Heat-conducting high-strength polypropylene composite sheet, fabric of heat-conducting high-strength polypropylene composite sheet, polypropylene composite and preparation method and application of polypropylene composite

Through the multi-layer structure of thermally conductive polypropylene sheets and fabrics, combined with homopolymerized and copolymerized polypropylene materials, the BAB' structure is designed, which solves the deficiencies in the mechanical and thermal conductive properties of existing polypropylene composite materials and achieves lower performance The inter-layer peel strength and thermal conductivity under hot pressing temperature are suitable for high-demand applications such as electronic components.

CN118849574AActive Publication Date: 2024-10-29CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310485612.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-29
Publication Date
2024-10-29
Estimated Expiration
2043-04-29

AI Technical Summary

Technical Problem

Existing polypropylene composite materials have shortcomings in having wide processing temperatures, strong mechanical properties, inter-layer peel strength and good thermal conductivity properties, making it difficult to meet high requirements such as electronic components.

Method used

It adopts multi-layer structure of thermally conductive polypropylene sheets and fabrics, which are prepared by co-extrusion molding and thermal pressing. It uses materials such as homopolypropylene, impact copolymerized polypropylene and random copolymerized polypropylene, combined with thermally conductive fillers and thermal bonding. Combined with reinforcing agents, the BAB' structure of layer A and layer B is designed to ensure interlayer peeling strength and thermal conductivity.

Benefits of technology

The polypropylene composite material has excellent mechanical properties and thermal conductivity at lower hot pressing temperatures, and is suitable for applications such as sheets, films, fabrics, etc., reducing equipment energy consumption and damage to materials caused by high-temperature operations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004211725120000221
    Figure BDA0004211725120000221
Patent Text Reader

Abstract

The invention relates to the field of polypropylene materials, and discloses a heat-conducting polypropylene sheet, a heat-conducting polypropylene fabric, a high-strength heat-conducting polypropylene composite material and a preparation method and application thereof. The heat-conducting polypropylene sheet comprises a thin film layer A containing a polypropylene composition A and a thin film layer B containing a polypropylene composition B. The thin film layers B on the two sides of the thin film layer Ai are the same or different. The heat-conducting polypropylene sheet is of a BAB sheet layer structure, and the thin film layers B are located on the two sides of the thin film layer A; wherein the polypropylene composition A comprises homo-polypropylene a, anti-impact co-polypropylene b and composite heat-conducting filler c; each polypropylene composition B comprises polypropylene random copolymer x, a heat bonding reinforcing agent y and a composite heat-conducting filler z. The polypropylene composite material obtained by hot-pressing the heat-conducting polypropylene sheet can simultaneously have good tensile property, impact resistance and heat-conducting property, and still has good interlayer peel strength when being prepared at a relatively low hot-pressing temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polypropylene materials, and more particularly to a thermally conductive polypropylene sheet, a thermally conductive polypropylene fabric, a high-strength thermally conductive polypropylene composite material, and a preparation method and application thereof. Background Art

[0002] With the development of miniaturization, miniaturization and multifunctionality of electronic products, the integration of electronic components is getting higher and higher, and the requirements for the heat dissipation performance of their materials are also getting higher and higher. However, the polymer materials commonly used in electronic components have poor thermal conductivity and can no longer meet the needs of further development of electronic products.

[0003] Polypropylene (PP) resin has a low density (0.89 ~ 0.91g / cm 3 ), good heat resistance, stiffness, hardness and other characteristics, which makes it have a wide range of applications.

[0004] The matrix and reinforcing phase of self-reinforced polymer composites are composed of different forms of the same polymer, and the reinforcing phase is usually a highly oriented fiber or flat ribbon. Most self-reinforced polymer composites are prepared using a hot pressing method. When the reinforcing phase is hot pressed at a certain pressure and temperature, the surface of the reinforcing phase fiber melts to become a matrix melt. The matrix melt and the reinforcing phase surface co-crystallize when melted, thereby providing sufficient interfacial bonding strength. As in US6312638B1, melt-spun oriented polyolefin fibers are hot pressed, and a specific temperature and pressure are used to partially melt-bond the surface layer of the polyolefin to prepare a polyolefin sheet. This preparation method is not only sensitive to the temperature of hot pressing, but also has a high hot pressing temperature. In addition, the oriented fibers produce a large decomposition orientation after hot pressing, and the mechanical strength decreases significantly.

[0005] In order to widen the hot pressing window and reduce the hot pressing pressure, polyolefins with different melting points can be hot pressed. For example, US8133537B2 hot presses three layers of polyolefin fibers with different melting points to obtain a polyolefin composite material, wherein the melting temperatures of the first and second layers of polyolefins are lower than the core layer. However, the hot pressing composite material prepared by this method has low impact strength and interlayer peeling strength.

[0006] In order to enhance the thermal conductivity of PP, Chinese invention patent CN107090129B discloses a mesophase asphalt-based graphite fiber / polypropylene composite material and its preparation method, which adopts a twin-screw extruder melt blending method, and uses mesophase asphalt-based graphite fiber, boron nitride, and magnesium hydroxide as thermal conductive fillers to prepare a mesophase asphalt-based graphite fiber / polypropylene composite material. Chinese invention patent CN104277323B discloses a thermally conductive and impact-resistant polypropylene / polyester composite material and its preparation method, which adopts a twin-screw extruder melt blending method, and uses metal powder and boron carbide powder as thermal conductive fillers to prepare a polypropylene / polyester composite material. Chinese invention patent CN108948417B discloses a compound thermal conductive powder, polypropylene composite material and its preparation method and application, which adopts a melt extrusion granulation method, and uses aluminum hydroxide, aluminum oxide, magnesium oxide, magnesium hydroxide, and zinc oxide as compound thermal conductive powder to prepare a polypropylene composite material.

[0007] The above-mentioned patents have their own obvious shortcomings. The mechanical properties of the thermally conductive polypropylene composite materials are poor, and the processing application scenarios are limited. They cannot be used for thin plates, films, fabrics, etc. CN107090129B and CN104277323B respectively use highly conductive graphite fibers and metal powders as fillers to improve the conductivity of the composite materials, which are not suitable for electronic components that require insulation; CN108948417B has a low composite thermal conductive powder filling ratio, and the thermal conductivity of the composite material is poor, which cannot meet the needs of high thermal conductivity applications. Summary of the invention

[0008] The purpose of the present invention is to overcome the technical defect that the existing polypropylene composite material is difficult to have a wide processing temperature, strong mechanical properties, high interlayer peeling strength and good thermal conductivity at the same time, and provide a thermal conductive high-strength polypropylene composite sheet and its fabric, a polypropylene composite material and its preparation method and application. The polypropylene composite material is obtained by hot pressing the polypropylene sheet of the present invention. The polypropylene composite material has excellent mechanical properties and thermal conductivity, and at the same time has good interlayer peeling strength. Even at a lower hot pressing temperature and a wider hot pressing temperature range, the interlayer peeling strength of the obtained thermal conductive polypropylene composite material is still high.

[0009] The first aspect of the present invention is to provide a thermally conductive polypropylene sheet, comprising a layer A and layers B and B' located on both sides of the layer A, with a structure of BAB';

[0010] Wherein layer A contains a polypropylene composition A, and the polypropylene composition A includes homopolymer polypropylene a, impact copolymer polypropylene b and an optional composite thermal conductive filler c; layer B is the same as or different from layer B', and each correspondingly contains a polypropylene composition B and a polypropylene composition B', and the polypropylene composition B and the polypropylene composition B' each include a random copolymer polypropylene x and a thermal adhesion enhancer y and an optional composite thermal conductive filler z; and the contents of the corresponding composite thermal conductive filler c and the composite thermal conductive filler z in the polypropylene composition A, the polypropylene composition B and the polypropylene composition B' are 0 when they are different;

[0011] The melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'.

[0012] According to the present invention, the film layers B on both sides of the film layer A are the same or different. In a preferred embodiment of the present invention, the film layers B on both sides of the film layer A are the same.

[0013] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 15-99wt% of homopolypropylene a, 0.3-50wt% of impact-resistant copolymer polypropylene b, and 0-70wt% of composite thermally conductive filler c; preferably, the polypropylene composition A comprises 35-81wt% of homopolypropylene a, 5-27wt% of impact-resistant copolymer polypropylene b, and 10-50wt% of composite thermally conductive filler c.

[0014] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each include 21-99wt% of random copolymer polypropylene x, 0.3-30wt% of thermal adhesion enhancer y, and 0-70wt% of composite thermal conductive filler z; preferably, the polypropylene composition B and the polypropylene composition B' each include 40-81wt% of random copolymer polypropylene x, 5-18wt% of thermal adhesion enhancer y, and 10-50wt% of composite thermal conductive filler z.

[0015] According to a preferred embodiment of the present invention, based on the total thickness of the thermally conductive polypropylene sheet, the thickness of layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%.

[0016] According to a preferred embodiment of the present invention, the melting point of the homopolypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene composition B and the polypropylene composition B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10° C. In this preferred embodiment, the inventors of the present invention surprisingly found that the obtained polypropylene sheet is subjected to hot pressing to obtain a polypropylene composite material, and the polypropylene composite material has more excellent mechanical properties and better interlayer peel strength. Even at a lower hot pressing temperature and a wider hot pressing temperature range, the obtained polypropylene composite material has a higher interlayer peel strength.

