Energy storage box and welding method thereof

Through cold metal transfer technology CMT welding and plug embedded structure, the problems of welding stress concentration and air tightness of the energy storage box are solved, the structural strength and air tightness are improved, and the production cost and hidden dangers are reduced.

CN118848432APending Publication Date: 2024-10-29SICHUAN TIANJUN PRECISION COMPONENTS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410932234.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-29

Smart Images

  • Figure CN118848432A_ABST
    Figure CN118848432A_ABST
Patent Text Reader

Abstract

The invention relates to an energy storage box and a welding method thereof, and the welding method adopts a cold metal transition technology (CMT) and comprises the following steps: material selection; a runner plate is welded; processing a runner plate; the plug strip is welded with the runner plate; the end plate is welded with the runner plate; welding spare parts; and checking air tightness. According to the invention, the traditional insertion and butt joint mode of the plug strip and the runner plate is changed into an embedded mode, so that the structure of the energy storage box body is optimized; a cold metal transition technology CMT welding method is adopted, the welding sequence of a skip bay method is designed, the heat input amount is dispersed, the local temperature is reduced, cracks are prevented, then the welding deformation amount is small, the production and manufacturing cost is reduced, the production efficiency is improved, and the problems of welding stress, cracks and the like in the production process of the energy storage box are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of energy storage systems, and in particular to an energy storage box and a welding method thereof. Background Art

[0002] The popularity of new energy vehicles has led to the continuous optimization of vehicle lightweighting and internal space requirements, while also placing higher requirements on the structural strength of energy storage boxes. During the design process, more consideration is given to the selection of material thickness and structural optimization. Sometimes, some structures may experience stress concentration and weld cracking during welding, which may lead to poor airtightness and leakage in the energy storage box during production and use, seriously endangering life safety. Welding stress concentration can directly lead to welding cracks. When the energy storage box is undergoing an airtightness test, leakage may occur at the crack position. If some tiny cracks cannot be detected, it may cause some great hidden dangers after installation, such as leakage and spontaneous combustion.

[0003] The original design of the plug strip at the sealing part of the flow plate of the energy storage box adopts a T-shaped structure. It is inserted into the flow plate and forms a butt joint with the flow plate, so that the weld is left on the upper and lower surfaces of the flow plate. Due to the close distance between the welds and partial overlap, the local heat input is too large and the stress increases, which leads to cracks. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide an energy storage box and a welding method thereof to solve one or more problems in the prior art.

[0005] To achieve the above object, the technical solution of the present invention is as follows:

[0006] A welding method, which adopts cold metal transfer technology (CMT), comprises the following steps:

[0007] Material selection;

[0008] Manifold plate welding;

[0009] Runner plate processing;

[0010] The plug strip is welded to the flow channel plate;

[0011] Welding of end plate and runner plate;

[0012] Welding of loose parts;

[0013] Air tightness check.

[0014] Furthermore, the material selection includes that the materials of the end plate, the side plate, the flow channel plate, and the plug strip are all one or more of 6 series aluminum alloys.

[0015] Furthermore, the shoulder of the flow channel plate welding is 10 mm, the needle length is 3.5 mm, the welding speed is 800-1300 mm / min, the welding needle speed is 2500-3600 rpm, and the welding pressure is 2850N-3850N.

[0016] Furthermore, the milling cutter speed for machining the flow channel plate is S3000-4500 r / min, and the travel speed is F200-800 mm / min.

[0017] Furthermore, the plug strip and the flow channel plate are welded in the following order:

[0018] The first section is welded;

[0019] The third section is welded;

[0020] The second section welding;

[0021] Fourth section welding.

[0022] Furthermore, the welding direction of the plug strip and the flow channel plate is the first direction.

[0023] Furthermore, the welding current of the plug strip and the flow channel plate is 70-110A, and the welding speed is 30-60cm / min.

[0024] Furthermore, the welding current of the end plate and the flow channel plate is 90-130A, and the welding speed is 45-65cm / min.

[0025] Furthermore, the welding current of the loose parts welding is 100-140A, and the welding speed is 50-60cm / min.

[0026] An energy storage box is formed by welding using the above-mentioned welding method. The energy storage box comprises the side plates, the end plates and the flow channel plate. The side plates are respectively connected to the end plates and the flow channel plate. The end plates are respectively connected to the side plates and the flow channel plate. The flow channel plate is provided with a cavity. The energy storage box also comprises a plugging strip embedded in the cavity.

[0027] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0028] The present invention changes the traditional insertion and docking mode of the plug strip and the flow channel plate into an embedding mode, thereby optimizing the energy storage box structure; adopts the cold metal transition technology CMT welding method and designs the welding sequence of the skip-bin method to disperse the heat input, reduce the local temperature, prevent the occurrence of cracks, and thus reduce the welding deformation, reduce the production cost, improve the production efficiency, and solve the problems of welding stress, cracks, etc. of the energy storage box during the production process. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic structural diagram of an energy storage box and a welding method thereof in which plugging strips are not assembled is shown in an embodiment of the present invention.

