Green all-inorganic metal halide CsCu2I3: Zn as well as preparation method and application thereof

The preparation of CsCu2I3:Zn through the anti-solvent method solves the problems of complex production process and low fluorescence emission intensity of lead-free perovskite materials, achieves high purity, high yield and high fluorescence intensity, and improves the quality and detection of scintillation imaging. ability.

CN118851243APending Publication Date: 2024-10-29GUILIN UNIV OF ELECTRONIC TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410836991.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing lead-free perovskite materials have complex production processes, low yields, and low fluorescence emission intensity, which limits their application in the scintillator field.

Method used

The green all-inorganic metal halide CsCu2I3:Zn was prepared using the antisolvent method. CsI, ZnI2 and CuI were weighed and heated in a mixed solvent of N,N-dimethylformamide and dimethyl sulfoxide, and anhydrous was added. Ethanol was used as an antisolvent, followed by centrifugation and drying to obtain high-purity, high-yield CsCu2I3:Zn microcrystalline powder.

Benefits of technology

The fluorescence emission intensity of CsCu2I3:Zn is increased, the production cost is reduced, the contrast and signal-to-noise ratio of scintillation imaging are enhanced, and the sensitivity and resolution of detection are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851243A_ABST
    Figure CN118851243A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lead-free perovskite scintillation materials, and discloses a green all-inorganic metal halide CsCu2I3: Zn and a preparation method and application thereof, the preparation method comprises the following steps: S1, weighing CsI, ZnI2 and CuI; s2, a mixed solvent of N, N-dimethylformamide and dimethyl sulfoxide is added, and the mixture is placed on a heating table to be stirred till the powder is completely dissolved; s3, adding absolute ethyl alcohol to serve as an anti-solvent, generating white precipitates in the solution, then putting the white precipitates into a centrifugal tube for centrifugation, and discarding supernate to reserve precipitates; s4, washing off the residual solvent of the precipitate obtained in S3 with isopropanol, then carrying out multiple times of centrifugation, discarding the supernatant, and drying the washed precipitate in a drying oven to obtain CsCu2I3: Zn microcrystalline powder; according to the invention, the CsCu2I3: Zn is prepared by using an anti-solvent method, so that the problems of complex production process, low yield and low fluorescence emission intensity of the existing lead-free perovskite material are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lead-free perovskite scintillating materials, in particular to a green all-inorganic metal halide CsCu2I3:Zn and a preparation method and application thereof. Background Art

[0002] Scintillator is an energy conversion luminescent material with the characteristics of flickering luminescence. Scintillator material converts luminescence by absorbing high-energy rays such as X-rays or high-energy particles such as alpha particles, and this luminescence is flickering luminescence, so it is called scintillator because of the flickering frequency. Because the decay time of the photons emitted by the scintillator is very fast, reaching the nanosecond level, it looks like it is constantly luminous, but in fact it is constantly flickering. Existing lead-based halide perovskite materials are the hot spots of perovskite research because they have excellent properties such as suitable band gaps, long hole-electron diffusion lengths, high defect tolerance, etc. However, the toxicity and poor stability of lead are the main bottlenecks for the further commercial application of these emerging materials. For environmental friendliness and sustainable development, it is an inevitable trend in the development of perovskite materials to replace lead with non-toxic or low-toxic non-lead elements and improve the stability of perovskite materials.

[0003] To solve these problems, new lead-free perovskite materials based on non-toxic elements and with high structural stability have attracted great attention from researchers. However, the production process of new lead-free perovskite materials on the market is complex, the yield is low, and the fluorescence emission intensity is low. Summary of the invention

[0004] The present invention aims to provide a green all-inorganic metal halide CsCu2I3:Zn and a preparation method and application thereof, and to prepare CsCu2I3:Zn by an anti-solvent method to solve the problems of complex production process, low yield and low fluorescence emission intensity of existing lead-free perovskite materials.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing green all-inorganic metal halide CsCu2I3:Zn comprises the following steps:

[0007] S1. Weigh CsI, ZnI2 and CuI and put them into a sample bottle to obtain reaction raw materials;

[0008] S2, adding a mixed solvent of N,N-dimethylformamide and dimethyl sulfoxide to the reaction raw material obtained in S1, and stirring on a heating table until the powder is completely dissolved to obtain a reaction precursor solution;

[0009] S3, adding anhydrous ethanol as an anti-solvent to the reaction precursor solution obtained in S2, generating a white precipitate in the solution, which is then placed in a centrifuge tube for centrifugation, discarding the supernatant and retaining the precipitate;

[0010] S4. Wash the residual solvent of the precipitate obtained in S3 with isopropanol, centrifuge for multiple times to discard the supernatant, put the washed precipitate into an oven to dry, and obtain CsCu2I3:Zn microcrystalline powder.