[0017] According to the present invention, the melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'. Preferably, the difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B, and the difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B' are each greater than or equal to 5°C, preferably greater than or equal to 10°C, and more preferably greater than or equal to 20°C.

[0018] According to a preferred embodiment of the present invention, the homopolypropylene a has:

[0019] The melting point is 150-170°C, preferably 160-170°C; and / or,

[0020] The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or,

[0021] The isotacticity (mm) is not less than 96%.

[0022] According to a preferred embodiment of the present invention, the impact-resistant copolymer polypropylene b has at least one of the following characteristics: the melting point of the impact-resistant copolymer polypropylene b is 150-170°C; and / or, the monomer copolymerized with propylene by the impact-resistant copolymer polypropylene b is ethylene or butene, preferably butene; and / or, the melt flow rate of the impact-resistant copolymer polypropylene b at 230°C and a load of 2.16 kg is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and further preferably 2.5-18 g / 10 min; and / or, the cantilever beam impact strength of the impact-resistant copolymer polypropylene b is not less than 20 KJ / m 2 (Test conditions: 23℃).

[0023] According to the research conducted by the inventors, when the melt mass flow rate and polymer composition ratio of the polypropylene composition A are within the above preferred ranges, the high impact copolymer polypropylene b in the composition can absorb impact energy well, meet the requirements of impact performance, and make the sheet have good impact performance. At the same time, since the macromolecular segments in the homopolymer polypropylene a are relatively regular, crystallization occurs during the sheet preparation process, so the sheet also has good tensile properties.

[0024] According to a preferred embodiment of the present invention, the random copolymer polypropylene x has at least one of the following characteristics:

[0025] The melting point is 110-150°C, preferably 120-140°C; and / or,

[0026] The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or,

[0027] The molecular weight distribution Mw / Mn is 5-12, preferably 7-10; and / or,

[0028] It is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.

[0029] According to a preferred embodiment of the present invention, the thermal adhesion enhancer y has at least one of the following characteristics:

[0030] The melting point or viscosity flow temperature is 70-110°C; and / or,

[0031] The melt flow rate at 190°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 1-18 g / 10 min; and / or,

[0032] One or more selected from polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA, petroleum resin; preferably, polyolefin elastomer and / or petroleum resin; more preferably,

[0033] The polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or α-olefin, the α-olefin is preferably a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene; and / or the petroleum resin is a C5 and / or C9 hydrogenated petroleum resin with a softening point of 100-150°C; preferably a cyclopentadiene type resin.

[0034] According to the research conducted by the present inventors, when the melt mass flow rate and the polymer composition ratio of the polypropylene composition B are within the preferred range, the low melting point random copolymer polypropylene x and the thermal bonding enhancer y in the composition can significantly reduce the hot pressing temperature and broaden the hot pressing temperature window, and the thermal bonding enhancer y provides good bonding properties for the sheet, which can further improve the interlayer peeling strength.

[0035] The material selection range of the composite thermally conductive filler z is relatively wide. In a preferred embodiment of the present invention, the composite thermally conductive filler z is the same as the composite thermally conductive filler c.

[0036] According to a preferred embodiment of the present invention, the layer A further contains a β-crystal nucleating agent; preferably,

[0037] The β-crystal nucleating agent is selected from at least one of condensed ring aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates.

[0038] The content range of the β-crystal nucleating agent is relatively wide. According to a preferred embodiment of the present invention, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight relative to 100 parts by weight of the polypropylene composition A. For example, 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5 parts by weight, and any two values ​​or any interval between any two values.

[0039] According to a preferred embodiment of the present invention, the composite thermally conductive filler c and the composite thermally conductive filler z are the same or different, and each comprises a thermally conductive main material, a thermally conductive auxiliary material and an interface modifier.

[0040] The material selection range of the composite thermally conductive filler c and the composite thermally conductive filler z is relatively wide. In a preferred embodiment of the present invention, the composite thermally conductive filler c and the composite thermally conductive filler z are respectively composed of a thermally conductive main material, a thermally conductive auxiliary material and an optional interface modifier. Based on the total weight of the composite thermally conductive filler c, the composite thermally conductive filler c includes 50-99wt% of the thermally conductive main material, 1-50wt% of the thermally conductive auxiliary material, and 0-3wt% of the interface modifier.

[0041] The thermal conductive main materials are commercial aluminum oxide, magnesium oxide, aluminum hydroxide, magnesium hydroxide, zinc oxide, silicon dioxide, and chopped glass fibers of different particle sizes, and the particle size range is 100nm-100μm. The thermal conductive main materials of different particle sizes have the function of synergistic filling to increase the thermal conductivity. Preferably, the weight percentage of the thermal conductive main materials is 60-95wt%.

[0042] The thermal conductive auxiliary material is commercial boron nitride, silicon carbide, and aluminum nitride of different particle sizes, with a particle size range of 100nm-100μm. The thermal conductive auxiliary material has higher thermal conductivity and can form an excellent thermal conductive channel between the thermal conductive main materials, thereby realizing the production of high thermal conductive composite materials at low cost. Preferably, the weight percentage of the thermal conductive auxiliary material is 5-40wt%.

[0043] The interface modifier is one or more (including two) of maleic anhydride, silane coupling agent, and polyvinyl pyrrolidone (PVP). The interface modifier has the function of regulating the interface compatibility between the thermal conductive main material and the thermal conductive auxiliary material and polypropylene, reducing the interface gap and the interface thermal resistance, and obtaining a composite material with higher thermal conductivity. Preferably, the weight percentage of the interface modifier is 0.5-2wt%.

[0044] As described above, according to a preferred embodiment of the present invention, based on the total weight of the composite thermally conductive filler c and the composite thermally conductive filler z, the composite thermally conductive filler c and the composite thermally conductive filler z each include 50-99wt% and more preferably 60-95wt% of a thermally conductive main material, 1-50wt% and more preferably 5-40wt% of a thermally conductive auxiliary material, and 0-3wt% and more preferably 0.5-2wt% of an interface modifier.

[0045] According to a preferred embodiment of the present invention, the thermal conductive main material is selected from at least one of aluminum oxide, magnesium oxide, aluminum hydroxide, magnesium hydroxide, zinc oxide, silicon dioxide, and chopped glass fibers, and / or has a particle size range of 100 nm-100 μm.

[0046] According to a preferred embodiment of the present invention, the thermal conductive auxiliary material is selected from at least one of boron nitride, silicon carbide and aluminum nitride, and / or has a particle size ranging from 100 nm to 100 μm.

[0047] According to a preferred embodiment of the present invention, the interface modifier is selected from one or more of maleic anhydride, silane coupling agent and polyvinyl pyrrolidone.

[0048] According to the research of the present inventors, when the components of the composite thermally conductive filler C are within the above preferred range, the thermally conductive auxiliary material in the composition can form a good thermally conductive channel between the thermally conductive main materials, meet higher thermal conductivity requirements, and make the sheet have good thermal conductivity. At the same time, the composite thermally conductive filler C does not have electrical conductivity, so that the sheet has good insulation properties.

[0049] According to the research of the present inventors, when the melt mass flow rate, polymer composition ratio and thickness distribution of the film layer A of the polypropylene composition A and the polypropylene combinations B and B' are within the preferred range, the sheet preparation process can be made smoother, thereby making the sheet have better uniformity, tensile strength, impact resistance and interlayer peeling strength.

[0050] The BAB' layer structure of the thermally conductive polypropylene sheet can be prepared by a variety of methods. In a preferred embodiment of the present invention, the BAB' layer structure of the thermally conductive polypropylene sheet is obtained by co-extruding a layer A raw material comprising a polypropylene composition A, a layer B raw material comprising a polypropylene composition B, and a layer B' raw material comprising a polypropylene composition B'.

[0051] The second aspect of the present invention is to provide a method for preparing the thermally conductive polypropylene sheet described in the first aspect, comprising co-extruding, casting or calendering, and stretching a layer A raw material containing a polypropylene composition A, a layer B raw material containing a polypropylene composition B, and a layer B' raw material containing a polypropylene composition B' according to a BAB' structure to obtain the thermally conductive polypropylene sheet.

[0052] According to a preferred embodiment of the present invention, the preparation of the raw material of layer A comprises melt blending the components including the homopolypropylene a, the impact copolymer polypropylene b and the optional composite thermal conductive filler c. The conditions and equipment for melt blending the polypropylene composition A are the conditions and equipment for melt blending of polyolefins in the prior art, preferably, the melting temperature is 150-170°C, and the equipment is preferably a twin-screw extruder.

[0053] According to a preferred embodiment of the present invention, the preparation of the raw materials of the layers B and B' comprises melt blending the components including the random copolymer polypropylene x, the thermal adhesion enhancer y and the optional composite thermal conductive filler z. The conditions and equipment for melt blending the polypropylene compositions B and B' are the same as those for melt blending polyolefins in the prior art, preferably, the melting temperature is 110-150°C, and the equipment is preferably a twin-screw extruder.