[0030] Figure 2 A schematic diagram showing the structure of a plug assembly of an energy storage box and a welding method thereof according to an embodiment of the present invention Figure Ⅰ .

[0031] Figure 3 A schematic structural diagram of a plugging strip of an energy storage box and a welding method thereof according to an embodiment of the present invention is shown.

[0032] Figure 4 A schematic diagram showing the welding sequence of a plug strip and a flow channel plate of an energy storage box and a welding method thereof according to an embodiment of the present invention.

[0033] Figure 5 A schematic diagram showing the structure of a plug assembly of an energy storage box and a welding method thereof according to an embodiment of the present invention Figure II .

[0034] Figure 6 A schematic cross-sectional structure diagram along the AA direction of an energy storage box and a welding method thereof according to an embodiment of the present invention is shown.

[0035] Figure 7 A partial enlarged view showing an energy storage box and a welding method thereof after plugging after assembly according to an embodiment of the present invention Figure Ⅰ .

[0036] Figure 8 A partial enlarged view showing an energy storage box and a welding method thereof after plugging after assembly according to an embodiment of the present invention Figure II .

[0037] Fig. 9 A schematic flow chart of a welding method for an energy storage box and a welding method thereof according to an embodiment of the present invention is shown.

[0038] Markings in the accompanying drawings: 1, side plate; 2, end plate; 3, flow channel plate; 301, cavity; 4, plug strip; 401, first section; 402, second section; 403, third section; 404, fourth section. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical scheme and advantages of the present invention clearer, the energy storage box and its welding method proposed by the present invention are further described in detail in combination with the accompanying drawings and specific embodiments. According to the following description, the advantages and features of the present invention will be clearer. It should be noted that the drawings are in a very simplified form and use non-precise proportions, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, please refer to the accompanying drawings. It should be noted that the structure, proportion, size, etc. illustrated in the drawings of this specification are only used to match the content disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions for the implementation of the present invention, so they have no technical substantive significance. Any structural modification, change in proportional relationship or adjustment of size, without affecting the effect that the present invention can produce and the purpose that can be achieved, should still fall within the scope of the technical content disclosed by the present invention.

[0040] See also Figures 1 to 3 , an energy storage box, the energy storage box includes a side plate 1, an end plate 2, and a flow channel plate 3, the side plate 1 is respectively connected to the end plate 2 and the flow channel plate 3, the end plate 2 is respectively connected to the side plate 1 and the flow channel plate 3, preferably, in this embodiment, the side plate 1, the end plate 2 and the flow channel plate 3 are connected by welding.

[0041] For further information, please refer to Figures 5 to 8 , the flow channel plate 3 is provided with a cavity 301, and the energy storage box body further includes a plugging strip 4, which can be embedded in the cavity 301. Compared with the traditional T-shaped structure, the plugging strip 4 in this embodiment requires less welding, which can fully avoid the weld seam, increase production efficiency, avoid stress concentration and micro cracks, and enhance structural strength. In addition, the previous T-shaped structure assembly is prone to excessive assembly gaps and dimensional tolerances. The current design does not need to consider the assembly gap problem, but only needs to ensure that the assembly is in place, which improves the assembly efficiency.

[0042] A welding method of this embodiment adopts cold metal transfer technology CMT, and realizes the alternation of hot and cold cycles in the welding process by coordinating wire feeding control and real-time monitoring. On the one hand, it reduces the welding heat input, and on the other hand, it improves the welding production efficiency. Because its voltage is lower than the ordinary welding voltage, the heat input is lower than the ordinary one, so it has great advantages in welding aluminum alloy thin plates and workpieces with low heat input requirements. The specific steps include the following steps, please continue to refer to Fig. 9 :

[0043] Step 1: Material Selection:

[0044] The material selection includes that the material of the end plate 2, the side plate 1, the flow channel plate 3, and the plug strip 4 are all one or more of 6 series aluminum alloys. Preferably, in this embodiment, AL6061-T6, i.e., 2 mm 6061 aluminum plate, is selected, which has the advantages of high strength and excellent welding forming.

[0045] Step 2: Welding of runner plate 3:

[0046] The flow channel plate 3 is welded, preferably by gantry friction stir welding, and the static shoulder is an important component in the friction stir welding technology. The shoulder remains stationary during the welding process, does not rotate with the stirring needle, and only moves along the welding direction, so it can effectively eliminate the burrs of the welding edge, provide greater forging pressure, and improve the strength of the joint. The shoulder of the flow channel plate 3 is 10mm, the needle length is 3.5mm, the welding speed is 800-1300mm / min, the welding needle speed is 2500-3600rpm, and the welding pressure is 2850N-3850N.

