Near-infrared fluorescent glass ceramic material, preparation method thereof and LED light source containing near-infrared fluorescent glass ceramic material

By developing near-infrared fluorescent glass ceramic materials with the chemical formula MP3O9: xCr3+, yLn3+, the problems of low luminous efficiency and poor thermal stability of existing near-infrared LED chips have been solved, and efficient and stable near-infrared luminescence effects have been achieved, which is suitable for high-power applications. LED and laser applications.

CN118851573APending Publication Date: 2024-10-29JIANGXI UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410874971.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The luminous efficiency of existing near-infrared LED chips is not high and the cost is high. The aging of packaging materials results in poor thermal stability, which limits their use in high-power and high-efficiency applications.

Method used

Develop a near-infrared fluorescent glass ceramic material with the chemical formula MP3O9: xCr3+, yLn3+, in which the M element is selected from Al, Ga, Sc, In, V, Fe or trivalent rare earth ions, and the Ln element is Yb, Nd, Pr, Eu , Dy, Sm, Cr3+ as the luminescent center ion, and Ln3+ as the sensitizing ion. The luminous efficiency and thermal stability are improved through specific preparation methods.

Benefits of technology

It significantly improves the luminous efficiency and thermal stability of near-infrared luminescent materials, is suitable for high-power LED devices and laser excitation devices, and solves the problems of aging and insufficient thermal stability of traditional powder materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851573A_ABST
    Figure CN118851573A_ABST
Patent Text Reader

Abstract

The invention discloses a near-infrared fluorescent glass ceramic material, a preparation method thereof and an LED light source containing the near-infrared fluorescent glass ceramic material, and belongs to the technical field of fluorescent materials. The chemical composition of the fluorescent glass ceramic is represented by a chemical formula MP3O9: xCr < 3 + >, yLn < 3 + >, and the element M is selected from one or more of Al, Ga, Sc, In, V, Fe and trivalent rare earth ions; the Ln element is selected from one or more of Yb, Pr, Nd, Eu, Dy and Sm rare earth ions, Cr < 3 + > is a luminescence center ion, 0.01 mol% < = x < = 100 mol%, and 0.00 mol% < = y < = 100 mol%. The near-infrared fluorescent glass ceramic material provided by the invention has higher luminous thermal stability and luminous quantum yield, and is suitable for high-power devices.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention belongs to the technical field of fluorescent glass ceramics, and specifically relates to a fluorescent glass ceramic with broadband near-infrared emission, a preparation method thereof, and an LED light source containing the luminescent material. Background Art

[0002] In the context of the continuous development of science and technology today, near-infrared spectroscopy and imaging technology are gradually becoming indispensable tools in the fields of food testing, biological testing and medical treatment. The rapid development of these technologies is driven by the growing demand for convenient testing equipment, but it also faces technical and material challenges. As one of the key components of these technologies, near-infrared LED devices excel in selective light sources in specific bands due to their narrow-band emission characteristics. However, there are some significant problems with near-infrared LED chips currently on the market, such as low luminous efficiency and high cost, which limits their widespread use in high-power, high-efficiency applications.

[0003] In recent years, LED lamps converted from near-infrared phosphors have gradually attracted attention due to their good performance in small and convenient detection. However, the encapsulation glue and phosphors used in the packaged devices may age or even carbonize over time, resulting in a decrease in luminous efficiency. In addition, these materials have poor thermal conductivity, which can easily cause the equipment to overheat, thus affecting its service life. Therefore, in order to promote the development of high-power laser lighting technology, it is urgent to develop luminescent inorganic fluorescent bulk materials with high luminous efficiency and excellent thermal stability.

[0004] Glass materials are an ideal choice in the field of near-infrared luminescent materials due to their unique physical and chemical properties. Compared with traditional resin materials, glass materials have better chemical stability and can effectively extend the service life of devices. In addition, the disordered but ordered network structure of glass allows activated ions to be doped into the glass matrix at high concentrations, thereby further improving luminescence efficiency and stability.

[0005] Recently, glass ceramics as an emerging material have attracted much attention from researchers. For example, Gd3Al2Ga3O prepared by Hangjie Jiang et al. 12 :Cr 3+ Fluorescent glass ceramics have significantly improved absorption efficiency and external quantum efficiency, showing excellent luminescence performance. In addition, some Chinese patents have also disclosed new methods and technologies for using glass ceramic materials to improve near-infrared luminescence efficiency. These technologies significantly improve the luminescence quantum yield by changing the organizational form of the material and optimizing the annealing system, thereby meeting the requirements of high-efficiency near-infrared detection technology for light source performance.

[0006] In summary, the luminescence properties of near-infrared luminescent materials, including luminescence efficiency and thermal stability, can be effectively improved by preparing and applying glass-ceramic materials. This not only helps promote the application of near-infrared LED devices in the field of detection, but also lays the foundation for the further development of high-power laser lighting technology. Future research and development will continue to focus on the optimization of glass-ceramic materials and their practical application in various applications. Summary of the invention

[0007] In order to solve the problems existing in the prior art, the present invention provides a near-infrared fluorescent glass-ceramic material, a preparation method thereof and a light-emitting device comprising the material.