[0054] According to a preferred embodiment of the present invention, the co-extrusion and casting temperatures are independently selected from 200-240°C.

[0055] According to a preferred embodiment of the present invention, the calendering temperature is 50-70°C.

[0056] According to a preferred embodiment of the present invention, the stretching conditions include: the stretching temperature is 90-165°C, preferably 90-140°C, and more preferably 90-119°C; the stretching ratio is 1-20 times, and preferably 2-15 times.

[0057] In a preferred embodiment of the present invention, the longitudinal tensile strength of the stretched polypropylene sheet is greater than or equal to 30 MPa, more preferably 30 MPa-1 GPa; most preferably 50-600 MPa.

[0058] According to some embodiments of the present invention, polypropylene composition A, polypropylene composition B, and polypropylene composition B' are co-extruded according to the BAB' structure and cast or calendered to obtain a thermally conductive polypropylene co-extruded sheet. The process of the extrusion calendering method may include sequentially passing the thermally conductive polypropylene co-extruded sheet through a calendering roller and a traction roller, and then solid phase stretching, trimming and winding to obtain the sheet. The temperature of the extrusion casting is 200-230°C, and the temperature of the calendering roller is 50-70°C. The specific process of preparing the film by the extrusion calendering method is a commonly used choice in the art and will not be repeated here.

[0059] The third aspect of the present invention is to provide a thermally conductive polypropylene fabric, which is a three-dimensional polypropylene fabric obtained by weaving the thermally conductive polypropylene sheet described in the second aspect;

[0060] Preferably, the thermally conductive polypropylene fabric is obtained by slitting and weaving the thermally conductive polypropylene sheet; and / or the thermally conductive polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.

[0061] In order to facilitate weaving, the thermally conductive polypropylene sheet is preferably cut into pieces with a width of 2-5 mm, and then the pieces are woven to obtain the thermally conductive polypropylene fabric.

[0062] In a more preferred embodiment of the present invention, the thermally conductive polypropylene fabric is a plain, twill, satin or three-dimensional thermally conductive polypropylene fabric obtained by weaving three layers of co-extruded thermally conductive polypropylene stretch flat tape, and the three-layer co-extruded thermally conductive polypropylene stretch flat tape includes at least one film layer A formed by a high melting point polypropylene combination A and at least one film layer B, B' formed by a low melting point polypropylene composition B, B', wherein the polypropylene composition A includes homopolymer polypropylene a, impact copolymer polypropylene b and an optional composite thermally conductive filler c; the polypropylene compositions B, B' each include a random copolymer polypropylene x, a thermal bonding enhancer y and an optional composite thermally conductive filler z, and the polymer film B, B' layers are located on both sides of the A layer.

[0063] The fourth aspect of the present invention is to provide a thermally conductive polypropylene composite material, wherein the thermally conductive polypropylene composite material is prepared by thermally pressing a plurality of layers of the thermally conductive polypropylene sheet material described in the first aspect and / or the thermally conductive polypropylene fabric described in the third aspect; preferably, the structure of the multi-layer thermally conductive polypropylene sheet material composition is as follows from bottom to top: B n A n B' n ……Bi A i B' i ...B2A2B'2, B1A1B'1, B2A2B'2...B i A i B' i ……B n A n B' n The total number of stacked layers of the thermally conductive polypropylene sheet unit is 2n-1; i and n are both integers not less than 2, and i≤n; the thermally conductive polypropylene fabric is stacked from top to bottom with a warp angle of 0-90° between the warp directions, preferably with more than or equal to 2 layers, more preferably 2-200 layers; and most preferably 4-100 layers.

[0064] Preferably, the thermally conductive polypropylene composite material is prepared by thermally pressing multiple layers of the thermally conductive polypropylene sheets or the thermally conductive polypropylene fabrics.

[0065] Preferably, the multi-layer thermally conductive polypropylene sheets are stacked from top to bottom in an angle of 0-90° along their respective machine directions.

[0066] Preferably, the multi-layer heat-conductive polypropylene fabric is stacked from top to bottom with an angle of 0-90 degrees between the warp directions.

[0067] Preferably, the number of layers of the multi-layer thermal conductive polypropylene sheet and / or the multi-layer thermal conductive polypropylene fabric is greater than or equal to 2 layers, more preferably 2-200 layers; most preferably 4-100 layers.

[0068] According to a preferred embodiment of the present invention, the thermally conductive polypropylene composite material comprises a plurality of sequentially stacked polypropylene sheet unit groups; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, and each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the thermally conductive polypropylene composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n;

[0069] Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition Bi , polypropylene composition B' i ,

[0070] The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1-th group.

[0071] As mentioned above, preferably, the polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points is respectively greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; more preferably 20-60°C.

[0072] According to the present invention, the core layers in each polypropylene sheet unit can be made of the same material or different materials. There is no particular limitation on this. As long as A i The melting point is greater than that of the polypropylene composition B i , polypropylene composition B' i The melting point can achieve better technical effects.

[0073] According to a preferred embodiment of the present invention, the average value of the melting points of all the outer layers in the i-th group is greater than or equal to the average value of the melting points of all the outer layers in the i-1th group. More preferably, the inventors of the present invention have found that when the melting point gradient structure of the laminated polypropylene is designed, that is, the average value of the melting points of all the outer layers in the i-th group is greater than the average value of the melting points of all the outer layers in the i-1th group, the obtained polypropylene composite material has more excellent mechanical properties and better interlayer peeling strength.

[0074] According to the present invention, in the structure of the polypropylene composite material, the upper i-th group and the lower i-th group may be the same or different.

[0075] More preferably, the difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1-th group, which are the same or different, is 1-40°C, preferably 1-10°C, more preferably 1-5°C.

[0076] According to the present invention, the total number of stacked groups of the polypropylene sheet unit group is 2n-1. The present invention has a wide selection range for the total number of stacked groups of the polypropylene sheet unit group. In a preferred embodiment of the present invention, 2≤n≤100 is selected, more preferably, 2≤n≤50, and further preferably, 2≤n≤30.

[0077] According to the present invention, the selection range of the number of polypropylene sheet units included in each polypropylene sheet unit group is relatively wide. In a preferred embodiment of the present invention, each polypropylene sheet unit group independently includes 1 to 10, preferably 1 to 5, more preferably 1 to 3 identical or different polypropylene sheet units, more preferably 1 polypropylene sheet unit. Preferably, the number of polypropylene sheet units included in each polypropylene sheet unit group is the same.

[0078] Preferably, but not necessarily, the melting point of any outer layer in each group is within ±10°C, within ±5°C, preferably within ±3°C, more preferably within ±1°C of the average melting point of all outer layers in the group.

[0079] In the embodiment where each polypropylene sheet unit group includes only one polypropylene sheet unit, for example, the structure of the polypropylene composite material can be B from bottom to top. n A n B' n ……B i A i B' i ...B2A2B'2, B1A1B'1, B2A2B'2...B i A i B' i ……B n A n B' n , the total number of stacked layers of the polypropylene sheet unit is 2n-1; i and n are both integers not less than 2, and i≤n.

[0080] In the embodiment where each polypropylene ply unit group includes 2 or more polypropylene ply units, for example, the structure of the i-th polypropylene ply unit group is B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip The structure of the polypropylene composite material can be sequentially as follows from bottom to top: n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq )……(B i1 A i1 B' i1 , B i2 Ai2 B' i2 ……B ip A ip B' ip )……(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )(B 11 A 11 B' 11 , B 12 A 12 B' 12 ……B 1j A 1j B' 1j )(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq ), the total number of stacked polypropylene sheet units is j+2k+...2p+...2q; j, k, p, q are each independently an integer not less than 2, preferably an integer from 2 to 10, more preferably from 2 to 5, and more preferably from 2 to 3.

[0081] The surface density of the multilayer thermal conductive polypropylene composite material is greater than or equal to 110 g / m 2 , more preferably 110g / m 2 -14000g / m 2 ; The most preferred is 220g / m 2 -7000g / m 2The thermal conductivity of the multilayer thermally conductive polypropylene composite material is greater than or equal to 0.5 W m -1 K -1 , more preferably 0.5-5.0 W m -1 K -1 ; Most preferably 0.7-3.0W m -1 K -1 .

[0082] In a preferred embodiment of the present invention, the thermally conductive polypropylene composite material has at least one of the following characteristics:

[0083] Longitudinal tensile strength ≥100Mpa, preferably ≥120Mpa;

[0084] Interlayer peel strength ≥1N / mm, preferably ≥1.1N / mm;

[0085] Thermal conductivity ≥ 0.5W m -1 K -1 , preferably ≥ 0.7W m -1 K -1 ;

[0086] The tensile strength is measured according to the method specified in GB / T1040.1-2018, the interlayer peel strength is measured according to the method specified in GB / T2358-98, and the thermal conductivity is measured according to the method specified in GB / T 10297-2015. The corresponding specimens in the above tests are the standard specimens required in the above test standards.

[0087] When the thermally conductive polypropylene composite material is obtained by hot pressing 24 layers of thermally conductive polypropylene fabrics and has a thickness of about 1.7 mm, the drop hammer impact strength is ≥200 J, preferably ≥220 J.

