turbine rotor blade tip reconstruction process capable of repairing weld cladding line cracks, comprising the following steps:

[0006] Step S1: welding protection process,

[0007] Specifically, argon is selected as the shielding gas; a welding shielding box is designed so that the blade tip welding completely places the moving blade in a uniform argon atmosphere;

[0008] Step S2: welding cladding process,

[0009] Specifically, use a smaller welding line energy during welding, control the interlayer temperature, and use a small current, thin welding wire, fast welding, and short arc welding to ensure good fusion of the weld.

[0010] Step S3: brazing cladding process,

[0011] Specifically, step S31: pretreatment of the surface of the component: ultrasonic alkaline washing and degreasing treatment is performed on the moving blades, the moving blades are placed in a cleaning device, heated to 50-70 degrees Celsius for insulation, and maintained at this temperature for 20-50 minutes, and then the moving blades are taken out and placed in a clean water tank for rinsing, and then placed in an oven for drying and finally cooled to below 30°C;

[0012] Step S32: Component degreasing: heating the moving blades to remove oil and grease; in an air circulation furnace, 330°C, 1H;

[0013] Step S33: Preliminary cleaning of the brazing area: sandblasting is used to perform necessary cleaning on the moving blades, wherein the sandblasting gun forms an angle of 20-60° with the sandblasting area of ​​the blades, the sandblasting pressure is 2-7 Bar, and the sandblasting cleaning material is corundum;

[0014] Step S34: Clean the brazing area again: Use nickel shot sandblasting to clean the brazing area surface again, wherein the sandblasting gun forms an angle of 20-60° with the spraying area of ​​the blade, and the sandblasting pressure is 2-7 Bar;

[0015] Step S35: Clean the inside of the component: Use compressed air to blow the inside of the blade to clean the residual nickel sand and other impurities inside the component;

[0016] Step S36: coating the coating, using a glass cup to hold the prepared special brazing material, adding a large amount of acetone solution, using a stirrer to stir the brazing material to form a special brazing paste, and using a brush to brush the brazing material to the argon arc welding surfacing area of ​​the blade top while stirring;

[0017] Step S37: vacuum brazing: put the moving blade into a vacuum furnace, use a blade molybdenum rack to place it upside down, use heat treatment process parameters to perform high-temperature brazing, so that the brazing material is completely penetrated, the cracks are covered, and the welding stress is released at the same time; quickly heat up to 1150-1230°C at a heating rate of 15-30°C / min, and keep warm for 15-30 minutes; the vacuum furnace equipment power is slowly reduced to 1050-1120°C at a cooling rate of 10-20°C / min, and then cooled to 900-1020°C with the furnace; inject 150mbar argon gas and cool to 700-850°C at a rate of 15-20°C / min, and then quickly cool; quickly cool at a rate of 20-30°C / min, inject 1000-1400mbar argon gas during rapid cooling, and turn on the rapid cooling fan at the same time. After the furnace temperature drops to 60°C, open the furnace door to let the moving blades drop to 30°C before taking them out;

[0018] Step S38: Grinding after brazing: After brazing, grind the brazing material to make it smooth.

[0019] Furthermore, in step S1, the welding protection box includes a box; a screw lifting mechanism is arranged in the box; the screw lifting mechanism includes a lifting platform on which the screw is arranged; a positioning fixture is arranged on the lifting platform; the positioning fixture is used to clamp the root of the moving blade; an argon diffusion device and left and right double argon channels are also arranged in the box; a turntable device is arranged at the bottom outer side of the box.

[0020] Furthermore, in step S2, the number of welding layers is 3-9 layers, the welding speed is 15-20 cm / min, the welding current is 40-55 A, the welding voltage is 8.5-9.3 V, the shielding gas is argon, the shielding gas flow rate is 10-15 L / min, the air flow rate in the welding protection box is 10-40 L / min, the preheating temperature is >0°C, and the interlayer temperature is <150°C.

[0021] Furthermore, in step S36, the special solder paste is mixed with special solder, glue and acetone, and the ratio of the components of the special solder, glue and acetone is 17:1:1. The special solder is mixed with a solder with a melting point of 1455-1900°C and a solder with a melting point of 1121-1218°C in a ratio of 2:1.