[0011] Furthermore, in S1, the molar ratio of CsI to CuI is 1:2.

[0012] Furthermore, in S1, the percentage of the molar mass of ZnI2 to the molar mass of CuI is any one of 5%, 10%, 15%, 20%, and 30%.

[0013] Further, in S2, the volume ratio of N,N-dimethylformamide to dimethyl sulfoxide is 3:1, and the heating temperature of the heating stage is 27°C.

[0014] Furthermore, in S3, the volume ratio of anhydrous ethanol to the mixed solvent of N,N-dimethylformamide and dimethyl sulfoxide in S2 is 3:1.

[0015] Further, in S4, the oven temperature is 70°C and the oven drying time is 12 hours.

[0016] The green all-inorganic metal halide CsCu2I3:Zn is prepared according to the above-mentioned preparation method of the green all-inorganic metal halide CsCu2I3:Zn.

[0017] The above-mentioned green all-inorganic metal halide CsCu2I3:Zn is used in scintillators, lighting, displays, solar cells, light-emitting diodes, X-ray detection and gamma-ray detection.

[0018] The beneficial effects of the technical solution are:

[0019] 1. The raw materials used in the present invention are abundant, low in cost and environmentally friendly;

[0020] 2. The CsCu2I3:Zn product prepared by the anti-solvent method of the present invention has high purity and high yield, thereby reducing production costs;

[0021] 3. The fluorescence emission intensity of CsCu2I3:Zn prepared by the present invention is relatively high, which is significantly higher than that of the matrix CsCu2I3. The intensity of the fluorescence signal directly affects the contrast and signal-to-noise ratio of the imaging, and therefore has an important influence on the scintillation imaging to be performed later. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a SEM image of CsCu2I3:Zn doped with 15% Zn (CsCu2I3:15%Zn) in Example 3 of the present invention;

[0023] Figure 2 XRD patterns of CsCu2I3 and CsCu2I3:Zn doped with 5%, 10%, 15%, 20%, and 30% Zn in Examples 1-5 of the present invention and Comparative Example 1;

[0024] Figure 3 The fluorescence emission spectra of CsCu2I3 and CsCu2I3 doped with 5%, 10%, 15%, 20%, and 30% Zn under 328nm excitation in Examples 1-5 of the present invention and Comparative Example 1;

[0025] Figure 4 The bar graph of the yield of CsCu2I3 prepared in Comparative Examples 1-4 of the present invention;

[0026] Figure 5 The XRD diagram of CsCu2I3 prepared in Comparative Examples 1-4 of the present invention;

[0027] Figure 6 This is the fluorescence emission spectrum of CsCu2I3 prepared in Comparative Examples 1-4 of the present invention under 328nm excitation. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments:

[0029] Example 1

[0030] A method for preparing green all-inorganic metal halide CsCu2I3:Zn comprises the following steps:

[0031] S1. Weigh 3.5 mmol (0.9093 g) of CsI, 0.35 mmol (0.1117 g) of ZnI2 and 7 mmol (1.3332 g) of CuI, and put them into a 30 ml sample bottle to obtain reaction raw materials, wherein the molar mass of ZnI2 accounts for 5% of the molar mass of CuI;

[0032] S2. Add 4 ml of a mixed solvent of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) to the reaction raw material obtained in S1, wherein the volume ratio of N,N-dimethylformamide (DMF) to dimethyl sulfoxide (DMSO) is 3:1, and stir on a heating table at 27°C until the powder is completely dissolved to obtain a reaction precursor solution;

[0033] S3, adding 12 ml of anhydrous ethanol to the reaction precursor solution obtained in S2 as an anti-solvent, with the addition of the anti-solvent, a large amount of white precipitate is rapidly generated in the solution, which is then placed in a centrifuge tube and centrifuged at 10000 r / min for 1 min, discarding the supernatant and retaining the precipitate;

[0034] S4. Wash the residual solvent of the precipitate obtained in S3 with isopropanol, centrifuge three times and discard the supernatant, put the washed precipitate into a 70° C. oven and dry it for 12 hours to obtain CsCu2I3:Zn microcrystalline powder.

[0035] Example 2

[0036] The difference between this embodiment and embodiment 1 is that in this embodiment, 0.7 mmol (0.2235 g) of ZnI2 is weighed, and the percentage of the molar mass of ZnI2 to the molar mass of CuI is 10%.