[0088] The drop weight impact strength is measured according to the method specified in GB / T14153-1993, and the thickness of the sample is the thickness of the prepared product.

[0089] The fifth aspect of the present invention is to provide a method for preparing the thermally conductive polypropylene composite material described in the fourth aspect, the method comprising laminating and hot-pressing the thermally conductive polypropylene sheet and / or the thermally conductive polypropylene fabric, and then cooling and shaping to produce the thermally conductive polypropylene composite material.

[0090] Preferably, the temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C.

[0091] Preferably, the pressure of the hot pressing fusion is 2-10 MPa.

[0092] Preferably, the preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s.

[0093] Preferably, the cooling and shaping pressure is 2-8 MPa, and the cooling and shaping time is 30-700 s.

[0094] Preferably, the number of layers of the thermally conductive polypropylene sheet and / or the thermally conductive polypropylene fabric laminate is greater than or equal to 2 layers, preferably 2-200 layers; more preferably 4-100 layers.

[0095] Preferably, adjacent layers of the thermally conductive polypropylene fabric laminate are placed at 0-90° between the warp direction, ie the stretching direction (MD).

[0096] Adjacent layers of the thermally conductive polypropylene sheet stack are placed at 0-90 degrees along their respective machine directions.

[0097] In a more preferred embodiment of the present invention, the method for preparing the high-strength thermal conductive polypropylene composite material comprises the following steps:

[0098] Step a: Prepare polypropylene composition A, polypropylene composition B and polypropylene composition B' according to B i A i B' i The structure is co-extruded and cast or calendered to obtain a polypropylene co-extruded sheet; preferably, the temperature of the extrusion casting or calendering is 200-240°C, and the temperature of the calendering roller is 50-70°C;

[0099] Step b: stretching the thermally conductive polypropylene coextruded sheet at a certain temperature to obtain a thermally conductive polypropylene stretched sheet; the stretching method is free stretching, and / or solid phase stretching, and / or multi-stage stretching; the stretching temperature is preferably 90-165°C, preferably 90-140°C, and more preferably 90-119°C; the stretching ratio is 1-20 times, preferably 2-15 times.

[0100] Step c: cutting the thermally conductive polypropylene stretched sheet into polypropylene flat strips, and weaving the flat strips into polypropylene fabrics; preferably, the thermally conductive polypropylene flat strips have a width of 2-5 mm, and the thermally conductive polypropylene fabrics include plain weave, twill weave, satin weave or other three-dimensional thermally conductive polypropylene fabrics;

[0101] Step d: stacking the thermally conductive polypropylene fabrics in sequence, hot pressing and fusing them, and then cooling and shaping them to form a thermally conductive polypropylene composite material; preferably, in the step d, the hot pressing conditions are: hot pressing temperature 115-170°C, preferably 115-159°C, and more preferably 140-159°C; hot pressing pressure 2-10MPa, preheating time 5-600s, hot pressing time 1-600s, preferably 10-500s, cooling pressure 2-8MPa, cooling time 30-700s; preferably, adjacent thermally conductive polypropylene fabrics in the thermally conductive polypropylene composite material can be placed at 0-90° between the warp and the warp.

[0102] According to some embodiments of the present invention, in step c, a high-speed slitting machine with multiple blades can be used for cutting to obtain an oriented thermal conductive polypropylene flat tape with a width of 2-5 mm; a commercial weaving machine is used to weave the oriented flat tape according to the designed fabric structure to obtain plain, twill, satin or other three-dimensional thermal conductive polypropylene fabrics.

[0103] According to the present invention, in a preferred specific embodiment, the pressure is preferably maintained continuously during the hot pressing and cooling process without being reduced. The hot pressing process is carried out continuously, and preferably a continuous hot pressing composite material molding equipment consisting of a preheating machine, a crawler-type continuous flat hot press, a crawler-type continuous flat cooling press, a sheet cutting machine and a sheet stacking machine arranged in sequence is used; preferably, the crawler-type continuous flat hot press has a preheating unit, an independent heating and pressurizing unit, an air cooling unit and a lifting mechanism.

[0104] During the preparation, the thermally conductive polypropylene sheet and / or the thermally conductive polypropylene fabric are stacked in sequence and then preheated by a preheater. The preheated samples are sequentially hot-pressed and fused by a crawler-type flat hot press, and then cooled and shaped by a crawler-type continuous flat cooling press to form a thermally conductive polypropylene composite material, i.e., a stacked hot-pressed product. Afterwards, the sheet is sliced ​​by a sheet cutter as needed, and the hot-pressed products are stacked and arranged by a sheet stacker. The hot-pressing temperature is controlled by a preheating unit, an independent heating and pressurizing unit, and an air-cooling unit in the crawler-type flat hot press, and the hot-pressing pressure is controlled by a lifting mechanism. According to the research of the inventors, when the preparation process parameters are within a preferred range, preferably when the preparation equipment is used to prepare the thermally conductive polymer composite material, the thermally conductive polymer composite material has better tensile strength, impact resistance, interlayer peeling strength and thermal conductivity.

[0105] The sixth aspect of the present invention is to provide an application of the thermally conductive polypropylene sheet described in the first aspect, the thermally conductive polypropylene fabric described in the third aspect, the thermally conductive polypropylene composite material described in the fourth aspect, and the thermally conductive polypropylene composite material prepared in the fifth aspect in the fields of heat dissipation of electronic components, communication manufacturing, sports protection, automobile manufacturing, military materials, and consumer products.

[0106] According to a specific embodiment of the present invention, the material fields include electrical and electronics industry, mobile communications industry, luggage and transportation industry, shoemaking industry, automobile manufacturing industry, sports equipment manufacturing industry, audio equipment manufacturing industry and military field.

[0107] Compared with the prior art, the present invention has the following beneficial effects:

[0108] (1) The thermally conductive polypropylene composite polymer composite material of the present invention has good tensile strength, impact resistance, interlayer peel strength and thermal conductivity;

[0109] The thermally conductive polypropylene composite material has the following characteristics:

[0110] Longitudinal (MD) tensile strength ≥100MPa, preferably ≥120MPa; interlayer peel strength ≥1N / mm, preferably ≥1.1N / mm; thermal conductivity ≥0.5W m -1 K -1 , preferably ≥ 0.7W m -1 K -1 ; When the composite material is only composed of 24 layers of polypropylene fabrics hot pressed together and the thickness is about 1.7 mm, the drop hammer impact strength is ≥ 200 J, preferably ≥ 220 J;

[0111] (2) The thermally conductive polypropylene composite material of the present invention can be prepared at a relatively low hot pressing temperature and within a relatively wide hot pressing temperature range, which effectively reduces the energy consumption of the equipment and the damage to the composite material caused by high-temperature operation. At the same time, when prepared at a relatively low hot pressing temperature, it still has good interlayer peeling strength.

[0112] (3) The preparation method can reduce the hot pressing operation time, while improving production efficiency and reducing production energy consumption.

[0113] (4) The present invention reduces the hot pressing temperature and expands the hot pressing temperature range to 50°C; it effectively reduces the energy consumption of the equipment and the damage to the composite material caused by high temperature operation. DETAILED DESCRIPTION

[0114] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0115] In the following examples and comparative examples:

[0116] The extrusion calender and solid phase drawing equipment were purchased from Tianjin Hengrui Company, and the model was HRPC-800 three-layer co-extrusion plastic stretching sheet production line.

[0117] The thermal conductive polypropylene composition and sheet properties were tested according to the following method, and the film test results are shown in Table 1:

[0118] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, where the test temperature is 230°C and the load is 2.16 kg;

[0119] (2) Density: measured according to the method specified in GB / T 1033.1-2008;

[0120] (3) Melting point: measured according to the method specified in GB / T 28724-2012;

[0121] (4) Tensile strength: measured according to the method specified in GB / T1040.1-2018;

[0122] (5) Drop weight impact strength: measured according to the method specified in GB / T14153-1993;

[0123] (6) Interlayer peel strength: measured according to the method specified in QB / T2358-98.

[0124] (7) Thermal conductivity: measured according to the method specified in GB / T 10297-2015.

[0125] In the following examples, the β-crystal nucleating agent with the brand name VP101B is sourced from Beijing Research Institute of Chemical Industry of Sinopec Corporation; the sources of some raw materials are described in the examples, and the other raw materials are commercially available unless otherwise specified.

[0126] Example 1

[0127] This example is used to illustrate the preparation of the thermally conductive polypropylene composition, the three-layer co-extruded thermally conductive polypropylene sheet, the thermally conductive polypropylene fabric, and the thermally conductive polypropylene composite material provided by the present invention.

[0128] (1) Preparation of polypropylene composition A:

[0129] Component a is a homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate (melt mass flow rate) of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an ethylene content of 11wt%, a melting point of 155°C, and an Izod impact strength of 23KJ / m 2(23℃), melt flow rate is 2.0g / 10min; component c is composed of 80wt% alumina, 19wt% boron nitride and 1wt% silane coupling agent, the average particle size of alumina is 20μm, the average particle size of boron nitride is 10μm, Shanghai Baitu High-tech Materials Technology Co., Ltd.