[0008] <Fluorescent Glass Ceramics>

[0009] The present invention provides a near-infrared fluorescent glass ceramic material, wherein the fluorescent glass ceramic material comprises a near-infrared fluorescent glass ceramic material having a chemical formula of MP3O9: xCr 3+ ,yLn 3+ The inorganic compound, wherein the M element is selected from one or more of Al, Ga, Sc, In, V, Fe or trivalent rare earth ions; the Ln element is one or more of Yb, Nd, Pr, Eu, Dy, Sm rare earth ions, Cr 3+ is the luminescent central ion, Ln 3+ is the sensitizing ion, where

[0010] 0.001mol%≤x≤100mol%, 0.00mol%≤y≤100mol%, that is, single doping Cr can be selected 3+ Cr can also be selected as the luminescent central ion. 3+ and Ln 3+ Co-doping.

[0011] According to an embodiment of the present invention, preferably Cr 3+ The concentration of Ln is 0.001mol%≤x≤0.12mol%, preferably Ln 3+ The concentration is 0.03mol%≤x≤0.12mol%.

[0012] According to the implementation scheme of the present invention, the chemical composition of the luminescent material can be AlP3O9:Cr 3+ 、GaP3O9:Cr 3 + ScP3O9:Cr 3+ 、InP3O9:Cr 3+ 、VP3O9:Cr 3+ 、FeP3O9:Cr 3+ ScP3O9:Cr 3+ ,Yb 3+ ScP3O9:Cr3+ ,Nd 3+ 、ScP3O9:Cr 3+ ,Pr 3+ 、ScP3O9:Cr 3+ ,Eu 3+ 、VP3O9:Cr 3+ ,Yb 3+ 、VP3O9:Cr 3+ ,Nd 3+ 、VP3O9:Cr 3+ ,Pr 3+ 、VP3O9:Cr 3+ ,Eu 3+ 、InP3O9:Cr 3+ ,Yb 3+ 、InP3O9:Cr 3+ ,Nd 3+ 、InP3O9:Cr 3+ ,Pr 3+ 、InP3O9:Cr 3+ ,Eu 3+ 、ScP3O9:Cr 3+ ,Pr 3+ ,Nd 3+ 、ScP3O9:Cr 3+ ,Pr 3+ ,Yb 3+ 、ScP3O9:Cr 3+ ,Sm 3+ ,Eu 3+ 、ScP3O9:Cr 3+ ,Dy 3+ ,Eu 3+ 、ScP3O9:Cr 3+ ,Dy 3+ ,Sm 3+ 、VP3O9:Cr 3+ ,Pr 3+ ,Nd 3+ 、VP3O9:Cr 3+ ,Pr 3+ ,Yb 3+ 、VP3O9:Cr 3+ ,Sm 3+ ,Eu 3+ 、VP3O9:Cr 3 + ,Sm 3+ ,Dy 3+ 、VP3O9:Cr 3+ ,Dy 3+ ,Eu 3+ 、InP3O9:Cr 3+ ,Pr3+ ,Yb 3+ 、InP3O9:Cr 3+ ,Pr 3+ ,Nd 3+ 、InP3O9:Cr 3 + ,Dy 3+ ,Sm 3+ 、InP3O9:Cr 3+ ,Dy 3+ ,Eu 3+ 、InP3O9:Cr 3+ ,Sm 3+ ,Eu 3+ .

[0013] According to an embodiment of the present invention, the fluorescent glass ceramic can be excited under blue light to emit near-infrared light with a wavelength of 650-1300 nm and a peak value in the range of 750-950 nm.

[0014] <Method for preparing fluorescent glass ceramics>

[0015] The present invention provides a method for preparing near-infrared fluorescent glass, the preparation method comprising the following steps: Step 1: According to the chemical formula MP3O9:xCr 3+ ,yLn 3+ The chemical ratio of the compound containing the M element, the compound containing the P element, the compound containing the Cr element and the compound containing the Ln element are weighed. The obtained compounds are mixed and ground to obtain a mixture, and the obtained mixture is pre-calcined at a low temperature to obtain a pre-calcined product. Step 2: The pre-calcined product obtained in step 1 is calcined for the first time, then ground, and then calcined for the second time. After the sample is taken out, it is post-processed to obtain a chemical formula of MP3O9:xCr 3+ ,yLn 3+ of phosphor.

[0016] Step 3: Put the phosphor obtained in step 2 into an alumina crucible, heat and melt it in an air atmosphere, anneal it, and cool it to room temperature along with the furnace to obtain a near-infrared fluorescent glass material.