[0037] Example 3

[0038] The difference between this embodiment and embodiment 1 is that in this embodiment, 1.05 mmol (0.3352 g) of ZnI2 is weighed, and the molar mass of ZnI2 accounts for 15% of the molar mass of CuI. The mass percentage and atomic percentage of each element of the prepared CsCu2I3:Zn are shown in Table 1:

[0039] Table 1 shows the mass percentage and atomic percentage of each element in CsCu2I3:Zn

[0040] element Wt% Atomic Percent Cu 1.31 34.21 Zn 0.06 1.49 I 3.70 48.44 Cs 1.27 15.86 Total 6.34 100.00

[0041] The SEM image of CsCu2I3:Zn obtained in this example is as follows Figure 1 As shown in Table 1 and Figure 1 It can be seen that the grains of CsCu2I3:Zn are micron-sized grains, and the corresponding constituent elements of Cs, Cu, I, and Zn are evenly distributed.

[0042] Example 4

[0043] The difference between this embodiment and embodiment 1 is that in this embodiment, 1.4 mmol (0.4469 g) of ZnI2 is weighed, and the percentage of the molar mass of ZnI2 to the molar mass of CuI is 20%.

[0044] Example 5

[0045] The difference between this embodiment and embodiment 1 is that in this embodiment, 2.1 mmol (0.6704 g) of ZnI2 is weighed, and the percentage of the molar mass of ZnI2 to the molar mass of CuI is 30%.

[0046] Comparative Example 1

[0047] The difference between this example and example 1 is that ZnI2 is not weighed in this example, and the product obtained by S4 is CsCu2I3. That is, this example adopts the antisolvent method to prepare CsCu2I3.

[0048] The XRD patterns of CsCu2I3:Zn obtained in Examples 1-5 and CsCu2I3 obtained in Comparative Example 1 are as follows: Figure 2 As shown, it can be seen from the figure that the products of Examples 1-5 and Comparative Example 1 are pure phases without impurity peaks, proving that the product prepared by the present invention has high purity.

[0049] The fluorescence emission spectra of CsCu2I3:Zn obtained in Examples 1-5 and CsCu2I3 obtained in Comparative Example 1 under 328nm excitation are shown in FIG. Figure 3 As shown in the figure, it can be seen that the fluorescence emission intensity of CsCu2I3:Zn doped with different proportions of Zn is higher than that of CsCu2I3 without Zn, and the CsCu2I3:Zn doped with 15% Zn in Example 3 has the highest fluorescence emission intensity, and the optimal emission wavelength is 556nm.

[0050] Comparative Example 2

[0051] CsCu2I3 was prepared by the saturated solution method: 3.5mmol (0.9093g) of CsI was placed in sample bottle one and 2ml of deionized water was added, 7mmol (1.3332g) of CuI was placed in sample bottle two and 2ml of hydroiodic acid and 0.5ml of hypophosphorous acid were added, sample bottles one and two were placed on a heating table at 27°C and stirred until the powder was completely dissolved to obtain a saturated aqueous solution and a saturated acid solution; the saturated acid solution in sample bottle two after the solution was quickly poured into the saturated aqueous solution in sample bottle one, and a large amount of white precipitate was quickly generated, which was then placed in a centrifuge tube and centrifuged at 10000r / min for 1min, and the supernatant was discarded and the precipitate was retained; next, isopropanol was used to wash away the residual acid, and the operation of centrifuging and discarding the supernatant was performed three times in total; the cleaned precipitate was placed in a 70°C oven and dried for 12h to obtain a white CsCu2I3 microcrystalline powder.

[0052] Comparative Example 3

[0053] CsCu2I3 was prepared by a simple solution method: 3.5mmol (0.9093g) CsI and 7mmol (1.3332g) CuI were weighed and placed in a 30ml sample bottle, 4ml of hydroiodic acid and 1ml of hypophosphorous acid were added, and the mixture was stirred on a heating platform at 27°C for 10min. The mixture was then placed in a centrifuge tube and centrifuged at 10000r / min for 1min, and the supernatant was discarded and the precipitate was retained. Next, isopropanol was used to wash away the residual solvent, and the operation of centrifuging and discarding the supernatant was performed three times in total. The cleaned precipitate was placed in a 70°C oven and dried for 12h to obtain a white CsCu2I3 microcrystalline powder.

[0054] Comparative Example 4

[0055] CsCu2I3 was prepared by solution-assisted crystallization: 3.5mmol (0.9093g) CsI and 7mmol (1.3332g) CuI were weighed and placed in a 30ml sample bottle, 20ml of anhydrous acetonitrile was added, and the mixture was stirred on a heating table at 27°C for 4h until the reaction was complete. The excess solution was then sucked out with a rubber-tipped dropper, leaving only the precipitate, which was washed once with n-hexane, centrifuged at 10000r / min for 1min, and the supernatant was discarded to keep the precipitate. The washed precipitate was placed in a 70°C oven and dried for 12h to obtain a white CsCu2I3 microcrystalline powder.

[0056] The yield bar graph of Comparative Examples 1-4 is as follows Figure 4 As shown in the figure, it can be seen that the yield of CsCu2I3 prepared by the anti-solvent method is as high as over 95%. Therefore, the anti-solvent method for preparing CsCu2I3:Zn has a higher yield.