[0130] The components prepared above were weighed and mixed according to the proportions, wherein the mass fraction Wa of component a was 40 parts by weight, the mass fraction Wb of component b was 10 parts by weight, and the mass fraction Wc of component c was 50 parts by weight.

[0131] 0.05 parts by weight of a β-crystal nucleating agent of grade VP101B was added. The mixture was then added to a high-speed stirrer for uniform mixing, and then the mixed material was added to a feeder of a twin-screw extruder manufactured by W&P Company, and the material entered the twin screw through the feeder. During the processing, the temperature of the screw was maintained between 200-230° C. The screw was melt-mixed uniformly, extruded, granulated and dried to obtain a polypropylene composition pellet A. The melting point of the polypropylene composition pellet A was found to be 159° C.

[0132] (2) Polypropylene composition B i Preparation:

[0133] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 8.9, a melt flow rate of 8.1 g / 10 min, and a melting point of 130°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.6, a melt flow rate of 7.2 g / 10 min, and a melting point of 135°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.6, a melt flow rate of 7.2 g / 10 min, and a melting point of 135°C. The random copolymer polypropylene made by the institute is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.3, a melt flow rate of 6.6g / 10min and a melting point of 140°C; component y is a polyolefin elastomer with a brand number of 6102, purchased from Exxon, which is an ethylene-propylene copolymer; component z is composed of 80wt% alumina, 19wt% boron nitride and 1wt% silane coupling agent, with an average particle size of 20μm for alumina and 10μm for boron nitride, purchased from Shanghai Baitu High-tech Materials Technology Co., Ltd.

[0134] The components prepared above are weighed and mixed according to the ratio, where the mass fraction of component x is Wx i The mass fraction Wy of component y is 42.5 parts by weight, the mass fraction Wy of component y is 7.5 parts by weight, the mass fraction Wz of component z is 50 parts by weight, and the other steps are the same as step (1), and finally a polypropylene composition B is obtained. i Granules (i.e. x i+y+z=B i , i=1, 2, 3), after testing, the melting point of B1 is 130°C, the melting point of B2 is 134°C, and the melting point of B3 is 139°C.

[0135] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0136] The polypropylene composition A and the polypropylene composition B obtained in the above steps (1) and (2) are i The pellets are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion calendering, and the polypropylene composition B is added to the core layer extruder of the multi-layer extrusion calendering. i Add to the upper and lower surface extruders of the multi-layer extrusion casting machine. After the pellets are co-extruded and compounded through the extruder die, they pass through the calendering roller and the traction roller in sequence, and then undergo solid phase stretching, trimming and winding to obtain sheets B1AB1, B2AB2, and B3AB3 respectively. Among them, the temperature of the extrusion casting is 230°C, and the temperature of the calendering roller is 58°C. The temperature during the solid phase stretching process is 140°C, the stretching rate is 2m / min, and the stretching ratio is 6 times.

[0137] The composite film (polypropylene sheet) made by stretching and rolling is composed of the upper surface layer (the outer layer of the film B i ), core layer (film A) and lower surface layer (outer film B i The thickness of the composite film is 85 μm, wherein the thickness of the film layer A accounts for 80% of the total thickness of the sheet.

[0138] (4) Preparation of polypropylene fabric:

[0139] The three-layer co-extruded polypropylene sheet obtained in the above step (3) is cut by a high-speed slitting machine with multiple blades to obtain an oriented polypropylene flat ribbon with a width of 3 mm; the oriented flat ribbon is woven by a commercial weaving machine according to the designed fabric structure to obtain plain polypropylene fabrics B1AB1, B2AB2, B3AB3.

[0140] (5) Preparation of polypropylene composite materials:

[0141] The polypropylene fabrics obtained in the above step (4) are stacked in order, from bottom to top, B3A3B3, B2A2B2, B1A1B1, B2A2B2, B3A3B3, and the total number of stacked layers is 5. The stacked polypropylene fabrics are hot-pressed and fused, and then cooled and shaped to form a polypropylene composite material. The polypropylene fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 145°C, hot pressing pressure 5MPa, preheating time 90s, hot pressing time 90s, and cooling time 300s. The thickness of the prepared polypropylene composite material is 410μm.

[0142] Example 2

[0143] This example is used to illustrate the preparation of the thermally conductive polypropylene composition, the three-layer co-extruded thermally conductive polypropylene sheet, the thermally conductive polypropylene fabric, and the thermally conductive polypropylene composite material provided by the present invention.

[0144] (1) Preparation of polypropylene composition A:

[0145] The preparation process is the same as step (1) of Example 1.

[0146] (2) Polypropylene composition B i Preparation:

[0147] The main preparation process is the same as step (2) of Example 1. The difference is that component B i and x i The materials are as follows:

[0148] Components x1-x4 are random copolymer polypropylenes produced by Sinopec Beijing Research Institute of Chemical Industry, which are ethylene-propylene-butene terpolymers with a melting point of 110°C; components x5-x8 are random copolymer polypropylenes produced by Sinopec Beijing Research Institute of Chemical Industry, which are ethylene-propylene-butene terpolymers with a melting point of 130°C; components x9-x 12 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 150°C; among them, components x1-x 12 The molecular weight distribution Mw / Mn is between 7 and 10, and the components x1-x 12 The melt flow rate is 1-20g / 10min.

[0149] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +y+z=B i , i=1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12). After testing, the melting points of B1-B4 are 112°C, the melting points of B5-B8 are 130°C, and the melting points of B9-B 12 The melting point is 149°C.

[0150] (3) Preparation of three-layer co-extruded thermal conductive polypropylene sheet:

[0151] The preparation process is the same as step (3) of Example 1.

[0152] (4) Preparation of thermally conductive polypropylene fabric:

[0153] The preparation process is the same as step (4) of Example 1.

[0154] (5) Preparation of thermally conductive polypropylene composite materials:

[0155] The polypropylene fabrics obtained in step (4) are stacked in order, from bottom to top: B 12 AB 12… B3AB3, B2AB2, B1AB1, B1AB1, B2AB2, B3AB3,…B 12 AB 12 The total number of stacked layers is 24, and the laminated polypropylene fabric is hot-pressed and fused, and then cooled and shaped to form a polypropylene composite material. The polypropylene fabric is placed at 90 degrees between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5MPa, preheating time 300s, hot pressing time 180s, and cooling time 600s. The thickness of the prepared polypropylene composite material is 1.75mm.

[0156] Example 3

[0157] This example is used to illustrate the preparation of the thermally conductive polypropylene composition, the three-layer co-extruded thermally conductive polypropylene sheet, the thermally conductive polypropylene fabric, and the thermally conductive polypropylene composite material provided by the present invention.

[0158] (1) Preparation of polypropylene composition A:

[0159] Component a is a homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry (under 23°C test conditions, the impact strength is 23KJ / m 2 ), ethylene content is 11wt%, melt flow rate is 2.0g / 10min, melting point is 155°C; component c is composed of 80wt% alumina, 19wt% boron nitride and 1wt% silane coupling agent, the average particle size of alumina is 20μm, the average particle size of boron nitride is 10μm, Shanghai Baitu High-tech Materials Technology Co., Ltd.

[0160] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 40 parts by weight, the mass fraction Wb of component b is 10 parts by weight, and the mass fraction Wc of component c is 50 parts by weight. 0.05 parts by weight of β-crystal nucleating agent with the grade of VP101B is added. Then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of the twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melted and mixed uniformly, extruded, granulated and dried, a polypropylene composition pellet is obtained. The melt mass flow rate MFRA is detected to be 3.6 / 10min; the melting point of the polypropylene composition A is 160°C.

[0161] (2) Preparation of polypropylene composition B:

[0162] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C and a melt flow rate of 6.6 g / 10 min; component y is a polyolefin elastomer with brand number 6102, purchased from Exxon, which is an ethylene-propylene copolymer with an ethylene content of 16wt% and a melt flow rate of 1.4 g / 10 min at 230°C and a load of 2.16 kg; component z is composed of 80wt% alumina, 19wt% boron nitride and 1wt% silane coupling agent, with an average alumina particle size of 20μm and an average boron nitride particle size of 10μm, purchased from Shanghai Baitu High-tech Materials Technology Co., Ltd.

[0163] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 42.5 parts by weight, the mass fraction Wy of component y is 7.5 parts by weight, and the mass fraction Wz of component z is 50 parts by weight. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFRB is 4.5 g / 10 min, and the melting point is 139° C.

[0164] (3) Preparation of three-layer co-extruded thermal conductive polypropylene sheet:

[0165] The pellets of polypropylene composition A and polypropylene composition B obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion calendering machine, and the polypropylene composition B is added to the upper and lower surface layer extruders of the multi-layer extrusion casting machine.

[0166] After the pellets are co-extruded and compounded out from the die of the extruder, they are sequentially passed through a calendering roller and a traction roller, and then subjected to solid phase stretching, edge cutting and winding, thereby obtaining the sheet.

[0167] The temperature of the extrusion casting was 230°C, and the temperature of the calendering roller was 55°C. The temperature during the solid phase stretching was 135°C, the stretching rate was 2m / min, and the stretching ratio was 6 times. After stretching, the film was rolled up to form a thermal conductive polypropylene sheet (composite film), which consisted of an upper surface layer (film layer B), a core layer (film layer A), and a lower surface layer (film layer B).