[0017] Step 4: The glass material obtained in step 3 is crystallized by an amorphous crystallization method under air atmosphere, and then the crystallized material is post-treated to obtain near-infrared fluorescent glass ceramics. According to the embodiment of the present invention, in step 1, there is no special requirement for the compound containing M. The preferred M source is selected from oxides containing M elements, hydroxides containing M elements, carbonates containing M, and nitrates containing M. Exemplary oxides containing M elements are Al2O3, Ga2O3, Sc2O3, In2O3, V2O5, and Fe2O3. According to the scheme implemented by the present invention, in step 1, the P-containing source compound is selected from one or more of phosphates containing P elements and oxides containing P elements, preferably ammonium dihydrogen phosphate and diammonium hydrogen phosphate. According to the scheme implemented by the present invention, in step 1, the Cr-containing compound is selected from one or more of carbonates containing Cr elements, oxides containing Cr elements, nitrates containing Cr elements, and halides containing Cr elements, preferably Cr2O3 and CrF3.

[0018] According to the scheme implemented in the present invention, in step 1, the compound containing Ln is selected from oxides containing Ln, hydroxides containing Ln, nitrates containing Ln, and halides containing Ln, preferably Yb2O3, Nd2O3, Pr2O3, Eu2O3, Dy2O3, and Sm2O3.

[0019] According to the solution implemented in the present invention, in step 1, the luminescent material MP3O9:xCr 3+ ,yLn 3+ The purity of the raw materials used is ≥99%, preferably ≥99.5%.

[0020] According to the scheme implemented in the present invention, in step 1, according to the chemical formula MP3O9:xCr 3+ ,yLn 3+ The compound containing M element, the compound containing P element, the compound containing Cr element, and the compound containing Ln element are weighed according to the stoichiometric ratio of each element in the mixture, wherein the amount of the P source compound used can be appropriately excessive, for example, an excess of 5-200wt.%. According to the scheme implemented in the present invention, in step 1, the weighed compound containing M element, the compound containing P element, the compound containing Cr element, and the compound containing Ln element are mixed, and the mixing method is not particularly limited, and grinding equipment such as a mortar, a ball mill, and a mixer can be used.

[0021] According to the implementation scheme of the present invention, in step 1, the pre-firing is carried out at a temperature lower than 300° C. for 2-5 hours, and the pre-firing atmosphere can be carried out in air or inert atmosphere.

[0022] According to the implementation scheme of the present invention, in step 2, the first and second calcinations can be carried out in air, an inert atmosphere or a reducing atmosphere. The inert atmosphere is, for example, nitrogen, argon, etc.; the reducing atmosphere is, for example, a mixture of (5-15v%) H2 and (95-85v%) N2, or an atmosphere containing carbon powder.

[0023] According to the scheme implemented in the present invention, in step 2, the conditions of the first calcination include: temperature of 300-900°C, preferably 400-800°C, calcination time of 1-30h, preferably 8-15h. The conditions of the second calcination include: temperature of 800-1400°C, preferably 1000-1300°C, calcination time of 1-30h, preferably 8-15h.

[0024] According to the scheme implemented in the present invention, in step 2, the number of calcinations is at least two, for example, two, three or more times. And preferably, the temperature of each calcination is different from each other. More preferably, the temperature of each calcination is on the rise. In addition, before the next calcination, the calcined product of the previous time can be ground.

[0025] According to the implementation scheme of the present invention, in step three, 0.5 mol%-5 mol% of a co-solvent may be added, for example: Li2CO3, H3BO3, NH4H2PO4, NH4F, LiF.

[0026] According to the scheme implemented in the present invention, in step three, the heating and melting temperature is 1300-1800°C, preferably 1550-1700°C, and the melting time is 10min-6h, preferably 20min-4h; the annealing temperature is 400-700°C, preferably 450-600°C; the annealing time is 1-20h, preferably 3-10h.

[0027] According to the implementation scheme of the present invention, in step four, the amorphous crystallization method is thermal crystallization, and its crystallization temperature is 600-1100°C, preferably 650-900°C; the crystallization time is 30min-30h, preferably 1-24h; the post-treatment includes: polishing with 180 mesh, 400 mesh, 800 mesh, 1000 mesh, 1500 mesh, and 2000 mesh sandpaper, and then polishing with polishing powder, preferably the main components of the polishing powder are aluminum oxide, titanium oxide, and cerium oxide, and finally washing and drying.

[0028] <LED light source including fluorescent glass ceramic>

[0029] The present invention also provides an LED light source, which comprises at least one of the above-mentioned near-infrared fluorescent glass-ceramic materials.

[0030] Furthermore, the present invention provides an LED light source, which includes a fluorescent conversion layer and an LED semiconductor chip or a laser light source, and the fluorescent conversion layer is carried on the LED semiconductor chip or the laser light source, wherein the fluorescent conversion layer includes at least one of the above-mentioned near-infrared fluorescent glass ceramic materials.

