Preparation method of hydrophobic broadband antireflection coating

The moth-eye nanostructured hydrophobic broadband anti-reflective coating is formed through an induced chemical vapor deposition process, which solves the problems of high cost and limited application of broadband anti-reflective coatings in the existing technology, and achieves full-spectrum transmission and hydrophobic automatic coating. The combination of cleaning properties is suitable for a variety of optoelectronic devices.

CN118851589APending Publication Date: 2024-10-29INST OF SEMICONDUCTORS - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310480898.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

When manufacturing broadband anti-reflective coatings in the existing technology, the physical vapor deposition method is costly and the size of the device substrate is limited. The sol-gel method is difficult to match the optical and thermal expansion characteristics, which limits its application scope.

Method used

Using an initiated chemical vapor deposition process, the gas group of the initiator, the first monomer and the second monomer reacts in the deposition chamber to form a hydrophobic broadband anti-reflective coating with a moth-eye nanostructure, combined with organic adhesive Coated to enhance hydrophobicity and anti-reflective properties.

Benefits of technology

It achieves the enhancement of full-spectrum transmission in the range of 190 to 2500nm, and also has hydrophobic self-cleaning properties, reducing light reflectivity, and is suitable for a wider range of optoelectronic device applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851589A_ABST
    Figure CN118851589A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a hydrophobic broadband antireflection coating. The preparation method comprises the following steps: placing a substrate in a deposition chamber with a heating device; based on an initiation type chemical vapor deposition technology, a first gas group comprising an initiator, a first monomer and a second monomer is introduced into a deposition chamber, free radicals generated by thermal decomposition of the initiator, the first monomer and the second monomer are diffused and adsorbed on the surface of a substrate in the deposition chamber, and the flow ratio of the first gas group and the pressure intensity of the deposition chamber are regulated and controlled; the first monomer is used as a cross-linking agent to enable the first monomer to be subjected to a first free radical polymerization reaction, the second monomer is used as a cross-linking agent to enable the first free radical polymerization reaction to tend to side chain crystallization, and the hydrophobic broadband antireflection coating with the moth-eye nanostructure is formed on the surface of the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of functionalized coating on the surface of materials and devices, and in particular relates to a method for preparing a hydrophobic broadband anti-reflection coating. Background Art

[0002] Generally, the light reflectivity of the glass surface when in contact with the air is about 4-5%. For the glass-air interface, the light energy loss caused by reflection is close to 8-10%. For this reason, in various optical and optoelectronic devices (such as optical lenses, displays, solar panels, optical filters, anti-glare glass surfaces, etc.), attempts to use anti-reflection coatings (ARC) that reduce substrate light reflection can effectively reduce the reflected light on the device substrate surface, thereby reducing light energy loss and glare effects, and improving the image quality and efficiency of optical and optoelectronic devices.

[0003] In the related art, the anti-reflection coating that can enhance visible light and near-infrared light in the wavelength range of 400 to 2500nm is called broadband ARC. The common method of manufacturing broadband ARC is mainly to adjust the thickness and refractive index of the multilayer film by physical vapor deposition or sol-gel method, resulting in a decrease in the reflectivity of destructive interference, making the multilayer ARC effective in a wide wavelength range. However, multilayer ARC technology is often used in small optical devices, such as optical lenses, and has great device limitations. In addition, physical vapor deposition technology is relatively expensive and the size of the device substrate is limited; the sol-gel method is limited by problems such as selecting suitable materials to match optical and thermal expansion properties, and it is difficult to promote the technology to a wider range of applications. Summary of the invention

[0004] In view of this, in order to solve at least one of the technical problems mentioned above and in other aspects in the related art, the present disclosure proposes a method for preparing a hydrophobic broadband anti-reflection coating. Through an initiated chemical vapor deposition (iCVD) process, a coating is obtained that is used in optoelectronic devices to enhance the full spectrum transmittance of ultraviolet-visible-near infrared and has hydrophobic self-cleaning properties.