[0168] The thickness of the thermal conductive polypropylene sheet (composite film) is 85 μm, wherein the thickness of the film layer A accounts for 80% of the total thickness of the sheet.

[0169] (4) Preparation of thermally conductive polypropylene fabric:

[0170] The three-layer co-extruded thermal conductive polypropylene sheet obtained in the above step (3) is cut by a high-speed slitting machine with multiple blades to obtain an oriented polypropylene flat strip with a width of 3 mm; the oriented flat strip is woven by a commercial weaving machine according to the designed fabric structure to obtain a plain weave thermal conductive polypropylene fabric.

[0171] (5) Preparation of thermally conductive polypropylene composite materials:

[0172] The thermally conductive polypropylene fabrics obtained in the above step (4) are laminated and hot-pressed in sequence to form a laminated thermally conductive polypropylene sheet. The laminated thermally conductive polypropylene sheet includes 24 layers of thermally conductive polypropylene fabrics, and the thermally conductive polypropylene fabrics are placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5MPa, preheating time 180s, hot pressing time 180s, and cooling time 600s. The thickness of the prepared thermally conductive polypropylene composite material is 1.76mm.

[0173] Example 4

[0174] This example is used to illustrate the preparation of the thermally conductive polypropylene composition, the three-layer co-extruded thermally conductive polypropylene sheet, the thermally conductive polypropylene fabric, and the thermally conductive polypropylene composite material provided by the present invention.

[0175] (1) Preparation of polypropylene composition A:

[0176] The preparation process is the same as step (1) of Example 3.

[0177] (2) Preparation of polypropylene composition B:

[0178] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C and a melt flow rate of 6.6 g / 10 min; component y is a polyolefin elastomer with brand number 6102, purchased from Exxon, which is an ethylene-propylene copolymer with an ethylene content of 16 wt% and a melt flow rate of 1.4 g / 10 min at 230°C and a load of 2.16 kg; component z is not added.

[0179] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 15 parts by weight, and the other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained, and the melt mass flow rate MFRB is 5.2 g / 10 min, and the melting point is 138° C.;

[0180] (3) Preparation of three-layer co-extruded thermal conductive polypropylene sheet:

[0181] The main steps are the same as those in Example 3. The preparation process is the same as step (3) in Example 3.

[0182] (4) Preparation of thermally conductive polypropylene fabric:

[0183] The preparation process is the same as step (4) of Example 3.

[0184] (5) Preparation of thermally conductive polypropylene composite materials:

[0185] The preparation process is the same as step (5) of Example 3.

[0186] The thickness of the prepared thermally conductive polypropylene composite material is close to that of Example 3.

[0187] Example 5

[0188] This example is used to illustrate the preparation of the thermally conductive polypropylene composition, the three-layer co-extruded thermally conductive polypropylene sheet, the thermally conductive polypropylene fabric, and the thermally conductive polypropylene composite material provided by the present invention.

[0189] (1) Preparation of polypropylene composition A:

[0190] Component a is a homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry (under 23°C test conditions, the impact strength is 23KJ / m 2 ), ethylene content is 11wt%, melt flow rate is 2.0g / 10min, melting point is 155°C; component c is not added.

[0191] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight. 0.05 parts by weight of β-crystal nucleating agent with the grade of VP101B is added. Then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melt-mixed, extruded, granulated and dried, a polypropylene composition pellet is obtained. The melt mass flow rate MFRA is detected to be 4.6 / 10min; the melting point of the polypropylene composition A is 157°C.

[0192] (2) Preparation of polypropylene composition B:

[0193] The preparation process is the same as step (2) of Example 3.

[0194] (3) Preparation of three-layer co-extruded thermal conductive polypropylene sheet:

[0195] The main steps are the same as those in Example 3. The preparation process is the same as step (3) in Example 3.

[0196] (4) Preparation of thermally conductive polypropylene fabric:

[0197] The preparation process is the same as step (4) of Example 3.

[0198] (5) Preparation of thermally conductive polypropylene composite materials:

[0199] The preparation process is the same as step (5) of Example 3.

[0200] The thickness of the prepared thermally conductive polypropylene composite material is close to that of Example 3.

[0201] Example 6

[0202] This example is used to illustrate the preparation of the thermally conductive polypropylene composition, the three-layer co-extruded thermally conductive polypropylene sheet, the thermally conductive polypropylene fabric, and the thermally conductive polypropylene composite material provided by the present invention.

[0203] (1) Preparation of polypropylene composition A:

[0204] Component a is a homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry (under 23°C test conditions, the impact strength is 23KJ / m 2 ), ethylene content is 11wt%, melt flow rate is 2.0g / 10min, melting point is 155°C; component c is composed of 80wt% magnesium oxide, 19wt% silicon carbide and 1wt% silane coupling agent, the average particle size of magnesium oxide is 4μm, the average particle size of silicon carbide is 10μm, Shanghai Baitu High-tech Materials Technology Co., Ltd.

[0205] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 60 parts by weight, the mass fraction Wb of component b is 15 parts by weight, and the mass fraction Wc of component c is 25 parts by weight. 0.05 parts by weight of β-crystal nucleating agent with the grade of VP101B is added. Then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of the twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melted and mixed uniformly, extruded, granulated and dried, a polypropylene composition pellet is obtained. The melt mass flow rate MFRA is detected to be 4.2 / 10min; the melting point of the polypropylene composition A is 158°C.

[0206] (2) Preparation of polypropylene composition B:

[0207] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C and a melt flow rate of 6.6 g / 10 min; component y is a polyolefin elastomer with brand number 6102, purchased from Exxon, which is an ethylene-propylene copolymer with an ethylene content of 16wt% and a melt flow rate of 1.4g / 10min at 230°C and a load of 2.16kg; component z is composed of 80wt% magnesium oxide, 19wt% silicon carbide and 1wt% silane coupling agent, with an average particle size of 4μm for magnesium oxide and an average particle size of 10μm for silicon carbide, and is from Shanghai Baitu High-tech Materials Technology Co., Ltd.

[0208] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 63.75 parts by weight, the mass fraction Wy of component y is 11.25 parts by weight, and the mass fraction Wz of component z is 25 parts by weight. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFRB is 5.0 g / 10 min, and the melting point is 138° C.

[0209] (3) Preparation of three-layer co-extruded thermal conductive polypropylene sheet:

[0210] The main steps are the same as those in Example 3. The preparation process is the same as step (3) in Example 3.

[0211] (4) Preparation of thermally conductive polypropylene fabric:

[0212] The preparation process is the same as step (4) of Example 3.

[0213] (5) Preparation of thermally conductive polypropylene composite materials:

[0214] The preparation process is the same as step (5) of Example 3.

[0215] The thickness of the prepared thermally conductive polypropylene composite material is close to that of Example 3.

[0216] Example 7

[0217] This example is used to illustrate the preparation of the thermally conductive polypropylene composition, the three-layer co-extruded thermally conductive polypropylene sheet, the thermally conductive polypropylene fabric, and the thermally conductive polypropylene composite material provided by the present invention.

[0218] (1) Preparation of polypropylene composition A:

[0219] The preparation process is the same as step (1) of Example 6.

[0220] (2) Preparation of polypropylene composition B:

[0221] The preparation process is the same as step (2) of Example 3.

[0222] (3) Preparation of three-layer co-extruded thermal conductive polypropylene sheet:

[0223] The main steps are the same as those in Example 3. The preparation process is the same as step (3) in Example 3.

[0224] (4) Preparation of thermally conductive polypropylene fabric:

[0225] The preparation process is the same as step (4) of Example 3.

[0226] (5) Preparation of thermally conductive polypropylene composite materials:

[0227] The preparation process is the same as step (5) of Example 3.

[0228] The thickness of the prepared thermally conductive polypropylene composite material is close to that of Example 3.

[0229] Example 8

[0230] This example is used to illustrate the preparation of the thermally conductive polypropylene composition, the three-layer co-extruded thermally conductive polypropylene sheet, the thermally conductive polypropylene fabric, and the thermally conductive polypropylene composite material provided by the present invention.

[0231] (1) Preparation of polypropylene composition A:

[0232] The preparation process is the same as step (1) of Example 5.

[0233] (2) Preparation of polypropylene composition B:

[0234] The preparation process is the same as step (2) of Example 6.

[0235] (3) Preparation of three-layer co-extruded thermal conductive polypropylene sheet:

[0236] The main steps are the same as those in Example 3. The preparation process is the same as step (3) in Example 3.

[0237] (4) Preparation of thermally conductive polypropylene fabric:

[0238] The preparation process is the same as step (4) of Example 3.

[0239] (5) Preparation of thermally conductive polypropylene composite materials:

[0240] The preparation process is the same as step (5) of Example 3.

[0241] The thickness of the prepared thermally conductive polypropylene composite material is close to that of Example 3.

[0242] Example 9

[0243] This example is used to illustrate the preparation of the thermally conductive polypropylene composition, the three-layer co-extruded thermally conductive polypropylene sheet, the thermally conductive polypropylene fabric, and the thermally conductive polypropylene composite material provided by the present invention.