[0031] According to an embodiment of the present invention, the fluorescent conversion layer comprises a packaging glue and a fluorescent glass ceramic, wherein the fluorescent glass ceramic is attached to the device through the packaging glue. The packaging can be an organic material such as epoxy resin, polycarbonate or silica gel, or an inorganic material such as boron oxide, potassium oxide, silicon dioxide, etc.; preferably silica gel. There is no particular limitation on the amount of the packaging material, as long as it can be attached to the LED semiconductor chip or laser light source according to the known operation in the art.

[0032] According to an embodiment of the present invention, the LED semiconductor chip is at least one of a blue light LED chip and a red light LED chip.

[0033] According to an embodiment of the present invention, the peak values ​​of the blue light LED chip and the laser light source are within the range of 400-500nm.

[0034] According to an embodiment of the present invention, the peak values ​​of the red light LED chip and the laser light source are within the range of 590-680 nm.

[0035] According to an embodiment of the present invention, the LED light source is a fluorescence conversion type near-infrared LED device. Further, the fluorescence conversion type near-infrared LED device is used in the fields of biometrics, sensing, food testing, medical testing, agricultural production or biological imaging.

[0036] Beneficial effects of the present invention:

[0037] (1) The present invention provides near-infrared fluorescent glass ceramics, which can be used as light conversion materials for blue LED chips and red LED chips. Compared with traditional powder materials, the glass ceramic material effectively improves the thermal stability and luminous efficiency of near-infrared luminescence. It can be used for high-power LED devices and laser excitation devices.

[0038] (2) The near-infrared fluorescent glass ceramics of the present invention are Cr 3+ As an activator, Ln 3+ As a sensitizer, near-infrared luminescence enhancement and spectrum broadening are achieved, making MP3O9:xCr 3+ ,yLn 3+ Compared with phosphor materials, the luminous efficiency and thermal stability of fluorescent glass-ceramics are significantly improved.

[0039] (3) The preparation process of the fluorescent glass ceramic material provided by the present invention is simple, pollution-free and low-cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments.

[0041] Figure 1 The XRD diagrams of the fluorescent glass ceramics prepared in Examples 1, 2, 3, 4 and 5 of the present invention are shown.

[0042] Figure 2 The glass materials and fluorescent glass ceramics prepared in Examples 1, 2, 3, 4 and 5 of the present invention.

[0043] Figure 3 This is the excitation emission spectrum of the fluorescent glass ceramic prepared in Example 3 of the present invention.

[0044] Figure 4 This is a comparison chart of the emission intensity of the fluorescent glass ceramics prepared in Example 3 of the present invention at different temperatures.

[0045] Figure 5 This is the excitation emission spectrum of the fluorescent glass ceramic prepared in Example 6 of the present invention.

[0046] Figure 6 This is the excitation emission spectrum of the fluorescent glass ceramic prepared in Example 7 of the present invention.

[0047] Figure 7 This is the excitation emission spectrum of the fluorescent glass ceramic prepared in Example 9 of the present invention.

[0048] Figure 8 This is the electroluminescence spectrum diagram and actual application diagram of the LED device prepared in Example 13 of the present invention. DETAILED DESCRIPTION

[0049] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0050] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0051] Example 1: AlP3O9:5%Cr 3+ Preparation of fluorescent glass ceramics

[0052] This embodiment adopts a high temperature solid phase method to synthesize phosphors, then melts them into near infrared fluorescent glass, and crystallizes them to obtain fluorescent glass ceramic materials. First, according to the chemical formula AlP3O9: 5% Cr 3+ The stoichiometric ratio of various elements in the material is weighed. The weighed raw materials are ground in a mortar, mixed evenly, and then put into a corundum crucible, kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace, calcined at 600°C for 3 hours in an air atmosphere, and ground again after cooling to room temperature. Then, it is kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace and sintered at 1100°C for 6 hours. After the calcination is completed, the obtained sample is ground to obtain a chemical formula of AlP3O9:5%Cr 3+ The fluorescent powder is then put into a corundum crucible, melted at 1600°C for 30 minutes, poured into a mold, annealed at 450°C for 4 hours, cooled to room temperature to obtain a near-infrared fluorescent glass material, heat treated at 835°C for 4 hours, and finally ground and polished to obtain fluorescent glass ceramics.