[0005] In one aspect of the present disclosure, a method for preparing a hydrophobic broadband anti-reflection coating is proposed, comprising: placing a substrate in a deposition chamber with a heating device; based on an initiated chemical vapor deposition technique, introducing a first gas group including an initiator, a first monomer and a second monomer into the deposition chamber, wherein free radicals generated by thermal decomposition of the initiator and the first monomer and the second monomer diffuse in the deposition chamber and adsorb on the surface of the substrate, and regulating the flow ratio of the first gas group and the pressure of the deposition chamber to cause a first free radical polymerization reaction to occur in the first monomer, wherein the second monomer serves as a cross-linking agent to cause the first free radical polymerization reaction to tend to side chain crystallization, and a hydrophobic broadband anti-reflection coating having a moth-eye nanostructure is formed on the surface of the substrate.

[0006] According to an embodiment of the present disclosure, the moth-eye nanostructure has a plurality of protrusions whose size is smaller than the wavelength of light to weaken the reflection ability of the hydrophobic broadband anti-reflection coating, and the water contact angle of the moth-eye nanostructure is greater than 90°.

[0007] According to an embodiment of the present disclosure, the method for preparing the above-mentioned hydrophobic broadband anti-reflection coating further includes: before the first gas group is introduced into the deposition chamber, based on the initiated chemical vapor deposition technology, a second gas group including an initiator and a second monomer is introduced into the deposition chamber, and the free radicals generated by the thermal decomposition of the initiator and the second monomer diffuse and adsorb on the surface of the substrate in the chamber and undergo a second free radical polymerization reaction, thereby forming an organic adhesive coating on the surface of the substrate; wherein the organic adhesive coating is combined with the hydrophobic broadband anti-reflection coating to promote the growth of the circular protrusions of the moth-eye nanostructure so that the water contact angle of the moth-eye nanostructure is greater than 150°.

[0008] According to the embodiment of the present disclosure, the bottom diameter of the protrusions ranges from 30 nm to 3 μm, the protrusion height ranges from 50 nm to 5 μm, and the spacing between adjacent protrusions ranges from 0 to 150 nm.

[0009] According to an embodiment of the present disclosure, before the substrate is placed in a deposition chamber with a heating device, the substrate is cleaned and surface activated to enhance the adhesion ability of the hydrophobic broadband anti-reflection coating or the organic adhesive coating.

[0010] According to the embodiment of the present disclosure, the temperature range of the heating device of the deposition chamber is 150-400°C; the working pressure of the deposition chamber for the induced chemical vapor deposition reaction is 100-600mTorr; and the temperature range of the substrate is 15-75°C.

[0011] According to an embodiment of the present disclosure, in the operation of preparing a hydrophobic broadband anti-reflective coating, the flow ratio of the initiator to the first monomer is 1:0.5 to 1:5; the flow ratio of the first monomer to the second monomer is 1:1 to 15:1.

[0012] According to an embodiment of the present disclosure, in the operation of preparing the organic adhesive coating, the flow ratio of the initiator to the second monomer is 0.5:1 to 10:1.

[0013] According to the embodiment of the present disclosure, the initiator includes one of benzoyl peroxide, propylbenzene hydroperoxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, diisopropylbenzene peroxide, and di-tert-amyl peroxide, and the gas flow rate of the initiator is 0.3 to 10 sccm; the first monomer includes one of pentafluorophenyl methacrylate, hexafluoropropylene oxide, perfluoroacrylate, 2-(perfluorooctyl)ethyl methacrylate, 2-(perfluorohexyl)acrylate, 2-(perfluorohexyl)ethyl acrylate, and 1H,1H,2H,2H-perfluorodecyl acrylate; the second monomer includes hydroxyethyl methacrylate, diethylene glycol divinyl ether, 1-vinyl-2-pyrrolidone, 2-(dimethylamino)ethyl methacrylate, and diethylene glycol diacrylate. One of alcohol ester, ethylene glycol dimethacrylate, furfuryl methacrylate, hydroxypropyl methacrylate, cyclohexyl methacrylate, propargyl methacrylate, glycidyl methacrylate, 2,4,6-trimethyl-2,4,6-trivinylcyclotrisiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, 1,3,5-trivinyl-1,3,5-trimethylcyclotrisilazane and 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasilazane; preferably, the substrate comprises glass, silicon wafer, silicon oxide wafer, ceramic, metal sheet, quartz, mica, polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, acrylic plate, cloth.