[0244] (1) Preparation of polypropylene composition A:

[0245] The preparation process is the same as step (1) of Example 3.

[0246] (2) Preparation of polypropylene composition B:

[0247] The preparation process is the same as step (2) of Example 3.

[0248] (3) Preparation of three-layer co-extruded thermal conductive polypropylene sheet:

[0249] The preparation process is the same as step (3) of Example 3.

[0250] (4) Preparation of thermally conductive polypropylene fabric:

[0251] The preparation process is the same as step (4) of Example 3.

[0252] (5) Preparation of thermally conductive polypropylene composite materials:

[0253] The main steps are the same as those in Example 3. The laminated thermally conductive polypropylene sheet includes two layers of thermally conductive polypropylene fabrics. The hot pressing conditions used are: temperature 140°C, hot pressing pressure 2MPa, preheating time 120s, hot pressing time 10s, and cooling time 300s. The thickness of the prepared thermally conductive polypropylene composite material is 149μm.

[0254] Example 10

[0255] This example is used to illustrate the preparation of the thermally conductive polypropylene composition, the three-layer co-extruded thermally conductive polypropylene sheet, the thermally conductive polypropylene fabric, and the thermally conductive polypropylene composite material provided by the present invention.

[0256] (1) Preparation of polypropylene composition A:

[0257] The preparation process is the same as step (1) of Example 3.

[0258] (2) Preparation of polypropylene composition B:

[0259] The preparation process is the same as step (2) of Example 3.

[0260] (3) Preparation of three-layer co-extruded thermal conductive polypropylene sheet:

[0261] The preparation process is the same as step (3) of Example 3.

[0262] (4) Preparation of thermally conductive polypropylene fabric:

[0263] The preparation process is the same as step (4) of Example 3.

[0264] (5) Preparation of thermally conductive polypropylene composite materials:

[0265] The main steps are the same as those in Example 3. The laminated thermally conductive polypropylene sheet includes 100 layers of thermally conductive polypropylene fabrics. The hot pressing conditions used are: 159° C., hot pressing pressure of 10 MPa, preheating time of 300 s, hot pressing time of 300 s, and cooling time of 700 s. The thickness of the prepared thermally conductive polypropylene composite material is 7.68 mm.

[0266] Comparative Example 1

[0267] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 3, except that only the polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 85 μm.

[0268] According to the method of Example 3, a polypropylene fabric and a polypropylene composite material were prepared.

[0269] The thickness of the prepared polypropylene composite material is close to that of Example 3.

[0270] Comparative Example 2

[0271] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 3, except that only the polypropylene composition B was used for extrusion casting into a single-layer film with a thickness of 85 μm.

[0272] According to the method of Example 3, a polypropylene fabric and a polypropylene composite material were prepared.

[0273] The thickness of the prepared polypropylene composite material is close to that of Example 3.

[0274] Comparative Example 3

[0275] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 6, except that only the polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 85 μm.

[0276] According to the method of Example 3, a polypropylene fabric and a polypropylene composite material were prepared.

[0277] The thickness of the prepared polypropylene composite material is close to that of Example 3.

[0278] Comparative Example 4

[0279] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 3, except that only the polypropylene composition B was used for extrusion casting into a single-layer film with a thickness of 85 μm.

[0280] According to the method of Example 3, a polypropylene fabric and a polypropylene composite material were prepared.

[0281] The thickness of the prepared polypropylene composite material is close to that of Example 3.

[0282] Comparative Example 5

[0283] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 3, except that the polypropylene composition A did not contain the composition c, and the polypropylene composition B did not contain the composition z. The film thickness was 85 μm. A polypropylene fabric and a polypropylene composite material were prepared according to the method of Example 3.

[0284] The thickness of the prepared polypropylene composite material is close to that of Example 3.

[0285] Comparative Example 6

[0286] According to the method of Example 1, a three-layer co-extruded polypropylene sheet and a polypropylene fabric were prepared.

[0287] The difference lies in the preparation of the polypropylene composite material. The prepared polypropylene fabrics are stacked in sequence, from bottom to top, B1A1B1, B2A2B2, B3A3B3, B2A2B2, B1A1B1, and the total number of stacked layers is 5. The stacked polypropylene fabrics are hot-pressed and fused, and then cooled and shaped to make a polypropylene composite material.

[0288] Experimental example

[0289] The thermally conductive polypropylene composite materials obtained in the above examples and comparative examples were tested according to the following method. The test results are shown in Table 1.

[0290] (1) Tensile strength: Prepare samples and measure them according to the method specified in GB / T1040.1-2018;

[0291] (2) Interlayer peel strength: Sample preparation and measurement shall be carried out according to the method specified in QB / T2358-98.

[0292] (3) Drop weight impact strength: measured according to the method specified in GB / T14153-1993.

[0293] (4) Thermal conductivity: The thermal conductivity was measured according to the method specified in GB / T 10297-2015. The thicknesses of the polypropylene composite materials obtained in Examples 3-10 and Comparative Examples 1-5 were close to each other, about 1.7 mm, and all within the range of 1.7 mm ± 0.1 mm.

[0294] Table 1

[0295]

[0296] From the results of the examples in Table 1, it can be concluded that the thermal conductive polypropylene composite material prepared according to the present invention has good tensile properties, impact resistance and thermal conductivity, and has good interlayer peel strength at a lower hot pressing temperature. The thermal conductive polypropylene composite sheet of the present invention has a longitudinal (MD) tensile strength of ≥120MPa, an interlayer peel strength of ≥1N / mm, and a thermal conductivity of ≥0.5W m -1 K -1 When the thermal conductive polypropylene composite material is formed by hot pressing 24 layers of thermal conductive polypropylene fabrics and has a thickness of about 1.7 mm, the drop hammer impact strength is ≥200J.

[0297] It can be seen from preferred embodiments 2, 3, 6, 9 and 10 that the thermal conductive polypropylene composite material prepared by the present invention has a longitudinal (MD) tensile strength of ≥130 MPa, an interlayer peel strength of ≥1.2 N / mm, and a thermal conductivity of ≥0.9 W m -1 K -1 When the thermal conductive polypropylene composite material is formed by hot pressing 24 layers of thermal conductive polypropylene fabrics and has a thickness of about 1.7 mm, the drop hammer impact strength is ≥200J.

[0298] It can be seen from Comparative Examples 1-6 that only using a single-layer sheet structure or using an interlayer ratio outside the scope of the embodiment will lead to a decrease in the performance of the laminated polypropylene sheet or fabric, and using process conditions outside the scope of the embodiment will greatly reduce the tensile strength, impact resistance, interlayer peel strength or thermal conductivity of the obtained polypropylene composite material.

[0299] Comparison of Example 1 with Comparative Example 6 shows that, compared with conventional polypropylene composite materials with non-gradient melting point structures, the polypropylene composite materials with melting point gradient structures of the present invention have higher tensile strength, impact properties and interlayer peeling strength. Compared with conventional polypropylene composite materials with non-gradient melting point structures, the polypropylene composite materials with melting point gradient structures of the present invention require shorter hot pressing time or lower hot pressing temperature during processing. It is believed that the reduction of hot pressing time or hot pressing temperature can reduce the damage to mechanical properties caused by molecular chain deorientation. In addition, the reduction of hot pressing time or hot pressing temperature can also achieve the beneficial effect of reducing costs and increasing efficiency.

[0300] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

[0301] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A thermally conductive polypropylene sheet, comprising a layer A and layers B and B' located on both sides of the layer A, with a structure of BAB'; wherein the layer A contains a polypropylene composition A, the polypropylene composition A contains homopolymerized polypropylene a, impact copolymerized polypropylene b and an optional composite thermally conductive filler c; the layer B and the layer B' are the same or different, and each correspondingly contains a polypropylene composition B and a polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each contain a random copolymerized polypropylene x and a thermal adhesion enhancer y and an optional composite thermally conductive filler z; and the contents of the corresponding composite thermally conductive filler c and the composite thermally conductive filler z in the polypropylene composition A, the polypropylene composition B and the polypropylene composition B' are not the same as 0; in, The melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'.

2. The thermally conductive polypropylene sheet according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 15-99 wt% of homopolypropylene a, 0.3-50 wt% of impact copolymer polypropylene b, and 0-70 wt% of composite thermal conductive filler c; preferably, The polypropylene composition A comprises 35-81 wt% of homopolypropylene a, 5-27 wt% of impact copolymer polypropylene b, and 10-50 wt% of composite thermal conductive filler c; and / or, Based on the total weight of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each include 21-99wt% of random copolymer polypropylene x, 0.3-30wt% of thermal adhesion enhancer y, and 0-70wt% of composite thermal conductive filler z; preferably, the polypropylene composition B and the polypropylene composition B' each include 40-81wt% of random copolymer polypropylene x, 5-18wt% of thermal adhesion enhancer y, and 10-50wt% of composite thermal conductive filler z.