[0053] Example 2-5: AlP3O9:5%Cr 3+ Preparation of fluorescent glass ceramics

[0054] This embodiment adopts the same method as Example 1, except that the crystallization treatment time and temperature of the prepared near-infrared fluorescent glass material are different. The specific treatment time and temperature are shown in Table 1

[0055] Table 1

[0056]

[0057] Example 6: ScP3O9:7%Cr 3+ Preparation of fluorescent glass ceramics

[0058] This embodiment adopts a high temperature solid phase method to synthesize phosphors, then melts them into near-infrared fluorescent glass, and crystallizes them to obtain fluorescent glass ceramic materials. First, according to the chemical formula ScP3O9:7%Cr 3+ The stoichiometric ratio of various elements in the raw materials is weighed. The weighed raw materials are ground in a mortar, mixed evenly and put into a corundum crucible, kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace, calcined at 500°C for 3 hours in an air atmosphere, and ground again after cooling to room temperature. Then, it is kept in an oven at 200°C for 2 hours again, cooled and taken out, and then put into a box furnace and sintered at 1250°C for 6 hours. After the calcination is completed, the obtained sample is ground to obtain a chemical formula of ScP3O9:7%Cr 3+The fluorescent powder was then put into a corundum crucible, melted at 1650°C for 40 minutes, poured into a mold, annealed at 500°C for 4 hours, cooled to room temperature to obtain a near-infrared fluorescent glass material, heat treated at 900°C for 12 hours, and finally ground and polished to obtain fluorescent glass ceramics.

[0059] Example 7: GaP3O9:6%Cr 3+ Preparation of fluorescent glass ceramics

[0060] This embodiment adopts a high temperature solid phase method to synthesize phosphors, then melts them into near-infrared fluorescent glass, and crystallizes them to obtain fluorescent glass ceramic materials. First, according to the chemical formula GaP3O9:6%Cr 3+ The stoichiometric ratio of various elements in the raw materials is weighed. The weighed raw materials are ground in a mortar, mixed evenly and put into a corundum crucible, kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace, calcined at 600°C for 3 hours in an air atmosphere, and ground again after cooling to room temperature. Then, keep in an oven at 200°C for 2 hours again, cool and take out, and then put into a box furnace and sintered at 950°C for 6 hours. After calcination, grind the obtained sample to obtain a chemical formula of GaP3O9:6%Cr 3+ The fluorescent powder was then put into a corundum crucible, melted at 1580°C for 30 minutes, poured into a mold, annealed at 500°C for 4 hours, cooled to room temperature to obtain a near-infrared fluorescent glass material, heat treated at 800°C for 6 hours, and finally ground and polished to obtain fluorescent glass ceramics.

[0061] Example 8: InP3O9:5%Cr 3+ Preparation of fluorescent glass ceramics

[0062] This embodiment adopts a high temperature solid phase method to synthesize phosphors, then melts them into near-infrared fluorescent glass, and crystallizes them to obtain fluorescent glass ceramic materials. First, according to the chemical formula InP3O9: 5% Cr 3+ The stoichiometric ratio of various elements in the raw materials is weighed. The weighed raw materials are ground in a mortar, mixed evenly and put into a corundum crucible, kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace, calcined at 550°C for 3 hours in an air atmosphere, and ground again after cooling to room temperature. Then, keep in an oven at 200°C for 2 hours again, cool and take out, and then put into a box furnace and sintered at 1100°C for 6 hours. After the calcination is completed, the obtained sample is ground to obtain a chemical formula of InP3O9:5%Cr 3+ The fluorescent powder is then put into a corundum crucible, melted at 1550°C for 20 minutes, poured into a mold, annealed at 450°C for 4 hours, cooled to room temperature to obtain a near-infrared fluorescent glass material, heat treated at 820°C for 8 hours, and finally ground and polished to obtain fluorescent glass ceramics.

[0063] Example 9: ScP3O9:7%Cr 3+ ,3%Nd 3+ Preparation of fluorescent glass ceramics

[0064] This embodiment adopts a high temperature solid phase method to synthesize phosphors, then melts them into near-infrared fluorescent glass, and crystallizes them to obtain fluorescent glass ceramic materials. First, according to the chemical formula ScP3O9:7%Cr 3+ ,3%Nd 3+ The stoichiometric ratio of various elements in the raw materials is weighed. The weighed raw materials are ground in a mortar, mixed evenly and put into a corundum crucible, kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace, calcined at 600°C for 3 hours in an air atmosphere, and ground again after cooling to room temperature. Then, keep in an oven at 200°C for 2 hours again, cool and take out, and then put into a box furnace and sintered at 1250°C for 8 hours. After the calcination is completed, the obtained sample is ground to obtain a chemical formula of ScP3O9:7%Cr 3+ ,3%Nd 3+ The fluorescent powder is then placed in a corundum crucible, melted at 1650°C for 20 minutes, introduced into a mold, annealed at 500°C for 4 hours, cooled to room temperature to obtain a glass precursor, heat treated at 850°C for 8 hours, and finally ground and polished to obtain fluorescent glass ceramics.