[0022] The beneficial effects of the present invention are as follows: the present invention can realize the repair of the blade tips of different models of moving blades by rebuilding the blades through welding protection process, welding cladding process and brazing cladding process. This repair process combines argon arc welding cladding and brazing cladding processes, which is different from the traditional blade repair process. It is particularly suitable for the situation where the moving blade material is difficult to weld due to degradation due to long-term operation. After the repair, various defects will no longer occur, and the repair success rate has been increased from the original 60% to more than 99%. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A schematic diagram of a crack defect caused by conventional welding repair in the background technology of the present invention;

[0024] Figure 2 A schematic diagram of pores and interlayer defects produced by traditional welding repair in the background technology of the present invention;

[0025] Figure 3 A schematic diagram of a crack defect after heat treatment by conventional welding repair in the background technology of the present invention;

[0026] Figure 4 Schematic diagram showing blades of different models in an embodiment of the present invention;

[0027] Figure 5 Schematic diagram of the tip welding area of ​​blades of different models in the embodiment of the present invention;

[0028] Figure 6 This is a schematic diagram of the structure of a welding protection box in an embodiment of the present invention;

[0029] Figure 7 The metallographic structure diagram of welding with final welding parameters in the embodiment of the present invention;

[0030] Figure 8 This is a schematic diagram of the top structure of a blade after repair according to an embodiment of the present invention;

[0031] Fig. 9 It is a schematic diagram of the brazing cladding process flow of an embodiment of the present invention.

[0032] In the attached drawings, 1. box body, 2. screw lifting mechanism, 21. screw, 22. lifting platform, 3. positioning fixture, 4. argon diffusion device, 5. double argon gas channel, 6. turntable device. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below through the accompanying drawings and embodiments. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of the present invention.

[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0035] This invention combines three major processes to finally solve this difficulty and achieve crack-free reconstruction of the blade tip. The three key processes are as follows: 1. Welding protection process; 2. Welding cladding process; 3. Brazing cladding process.

[0036] 1. Welding protection process

[0037] The welding protection process is a key factor in achieving arc temperature combustion, determining arc column heat distribution, improving process stability and achieving deep fusion welding. Moreover, for the welding molten pool, the protection process is a necessary means to prevent oxidation and contamination of the high-temperature welding molten pool. Therefore, formulating a suitable welding protection process is a necessary prerequisite for conducting research on blade tip repair technology.

[0038] Inert gases helium and argon are the most commonly used welding shielding gases, but since helium is very expensive, more than 20 times that of argon, and helium has a lower density, more helium is required to achieve the same shielding effect as argon. Considering the production cost comprehensively, argon was finally selected as the shielding gas.

[0039] The blade tip welding must be carried out by placing the moving blade completely in a uniform argon atmosphere to achieve the best protection effect. Therefore, a welding gas protection box is designed to fix the blade in an argon atmosphere for welding. The designed welding protection box must solve the following problems:

[0040] 1. Convenient model change: Huarui Company undertakes maintenance of various models, including GE, Siemens, Mitsubishi and other models. The height and shape of the moving blades of different models are different. For details, see Figure 4 , so the designed welding protection box must be able to quickly adapt to all types of moving blades;

[0041] 2. Easy to operate: Due to the different blade top shapes of different models Figure 5 Therefore, the designed welding protection box must have the characteristics of easy operation to facilitate the welding operator to achieve different welding process requirements.

[0042] 3. Adequate protection: The argon protection atmosphere is extremely important in the welding process, so the designed welding protection box must have the best protection and sealing effect.

[0043] In view of the above three key points, the schematic diagram of the blade tip welding protection box is designed and produced as shown below: Figure 6 As shown, the welding protection box includes a box 1; a screw lifting mechanism 2 is arranged in the box 1; the screw lifting mechanism 2 includes a screw 21 and a lifting platform 22 arranged on the screw 21; a positioning fixture 3 is arranged on the lifting platform 22; the positioning fixture 3 is used to clamp the root of the moving blade; an argon diffusion device 4 and left and right double argon channels 5 are also arranged in the box 1; a turntable device 6 is arranged at the bottom of the outer side of the box 1.

[0044] The welding protection box is provided with a screw lifting mechanism in the welding box body, thereby solving the problem of lengthy model change caused by the non-uniform blade tip heights of different models of moving blades; at the same time, a universal positioning fixture structure is provided, so that the moving blades of all different models can be positioned by simply adjusting the screw installation position, which is convenient and reliable; a rotating structure is provided at the bottom of the box body, so that when dealing with welding areas of different shapes, the operator can easily rotate and move it to meet the requirements of different welding processes; a double argon protection inlet is designed above the protection box (close to the blade tip welding part), and an argon diffusion device is added at the inlet, so that the argon gas is fully diffused, so that the welding area is fully immersed in a uniform argon protection atmosphere, and all openings are specially sealed to ensure the sealing effect of the protection box, effectively improve the welding quality, and reduce argon gas waste.

[0045] 2. Welding cladding process

[0046] The base materials of heavy-duty combustion engine blades are all high-temperature nickel-based alloy materials. Nickel-based alloys are different from traditional alloy materials and are unidirectional. Traditional welding is prone to macro cracks and micro cracks in the weld. The most common defects in nickel-based alloy welding are thermal cracks and pores. The weldability of nickel-based alloy steel is not very good. Reasonable welding technology and corresponding measures must be adopted during welding to avoid various welding defects.