[0057] The XRD patterns of CsCu2I3 obtained in Comparative Examples 1-4 are as follows Figure 5 As shown in the figure, it can be seen that the CsCu2I3 prepared by the saturated solution method is impure and there is still some CuI that has not reacted completely.

[0058] The fluorescence emission spectra of CsCu2I3 obtained in Comparative Examples 1-4 under 328nm excitation are as follows: Figure 6 As shown in the figure, it can be seen that the CsCu2I3 sample prepared by the simple solution method has the emission peak of Cs3Cu2I5, and the sample prepared by this method is impure.

[0059] In summary, although the fluorescence intensity of CsCu2I3 prepared by the saturated solution method and the simple solution method is high, they are not pure phases. The fluorescence intensity of the solution-assisted crystallization method and the anti-solvent method is not much different, but the solution-assisted crystallization method takes a long time to prepare, and the sample yield is not as good as the anti-solvent method. Therefore, relatively speaking, the anti-solvent method is the best preparation method.

[0060] The green all-inorganic metal halide CsCu2I3:Zn is prepared according to the above-mentioned preparation method of the green all-inorganic metal halide CsCu2I3:Zn.

[0061] Utilizing the above-mentioned green all-inorganic metal halide CsCu2I3:Zn, it is applied to scintillators, lighting, displays, solar cells, light-emitting diodes, X-ray detection and gamma-ray detection.

[0062] In summary, the raw materials used in the present invention are abundant, low-cost and environmentally friendly; the CsCu2I3:Zn product prepared by the anti-solvent method of the present invention has high purity and high yield, which reduces production costs; the fluorescence intensity of the CsCu2I3:Zn prepared by the present invention is significantly improved compared with the matrix CsCu2I3. In the field of scintillation imaging, the intensity of the fluorescent signal of the material directly affects the contrast, signal-to-noise ratio, sensitivity and resolution of the imaging, and therefore has a very important influence on the scintillation imaging to be performed later. The greater the intensity of the fluorescent signal, the clearer and more recognizable the image formed; and the signal-to-noise ratio of the imaging can be improved, making the formed image more stable and reliable; in addition, the sensitivity and resolution will also be improved accordingly, so that the target object can be better detected and distinguished.

[0063] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the technical solution of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for preparing green all-inorganic metal halide CsCu2I3:Zn, characterized in that: The following steps are involved: S1. Weigh CsI, ZnI2 and CuI and put them into a sample bottle to obtain reaction raw materials; S2, adding a mixed solvent of N,N-dimethylformamide and dimethyl sulfoxide to the reaction raw material obtained in S1, and stirring on a heating table until the powder is completely dissolved to obtain a reaction precursor solution; S3, adding anhydrous ethanol as an anti-solvent to the reaction precursor solution obtained in S2, generating a white precipitate in the solution, which is then placed in a centrifuge tube for centrifugation, discarding the supernatant and retaining the precipitate; S4. Wash the residual solvent of the precipitate obtained in S3 with isopropanol, centrifuge for multiple times to discard the supernatant, put the washed precipitate into an oven to dry, and obtain CsCu2I3:Zn microcrystalline powder.

2. The method for preparing a green all-inorganic metal halide CsCu2I3:Zn according to claim 1, characterized in that: In S1, the molar ratio of CsI and CuI is 1:

2.

3. The method for preparing a green all-inorganic metal halide CsCu2I3:Zn according to claim 1, characterized in that: In S1, the percentage of the molar mass of ZnI2 to the molar mass of CuI is any one of 5%, 10%, 15%, 20%, and 30%.

4. The method for preparing a green all-inorganic metal halide CsCu2I3:Zn according to claim 1, characterized in that: In S2, the volume ratio of N,N-dimethylformamide to dimethyl sulfoxide was 3:1, and the heating temperature of the heating stage was 27°C.

5. The method for preparing a green all-inorganic metal halide CsCu2I3:Zn according to claim 1, characterized in that: In S3, the volume ratio of anhydrous ethanol to the mixed solvent of N,N-dimethylformamide and dimethyl sulfoxide in S2 is 3:

1.

6. The method for preparing a green all-inorganic metal halide CsCu2I3:Zn according to claim 1, characterized in that: In S4, the oven temperature is 70°C and the oven drying time is 12 h.

7. A green all-inorganic metal halide CsCu2I3:Zn obtained according to the preparation method of a green all-inorganic metal halide CsCu2I3:Zn according to any one of claims 1 to 6.

8. The use of the green all-inorganic metal halide CsCu2I3:Zn according to claim 7, characterized in that: It is used in scintillators, lighting, displays, solar cells, light-emitting diodes, X-ray detection and gamma-ray detection.