[0065] Example 10: ScP3O9: 7% Cr 3+ ,3%Pr 3+ Preparation of fluorescent glass ceramics

[0066] This embodiment adopts a high temperature solid phase method to synthesize phosphors, then melts them into near-infrared fluorescent glass, and crystallizes them to obtain fluorescent glass ceramic materials. First, according to the chemical formula ScP3O9:7%Cr 3+ ,3%Pr 3+ The stoichiometric ratio of various elements in the raw materials is weighed. The weighed raw materials are ground in a mortar, mixed evenly and put into a corundum crucible, kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace, calcined at 600°C for 3 hours in an air atmosphere, and ground again after cooling to room temperature. Then, keep in an oven at 200°C for 2 hours again, cool and take out, and then put into a box furnace and sintered at 1150°C for 6 hours. After calcination, the obtained sample is ground to obtain a chemical formula of ScP3O9:7%Cr 3+ ,3%Pr 3+The fluorescent powder is then placed in a corundum crucible, melted at 1650°C for 20 minutes, introduced into a mold, annealed at 500°C for 4 hours, cooled to room temperature to obtain a glass precursor, heat treated at 820°C for 6 hours, and finally ground and polished to obtain fluorescent glass ceramics.

[0067] Example 11: VP3O9: 3% Cr 3+ ,3%Yb 3+ Preparation of fluorescent glass ceramics

[0068] This embodiment adopts a high temperature solid phase method to synthesize phosphors, then melts them into near-infrared fluorescent glass, and crystallizes them to obtain fluorescent glass ceramic materials. First, according to the chemical formula VP3O9: 3%Cr 3+ ,3%Yb 3+ The stoichiometric ratio of various elements in the raw materials is weighed. The weighed raw materials are ground in a mortar, mixed evenly and put into a corundum crucible, kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace, calcined at 600°C for 3 hours in an air atmosphere, and ground again after cooling to room temperature. Then, keep in an oven at 200°C for 2 hours again, cool and take out, and then put into a box furnace and sintered at 1050°C for 10 hours. After calcination, the obtained sample is ground to obtain a chemical formula of VP3O9: 3%Cr 3+ ,3%Yb 3+ The fluorescent powder is then placed in a corundum crucible, melted at 1550°C for 20 minutes, introduced into a mold, annealed at 450°C for 4 hours, cooled to room temperature to obtain a glass precursor, heat treated at 780°C for 6 hours, and finally ground and polished to obtain fluorescent glass ceramics.

[0069] Example 12: InP3O9:3%Cr 3+ ,3%Dy 3+ Preparation of fluorescent glass ceramics

[0070] This embodiment adopts a high temperature solid phase method to synthesize phosphors, then melts them into near-infrared fluorescent glass, and crystallizes them to obtain fluorescent glass ceramic materials. First, according to the chemical formula InP3O9: 3% Cr 3+ ,3%Dy 3+ The stoichiometric ratio of various elements in the material is weighed. The weighed raw materials are ground in a mortar, mixed evenly, and then put into a corundum crucible, kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace, calcined at 600°C for 3 hours in an air atmosphere, and ground again after cooling to room temperature. Then, it is kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace and sintered at 1100°C for 8 hours. After the calcination is completed, the obtained sample is ground to obtain a chemical formula of InP3O9:3%Cr 3+ ,3%Dy3+ The fluorescent powder is then placed in a corundum crucible, melted at 1600°C for 30 minutes, introduced into a mold, annealed at 500°C for 4 hours, cooled to room temperature to obtain a glass precursor, heat treated at 830°C for 10 hours, and finally ground and polished to obtain fluorescent glass ceramics.

[0071] Example 13: LED device packaging and application

[0072] The chemical formula of AlP3O9:5%Cr prepared in Example 3 is 3+ Fluorescent glass ceramic materials are used to encapsulate LED devices. First, the silica gel is evenly coated on the fluorescent glass ceramic material and attached to the surface of the 450nm InGaN chip. Then it is placed in an oven and dried at 80℃ for 2h, and then dried at 150℃ for 2h to completely solidify the silica gel and obtain an LED device. The LED device is used for night vision photography and non-destructive testing. Comparative Example 1: AlP3O9:5%Cr 3+ Preparation of phosphor

[0073] This embodiment adopts the high temperature solid phase method to synthesize, first according to the chemical formula AlP3O9: 5%Cr 3+ The stoichiometric ratio of various elements in the raw material is weighed, the weighed raw materials are ground in a mortar, mixed evenly and put into a corundum crucible, kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace, calcined at 600°C for 3 hours in an air atmosphere, and ground again after cooling to room temperature. Then, it is kept in an oven at 200°C for 2 hours again, cooled and taken out, and then put into a box furnace and sintered at 1100°C for 6 hours. After calcination, the obtained sample is ground to obtain a near-infrared luminescent material.

[0074] Comparative Example 2: GaP3O9:6%Cr 3+ Preparation of phosphor

[0075] This embodiment adopts the high temperature solid phase method to synthesize, first according to the chemical formula GaP3O9:6%Cr 3+ The stoichiometric ratio of various elements in the raw material is weighed. The weighed raw materials are ground in a mortar, mixed evenly and put into a corundum crucible, kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace, calcined at 500°C for 3 hours in an air atmosphere, and ground again after cooling to room temperature. Then, keep in an oven at 200°C for 2 hours again, cool and take out, and then put into a box furnace and sintered at 950°C for 8 hours. After calcination, grind the obtained sample to obtain a near-infrared luminescent material.