[0047] Due to the poor thermal conductivity of nickel-based alloys, smaller welding line energy should be used as much as possible during welding, and the interlayer temperature should be controlled as much as possible. When ensuring good fusion of the weld, small current, thin welding wire, fast welding and short arc welding should be used as much as possible.

[0048] Through a large number of orthogonal comparison tests, the metallographic structure and various properties of the test pieces with different welding parameters were analyzed, and then various tests were adjusted to finally obtain the optimal welding parameters (see Table 1 below).

[0049]

[0050] After welding, all indicators, non-destructive testing, metallographic structure, welding head strength, etc. have reached the optimal level. The metallographic structure of the welding with this welding parameter is shown in Figure 7 .

[0051] 3. Brazing cladding process

[0052] After repeated research, it was found that the high-temperature nickel-based alloy brazing cladding process is a suitable means to solve this problem. High-temperature brazing refers to a method of welding metals by using liquid brazing filler metal to fill the gaps in solid parts after the brazing filler metal and the weldment are heated to the melting temperature of the brazing filler metal at a temperature lower than the melting point of the weldment.

[0053] Final determination of qualified brazing process:

[0054] First, the surface of the parts is pretreated: the moving blades are subjected to ultrasonic alkaline washing and degreasing treatment, the moving blades are placed in a cleaning device, heated to 50-70 degrees Celsius for insulation, and maintained at this temperature for 20-50 minutes, and then the moving blades are taken out and placed in a clean water pool for rinsing, and then placed in an oven for drying and finally cooled to below 30°C.

[0055] Then, the parts are degreased: the moving blades are heated to remove oil and grease; in an air circulation furnace, 330℃, 1H.

[0056] Next, the brazing area is preliminarily cleaned: sandblasting is used to clean the moving blades as necessary, wherein the sandblasting gun forms an angle of 20-60° with the sandblasting area of ​​the blades, the sandblasting pressure is 2-7 Bar, and the sandblasting cleaning material is corundum;

[0057] Then, the brazing area is cleaned again: the surface of the brazing area is cleaned again by using nickel shot blasting, wherein the sandblasting gun forms an angle of 20-60° with the spraying area of ​​the blade, and the sandblasting pressure is 2-7 Bar; using nickel shot for cleaning helps to improve the surface bonding strength.

[0058] Next, clean the inside of the component: use compressed air to blow the inside of the blade to clean the residual nickel sand and other impurities inside the component;

[0059] Then, a glass cup is used to hold the prepared brazing material, a large amount of acetone solution is added, the brazing material is stirred by a stirrer, and the brazing material is brushed to the argon arc welding surfacing area of ​​the blade top with a brush while stirring; the special brazing paste is mixed with special brazing material, glue and acetone, and the ratio of each component of the special brazing material, glue and acetone is 17:1:1; the special brazing material is mixed with a brazing material with a melting point of 1455-1900°C and a brazing material with a melting point of 1121-1218°C in a ratio of 2:1.

[0060] Secondly, vacuum brazing: put the moving blade into a vacuum furnace, place it upside down on a molybdenum rack specially designed for the blade, and use heat treatment process parameters for high-temperature brazing to make the brazing material fully penetrate, cover the cracks, and release the welding stress at the same time; quickly heat up to 1150-1230℃ at a heating rate of 15-30℃ / min, and keep warm for 15-30 minutes; the vacuum furnace equipment power is slowly reduced to 1050-1120℃ at a cooling rate of 10-20℃ / min, and then cooled to 900-1020℃ with the furnace; inject 150mbar argon gas and cool to 700-850℃ at a speed of 15-20℃ / min, and then cool rapidly; rapidly cool at a rate of 20-30℃ / min, and inject 1000-1400mbar argon gas during rapid cooling, and turn on the rapid cooling fan at the same time. After the furnace temperature drops to 60℃, open the furnace door to let the moving blades drop to 30℃ before taking them out.

[0061] Finally, polishing after brazing: After brazing, polish the brazing material to make the transition smooth.

[0062] After using this brazing cladding process, all the moving blade welding areas were tested by flaw detection, slice analysis and other means, and no cracks were found, and the repair was effectively achieved. Figure 8 .

[0063] The present invention can realize the repair of the blade tips of different models of moving blades through the research and development of welding protection technology, welding cladding technology and brazing cladding technology. This repair technology combines argon arc welding cladding and brazing cladding technology, which is different from the traditional blade repair technology. It is particularly suitable for the situation where the moving blade material is difficult to weld due to degradation due to long-term operation. After the repair, various defects will no longer occur, and the repair success rate has been increased from the original 60% to more than 99%.