[0047] Step 3: Processing of runner plate 3:

[0048] The sides of both ends of the flow channel plate 3 are CNC-processed, and the movement of the machine tool and the tool is precisely controlled by a computer control system to achieve precise processing of parts. In order to add a plug strip to mill out space, the milling cutter speed for processing the flow channel plate 3 is S3000~4500r / min, and the travel speed is F200~800mm / min.

[0049] Step 4: Welding the plug strip 4 to the flow channel plate 3:

[0050] Please continue reading Figure 4 In this embodiment, the plug strip 4 is divided into four sections and welded by a jump welding method, namely, the first section 401 is welded, the third section 403 is welded, the second section 402 is welded, and the fourth section 404 is welded. The welding direction is the first direction, which is Figure 4 As shown from the left to the rear, by using the skip welding method, the welding heat input is dispersed, the local temperature is reduced, stress and strain are avoided, and the welding deformation is small, which reduces the production cost and improves production efficiency.

[0051] Furthermore, the welding current of the plugging strip 4 and the flow channel plate 3 is 70-110A, and the welding speed is 30-60cm / min.

[0052] Step 5: Welding of end plate 2 and runner plate 3:

[0053] The welding current of the end plate 2 and the flow channel plate 3 is 90-130A, and the welding speed is 45-65cm / min.

[0054] Step 6: Welding of loose parts:

[0055] The scattered parts of the energy storage box are welded to form a whole. When the scattered parts are welded, the welding current is 100-140A and the welding speed is 50-60cm / min.

[0056] When welding the entire energy storage box, pay attention to the changes in the molten pool, adjust the welding angle appropriately, increase the weld depth and effective thickness, and enhance the welding strength.

[0057] Step 7: Air tightness check:

[0058] The energy storage box is first inflated with high pressure using a known detection method, and then soapy water is sprayed on the welding part outside the energy storage box, and bubbles appearing in the soapy water are observed to detect its air tightness. If bubbles are generated, it indicates that there is a leak in the part, otherwise there is no leak.

[0059] Furthermore, airtightness tests are performed on the first section 401, the second section 402, the third section 403, and the fourth section 404 respectively. The airtightness test method is as described above. The method of the present invention can achieve a one-time pass rate of airtightness test of more than 97%, which is 32% higher than the traditional method of 65%.

[0060] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0061] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A welding method, the welding method adopts cold metal transfer technology CMT, characterized in that: The following steps are involved: Material selection; Manifold plate welding; Runner plate processing; The plug strip is welded to the flow channel plate; Welding of end plate and runner plate; Welding of loose parts; Air tightness check.

2. A welding method according to claim 1, characterized in that: The material selection includes that the materials of the end plate, the side plate, the flow channel plate, and the plug strip are all one or more of 6 series aluminum alloys.

3. A welding method according to claim 1, characterized in that: The shoulder of the flow channel plate welding is 10mm, the needle length is 3.5mm, the welding speed is 800-1300mm / min, the welding needle rotation speed is 2500-3600rpm, and the welding pressure is 2850N-3850N.

4. A welding method according to claim 1, characterized in that: The milling cutter speed for machining the flow channel plate is S3000-4500r / min, and the travel speed is F200-800mm / min.

5. A welding method according to claim 1, characterized in that: The plug strip and the flow channel plate are welded in the following order: The first section of welding; The third section is welded; The second welding section; The fourth section is welded.

6. A welding method according to claim 5, characterized in that: The welding direction of the plug strip and the flow channel plate is the first direction.

7. A welding method according to claim 6, characterized in that: The welding current of the plug strip and the flow channel plate is 70-110A, and the welding speed is 30-60cm / min.

8. A welding method according to claim 1, characterized in that: The welding current of the end plate and the flow channel plate is 90-130A, and the welding speed is 45-65cm / min.

9. A welding method according to claim 1, characterized in that: The welding current of the loose parts welding is 100-140A, and the welding speed is 50-60cm / min.

10. An energy storage box, the energy storage box is welded by a welding method according to any one of claims 1 to 9, the energy storage box comprises the side plate, the end plate, and the flow channel plate, the side plate is respectively connected to the end plate and the flow channel plate, the end plate is respectively connected to the side plate and the flow channel plate, the flow channel plate is provided with a cavity, characterized in that: The energy storage box also includes a plug, which is embedded in the cavity.

Citation Information

Patent Citations

  • Lower box body of integrated liquid-cooled battery pack

    CN113381090A

  • Battery box body assembly, battery pack and battery system

    CN115312923A

  • Battery box body assembly, battery pack and battery system

    CN116053647A

  • New energy water-cooling integrated box structure

    CN212783645U