[0076] Comparative Example 3: ScP3O9:7%Cr 3+ Preparation of fluorescent materials

[0077] This embodiment adopts the high temperature solid phase method to synthesize, first according to the chemical formula ScP3O9:7%Cr 3+ The stoichiometric ratio of various elements in the raw material is weighed. The weighed raw materials are ground in a mortar, mixed evenly and put into a corundum crucible, kept in an oven at 200°C for 2 hours, cooled and taken out, and then put into a box furnace, calcined at 600°C for 3 hours in an air atmosphere, and ground again after cooling to room temperature. Then, keep in an oven at 200°C for 2 hours again, cool and take out, and then put into a box furnace and sintered at 1250°C for 6 hours. After calcination, grind the obtained sample to obtain a near-infrared luminescent material.

[0078] The phases of the samples of the embodiments and comparative examples were analyzed by X-ray powder diffractometer (D8 advanced, Germany).

[0079] The excitation and emission spectra of the samples were measured by using a FLS980 (Edinburgh Instruments) fluorescence spectrometer. The temperature-dependent emission spectra of the materials were tested in combination with a 77-600K variable temperature stage to evaluate the thermal stability of the materials. The thermal stability of the fluorescent glass-ceramics prepared in Example 3 was as follows: Figure 3 shown.

[0080] A fiber optic spectrometer (ATP5020R) was used to test the luminescence quantum yield of the material through fiber coupling and integrating sphere.

[0081] The samples synthesized by solid phase reaction method show pure phase by XRD analysis. The fluorescent glass ceramics obtained after high temperature melting and crystallization treatment have some impurities, which do not affect their luminescence performance. For example, the XRD diffraction pattern of the near-infrared fluorescent glass ceramics prepared in Example 1 is as follows: Figure 1 shown.

[0082] The excitation and emission spectra of the samples were measured using a FLS980 (Edinburgh Instruments) fluorescence spectrometer. The excitation and emission spectra of the luminescent material of Example 3 are shown in Figure 2 As shown, the excitation spectrum of the luminescent material contains three effective excitation bands, namely 250-350nm, 420-580nm and 600-800nm; it can be seen that the emission spectrum of the luminescent material covers 800-1100nm, that is, it has near-infrared broadband emission performance. Figure 4 The excitation emission spectrum of the fluorescent glass ceramic prepared in Example 6 of the present invention is as follows: Figure 4 It can be seen that under the excitation of 780nm, the excitation spectrum ranges from 250-350nm, 420-550nm, and 600-800nm. Figure 5The excitation emission spectra of the fluorescent glass ceramics prepared in Example 7 of the present invention are as follows: the excitation spectrum ranges from 250-350nm, 420-550nm, and 600-800nm, and the emission wavelength ranges from 800-1100nm, which indicates that the material has broadband emission.

[0083] In addition, the luminescence quantum yield and thermal stability of the near-infrared luminescent materials prepared in Examples 1-12 and Comparative Examples 1-3 were tested. The test results are shown in Table 2. Compared with the comparative example, the fluorescent glass ceramics in the embodiments have better absorption efficiency and higher external quantum efficiency due to their uniform grain distribution and the optical transmission properties of the glass ceramics themselves. In addition, since the crystalline phase of the glass ceramics is closely connected to the glass phase, the material obtains better fluorescence thermal stability. According to the comparison of the embodiments, different crystallization times and temperatures will affect the luminescence efficiency, and different crystallization treatment processes should be selected for different materials. The near-infrared fluorescent glass ceramics prepared by the present invention have significantly higher absorption efficiency, external quantum yield and better thermal stability.

[0084] Table 2

[0085]

[0086] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A near-infrared fluorescent glass-ceramic material, characterized in that: The chemical composition of the material is MP3O9:xCr 3+ ,yLn 3+ Indicates that, the M element is selected from one or more of Al, Ga, Sc, In, V, Fe or trivalent rare earth ions; the Ln element is one or more of Yb, Nd, Pr, Eu, Dy, Sm rare earth ions; Cr 3+ is the luminescent central ion, Ln 3+ is a sensitizing ion, wherein 0.01 mol%≤x≤100 mol%, 0.00 mol%≤y≤100 mol%.