[0064] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A gas turbine blade tip reconstruction process capable of repairing weld cladding line cracks. It is characterized in that The following steps are involved: Step S1: welding protection process, Specifically, argon is selected as the shielding gas; a welding shielding box is designed so that the blade tip welding completely places the moving blade in a uniform argon atmosphere; Step S2: welding cladding process, Specifically, use a smaller welding line energy during welding, control the interlayer temperature, and use a small current, thin welding wire, fast welding, and short arc welding to ensure good fusion of the weld. Step S3: brazing cladding process, Specifically, step S31: pretreatment of the surface of the component: ultrasonic alkaline washing and degreasing treatment is performed on the moving blades, the moving blades are placed in a cleaning device, heated to 50-70 degrees Celsius for insulation, and maintained at this temperature for 20-50 minutes, and then the moving blades are taken out and placed in a clean water tank for rinsing, and then placed in an oven for drying and finally cooled to below 30°C; Step S32: Component degreasing: heating the moving blades to remove oil and grease; in an air circulation furnace, 330°C, 1H; Step S33: Preliminary cleaning of the brazing area: sandblasting is used to perform necessary cleaning on the moving blades, wherein the sandblasting gun forms an angle of 20-60° with the sandblasting area of ​​the blades, the sandblasting pressure is 2-7 Bar, and the sandblasting cleaning material is corundum; Step S34: Clean the brazing area again: Use nickel shot sandblasting to clean the brazing area surface again, wherein the sandblasting gun forms an angle of 20-60° with the spraying area of ​​the blade, and the sandblasting pressure is 2-7 Bar; Step S35: Clean the inside of the component: Use compressed air to blow the inside of the blade to clean the residual nickel sand and other impurities inside the component; Step S36: coating the coating, using a glass cup to hold the prepared special brazing material, adding a large amount of acetone solution, using a stirrer to stir the brazing material to form a special brazing paste, and using a brush to brush the brazing material to the argon arc welding surfacing area of ​​the blade top while stirring; Step S37: vacuum brazing: put the moving blade into a vacuum furnace, use a blade molybdenum rack to place it upside down, use heat treatment process parameters to perform high-temperature brazing, so that the brazing material is completely penetrated, the cracks are covered, and the welding stress is released at the same time; quickly heat up to 1150-1230°C at a heating rate of 15-30°C / min, and keep warm for 15-30 minutes; the vacuum furnace equipment power is slowly reduced to 1050-1120°C at a cooling rate of 10-20°C / min, and then cooled to 900-1020°C with the furnace; inject 150mbar argon gas and cool to 700-850°C at a rate of 15-20°C / min, and then quickly cool; quickly cool at a rate of 20-30°C / min, inject 1000-1400mbar argon gas during rapid cooling, and turn on the rapid cooling fan at the same time. After the furnace temperature drops to 60°C, open the furnace door to let the moving blades drop to 30°C before taking them out; Step S38: Grinding after brazing: After brazing, grind the brazing material to make it smooth.

2. A gas turbine rotor blade tip reconstruction process capable of repairing weld cladding line cracks according to claim 1, It is characterized in that In the step S1, the welding protection box comprises a box (1); a screw lifting mechanism (2) is arranged in the box (1); the screw lifting mechanism (2) comprises a screw (21) and a lifting platform (22) arranged on the screw (21); a positioning fixture (3) is arranged on the lifting platform (22); the positioning fixture (3) is used to clamp the root of the moving blade; an argon diffusion device (4) and left and right double argon channels (5) are also arranged in the box (1); and a turntable device (6) is arranged at the outer bottom of the box (1).

3. A gas turbine rotor blade tip reconstruction process capable of repairing weld cladding line cracks according to claim 1, It is characterized in that In the step S2, the number of welding layers is 3-9 layers, the welding speed is 15-20 cm / min, the welding current is 40-55 A, the welding voltage is 8.5-9.3 V, the shielding gas is argon, the shielding gas flow rate is 10-15 L / min, the air flow rate in the welding protection box is 10-40 L / min, the preheating temperature is >0°C, and the interlayer temperature is <150°C.

4. A gas turbine rotor blade tip reconstruction process capable of repairing weld cladding line cracks according to claim 1, It is characterized in that In step S36, the special solder paste is mixed with special solder, glue and acetone, and the ratio of the special solder, glue and acetone is 17:1:

1. The special solder is mixed with solder with a melting point of 1455-1900°C and solder with a melting point of 1121-1218°C in a ratio of 2:1.

Citation Information

Patent Citations

  • Hot working method of nickel-based superalloy workpiece and product

    CN116607088A

  • Method of repairing a stator vane of gas turbine without removing all the cracks , repaired gas turbine

    CN1734061A

  • Crack repair process for high-pressure turbine blade tip in gas turbine

    CN1883872A

  • Induction heating device for repairing blade tip of turbine blade

    CN213969585U

  • Method for repairing parts composed of superalloys

    EP1705338A1