3. The thermally conductive polypropylene sheet according to claim 1, characterized in that: Based on the total thickness of the thermally conductive polypropylene sheet, the thickness of the layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%; and / or, The melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene composition B and the polypropylene composition B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10°C and / or, The difference between the melting points of the polypropylene composition A and the polypropylene composition B and the difference between the melting points of the polypropylene composition A and the polypropylene composition B' are each equal to or greater than 5°C, preferably equal to or greater than 10°C, more preferably equal to or greater than 20°C.

4. The thermally conductive polypropylene sheet according to any one of claims 1 to 3, characterized in that: The homopolymer polypropylene a has: The melting point is 150-170°C, preferably 160-170°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The isotacticity (mm) is not less than 96%.

5. The thermally conductive polypropylene sheet according to any one of claims 1 to 3, characterized in that: The melting point of the impact-resistant copolymer polypropylene b is 150-170° C.: and / or, The monomer of the impact copolymer polypropylene b and propylene copolymer is ethylene or butene, preferably butene; and / or, The impact copolymer polypropylene b has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The cantilever beam impact strength of the impact-resistant copolymer polypropylene b is not less than 20KJ / m 2 .

6. The thermally conductive polypropylene sheet according to any one of claims 1 to 3, characterized in that: The random copolymer polypropylene x has: The melting point is 110-150°C, preferably 120-140°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or, The molecular weight distribution Mw / Mn is 5-12, preferably 7-10; and / or, It is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.

7. The thermally conductive polypropylene sheet according to any one of claims 1 to 3, characterized in that: The thermal bonding enhancer y has: The melting point or viscosity flow temperature is 70-110°C; and / or, The melt flow rate at 190°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 1-18 g / 10 min; and / or, One or more selected from polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA, petroleum resin; preferably, polyolefin elastomer and / or petroleum resin; more preferably, The polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or α-olefin, the α-olefin is preferably a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene; and / or the petroleum resin is a C5 and / or C9 hydrogenated petroleum resin with a softening point of 100-150°C; preferably a cyclopentadiene type resin.

8. The thermally conductive polypropylene sheet according to any one of claims 1 to 3, characterized in that: The BAB' sheet structure of the thermally conductive polypropylene sheet is obtained by co-extruding a layer A raw material comprising a polypropylene composition A, a layer B raw material comprising a polypropylene composition B, and a layer B' raw material comprising a polypropylene composition B'; and / or, The layer A also contains a β-crystalline nucleating agent; preferably, The β-crystal nucleating agent is at least one selected from the group consisting of condensed aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates; and / or, Relative to 100 parts by weight of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight.

9. The thermally conductive polypropylene sheet according to any one of claims 1 to 3, characterized in that: The composite thermally conductive filler c and the composite thermally conductive filler z are the same or different, and each comprises a thermally conductive main material, a thermally conductive auxiliary material and an optional interface modifier; preferably, Based on the total weight of the composite thermally conductive filler c and the composite thermally conductive filler z, the composite thermally conductive filler c and the composite thermally conductive filler z each include 50-99wt% and more preferably 60-95wt% of a thermally conductive main material, 1-50wt% and more preferably 5-40wt% of a thermally conductive auxiliary material, and 0-3wt% and more preferably 0.5-2wt% of an interface modifier; more preferably: The thermal conductive main material is selected from at least one of aluminum oxide, magnesium oxide, aluminum hydroxide, magnesium hydroxide, zinc oxide, silicon dioxide, and chopped glass fibers, and / or the particle size range is 100 nm-100 μm; and / or, The thermal conductive auxiliary material is selected from at least one of boron nitride, silicon carbide and aluminum nitride, and / or has a particle size ranging from 100 nm to 100 μm; and / or, The interface modifier is selected from one or more of maleic anhydride, silane coupling agent and polyvinyl pyrrolidone.

10. The method for preparing the thermally conductive polypropylene sheet according to any one of claims 1 to 9, comprising co-extruding, casting or calendering, and stretching a layer A raw material comprising a polypropylene composition A, a layer B raw material comprising a polypropylene composition B, and a layer B' raw material comprising a polypropylene composition B' according to a BAB' structure to obtain the thermally conductive polypropylene sheet.

11. The method for preparing the thermally conductive polypropylene sheet according to claim 10, characterized in that: The preparation of the raw material of layer A comprises melt blending the components including the homopolypropylene a, the impact copolymer polypropylene b and the optional composite thermal conductive filler c; and / or, The preparation of the raw materials of the layers B and B' comprises melt blending the components including the random copolymer polypropylene x, the thermal adhesion enhancer y and the optional composite thermal conductive filler z; and / or, The co-extrusion and casting temperatures are independently selected from 200-240° C.; and / or, The calendering temperature is 50-70°C; and / or, The stretching conditions include: the stretching temperature is 90-165° C., preferably 90-140° C., and more preferably 90-119° C.; and the stretching ratio is 1-20 times.

12. A thermally conductive polypropylene fabric, a three-dimensional polypropylene fabric obtained by weaving the thermally conductive polypropylene sheet according to any one of claims 1 to 9; Preferably, the thermally conductive polypropylene fabric is obtained by slitting and weaving the thermally conductive polypropylene sheet; and / or the thermally conductive polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.

13. A thermally conductive polypropylene composite material, wherein the thermally conductive polypropylene composite material is prepared by thermally pressing multiple layers of the thermally conductive polypropylene sheet according to any one of claims 1 to 9 and / or the thermally conductive polypropylene fabric according to claim 12; preferably, The thermally conductive polypropylene composite material is prepared by thermally pressing multiple layers of the thermally conductive polypropylene sheets or the thermally conductive polypropylene fabric; and / or, The multi-layer thermally conductive polypropylene sheets are stacked from top to bottom in an angle of 0-90° along their respective machine directions; and / or, The multi-layer heat-conductive polypropylene fabric is stacked from top to bottom with the warp direction at an angle of 0-90°; and / or, The number of layers of the multi-layer thermal conductive polypropylene sheet and / or the multi-layer thermal conductive polypropylene fabric is greater than or equal to 2 layers, more preferably 2-200 layers, and most preferably 4-100 layers.

14. The thermally conductive polypropylene composite material according to claim 13, characterized in that: The thermally conductive polypropylene composite material comprises a plurality of sequentially stacked polypropylene sheet unit groups; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, and each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the thermally conductive polypropylene composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n; Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i , The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1-th group.

15. The thermally conductive polypropylene composite material according to claim 14, characterized in that: Polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points of each is greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; and / or, The difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1th group is the same or different, and is 1-40°C, preferably 1-10°C, more preferably 1-5°C; and / or, 2≤n≤100, preferably, 2≤n≤50; and / or, Each group of polypropylene ply units, independently of one another, comprises 1 to 10, preferably 1 to 5, identical or different polypropylene ply units.

16. The method for preparing the thermally conductive polypropylene composite material according to claim 14 or 15, comprising laminating and hot-pressing the thermally conductive polypropylene sheet and / or the thermally conductive polypropylene fabric, and then cooling and shaping to prepare the thermally conductive polypropylene composite material; preferably, The temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C; and / or, The pressure of the hot pressing fusion is 2-10 MPa; and / or, The preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s; and / or, The cooling and shaping pressure is 2-8 MPa, and the cooling and shaping time is 30-700 s; and / or, The number of layers of the thermally conductive polypropylene sheet and / or the thermally conductive polypropylene fabric laminate is greater than or equal to 2 layers, preferably 2-200 layers; more preferably 4-100 layers; and / or, Adjacent layers of the thermally conductive polypropylene fabric laminate are placed at an angle of 0-90° between the warp direction; and / or, Adjacent layers of the thermally conductive polypropylene sheet stack are placed at 0-90 degrees along their respective machine directions.

17. Application of the thermally conductive polypropylene sheet according to any one of claims 1 to 9, the thermally conductive polypropylene fabric according to claim 12, the thermally conductive polypropylene composite material according to any one of claims 13 to 15, and the thermally conductive polypropylene composite material prepared by the preparation method according to claim 16 in the fields of heat dissipation of electronic components, communication manufacturing, sports protection, automobile manufacturing, military materials, and consumer products.

Citation Information

Patent Citations

  • High-thermal-conductivity low-dielectric polypropylene continuous composite sheet composition and preparation method thereof

    CN113337035A

  • Low-filling high-thermal-conductivity polypropylene / SEBS composite material and preparation method thereof

    CN113817265A

  • Antistatic polypropylene composite film as well as preparation method and application thereof

    CN115991025A

  • Electromagnetic shielding polypropylene composite film as well as preparation method and application thereof

    CN115991036A

Cited By

  • Antistatic polypropylene sheet and fabric thereof, high-strength high-impact-resistance antistatic polypropylene composite material and preparation method and application of high-strength high-impact-resistance antistatic polypropylene composite material

    CN118849572A

  • Antistatic polypropylene sheet and fabric thereof, high strength high impact antistatic polypropylene composite and method and use thereof

    CN118849572B

  • Conductive high-strength polypropylene sheet and fabric thereof, polypropylene composite material and preparation method and application thereof

    CN118849575A

  • Electrically conductive high-strength polypropylene sheet and fabric thereof, polypropylene composite material and its manufacturing method and application

    CN118849575B

  • Aluminum-plastic film with high thermal conductivity and high deep-drawing performance, preparation method of aluminum-plastic film and lithium ion battery

    CN119502510A