2. A near-infrared fluorescent glass-ceramic material according to claim 1, characterized in that: The chemical composition of the material is AlP3O9:Cr 3+ 、GaP3O9:Cr 3+ ScP3O9:Cr 3+ 、InP3O9:Cr 3+ 、VP3O9:Cr 3+ 、FeP3O9:Cr 3+ ScP3O9:Cr 3+ ,Yb 3+ ScP3O9:Cr 3+ ,Nd 3+ ScP3O9:Cr 3+ ,Pr 3+ ScP3O9:Cr 3+ ,Eu 3+ 、VP3O9:Cr 3+ ,Yb 3+ 、VP3O9:Cr 3+ ,Nd 3+ 、VP3O9:Cr 3+ ,Pr 3+ 、VP3O9:Cr 3+ ,Eu 3+ 、InP3O9:Cr 3+ ,Yb 3+ 、InP3O9:Cr 3+ ,Nd 3+ 、InP3O9:Cr 3+ ,Pr 3+ 、InP3O9:Cr 3+ ,Eu 3+ ScP3O9:Cr 3+ ,Pr 3+ ,Nd 3+ ScP3O9:Cr 3+ ,Pr 3+ ,Yb 3+ ScP3O9:Cr 3+ ,Sm 3+ ,Eu 3+ ScP3O9:Cr 3+ ,Dy 3+ ,Eu 3+ ScP3O9:Cr 3+ ,Dy 3+ ,Sm 3+ 、VP3O9:Cr 3+ ,Pr 3+ ,Nd 3+ 、VP3O9:Cr 3+ ,Pr 3+ ,Yb 3+ 、VP3O9:Cr 3+ ,Sm 3+ ,Eu 3+ 、VP3O9:Cr 3+ ,Sm 3+ ,Dy 3+ 、VP3O9:Cr 3+ ,Dy 3+ ,Eu 3+ 、InP3O9:Cr 3+ ,Pr 3+ ,Yb 3+ 、InP3O9:Cr 3+ ,Pr 3+ ,Nd 3+ 、InP3O9:Cr 3+ ,Dy 3+ ,Sm 3+ 、InP3O9:Cr 3+ ,Dy 3+ ,Eu 3+ 、InP3O9:Cr 3+ ,Sm 3+ ,Eu 3+ ; The near-infrared fluorescent glass-ceramic material can be excited by blue light and red light.

3. The method for preparing the near-infrared fluorescent glass-ceramic material according to claim 1 and claim 2, characterized in that: The following steps are involved: Step 1: According to the stoichiometric ratio in the chemical formula, weigh the compounds containing each element, mix and grind them to obtain a mixture, and pre-calcine the obtained mixture at a low temperature to obtain a pre-calcined product; Step 2: calcining the pre-calcined product obtained in step 1 for the first time, grinding it later, and then calcining it for the second time. After taking out the sample, post-processing is performed to obtain a near-infrared luminescent material powder; Step 3: putting the luminescent material powder obtained in step 2 into an alumina crucible, heating and melting it in an air atmosphere, annealing it, and cooling it to room temperature with the furnace to obtain a near-infrared fluorescent glass material; Step 4: crystallize the glass material obtained in step 3 in an air atmosphere using an amorphous crystallization method, and then post-treat the crystallized material to obtain near-infrared fluorescent glass ceramics.

4. The preparation method according to claim 3, characterized in that: In the step 1, the low-temperature pre-calcination is carried out in an oven at a temperature below 300° C. for 2-5 hours.

5. The preparation method according to claim 3, characterized in that: In the step 2, the first calcination is carried out in air or an inert atmosphere; the temperature of the first calcination is 400-800°C, and the calcination time is 8-15h; the conditions of the second calcination include: the temperature is 1000-1300°C, and the calcination time is 8-15h.

6. The preparation method according to claim 3, characterized in that: In the step three, the heating melting temperature is 1550-1700° C., and the melting time is 20 min-4 h; the annealing temperature is 450-600° C., and the annealing time is 3-10 h.

7. The preparation method according to claim 3, characterized in that: In the step 4, the amorphous crystallization method is thermal crystallization, the crystallization temperature is 650-900°C, and the crystallization time is 1-24h; the post-treatment includes grinding with 180 mesh, 400 mesh, 800 mesh, 1000 mesh, 1500 mesh and 2000 mesh sandpaper respectively, and then polishing with polishing powder, washing and drying.

8. An LED light source, characterized in that: The LED light source comprises a fluorescent conversion layer and an LED semiconductor chip or a laser light source, and the fluorescent conversion layer is mounted on the LED semiconductor chip or the laser light source; wherein the fluorescent conversion layer comprises at least one near-infrared fluorescent glass ceramic material as described in any one of claims 1 or 2; the LED semiconductor chip is selected from at least one of a blue light LED chip and a red light LED chip, and the laser light source is at least one of a blue light laser or a red light laser.

9. The use of the LED light source according to claim 8 is used in the fields of biometrics, sensing, food testing, medical testing, agricultural production or biological imaging.

Citation Information

Patent Citations

  • Novel nir broadband emitting phosphors for infrared spectroscopy

    CN113811590A

  • Near-infrared luminescent material, preparation method thereof and LED light source containing luminescent material

    CN116200194A

  • Oxide near-infrared luminescent glass ceramic and preparation method thereof

    CN116715441A

  • Near-infrared luminescent material, preparation method thereof and LED light source containing near-infrared luminescent material

    CN116751588A

  • Full-spectrum fluorescent ceramic with high color rendering index and preparation method thereof