[0014] According to the embodiments of the present disclosure, the thickness of the hydrophobic broadband anti-reflection coating ranges from 0.01 to 5 μm; the thickness of the organic adhesive coating ranges from 2 to 200 nm.

[0015] According to the embodiment of the present disclosure, the present disclosure proposes a method for preparing a hydrophobic broadband anti-reflection coating. The hydrophobic broadband anti-reflection coating having a moth-eye nanostructure is obtained by initiating free radical polymerization to generate an initiated chemical vapor deposition reaction. The conditions of the preparation method are mild, and the morphology of the moth-eye nanostructure is adjusted by adjusting the flow ratio of the reactants and the coating thickness, so that the hydrophobic broadband anti-reflection coating has both hydrophobic self-cleaning properties and reduced full-spectrum light reflectivity in the range of 190 to 2500 nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is an operation flow chart of a method for preparing a hydrophobic broadband anti-reflection coating according to an embodiment of the present disclosure;

[0017] Figure 2 Schematic diagram of the operation process of the method for preparing the super-hydrophobic broadband anti-reflection coating according to an embodiment of the present disclosure;

[0018] Figure 3 is a schematic diagram of an iCVD system in the present disclosure;

[0019] Figure 4 is a scanning electron microscope image of an uncoated sample of an embodiment of the present disclosure;

[0020] Figure 5 is a scanning electron microscope image of a super-hydrophobic broadband anti-reflection coating prepared in an embodiment of the present disclosure;

[0021] Figure 6 is a scanning electron microscope image of a hydrophobic broadband anti-reflection coating prepared in an embodiment of the present disclosure;

[0022] Figure 7 This is a photograph of the water contact angle of an uncoated sample according to an embodiment of the present disclosure;

[0023] Figure 8 This is a photograph of the water contact angle of a super-hydrophobic broadband anti-reflection coating prepared in one embodiment of the present disclosure;

[0024] Fig. 9 is a photograph of the water contact angle of a hydrophobic broadband anti-reflection coating prepared in another embodiment of the present disclosure;

[0025] Fig.10 is a comparison chart of transmittance curves of an uncoated sample and a super-hydrophobic broadband anti-reflection coating according to an embodiment of the present disclosure;

[0026] Fig.11 is a comparison chart of reflectivity curves of an uncoated sample and a super-hydrophobic broadband anti-reflection coating according to an embodiment of the present disclosure;

[0027] Fig.12 It is a comparison chart of the transmittance curves of an uncoated sample and a hydrophobic broadband anti-reflection coating according to another embodiment of the present disclosure. DETAILED DESCRIPTION

[0028] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0029] The endpoints and any values ​​of the ranges disclosed in this disclosure are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this disclosure.

[0030] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.

[0031] All terms (including technical and scientific terms) used herein have the meanings commonly understood by those skilled in the art, unless otherwise defined. It should be noted that the terms used herein should be interpreted as having a meaning consistent with the context of this specification, and should not be interpreted in an idealized or overly rigid manner.

[0032] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present disclosure shall have the usual meanings understood by persons with ordinary skills in the field to which the present disclosure belongs. If the full text involves descriptions such as "first", "second", etc., the descriptions such as "first", "second", etc. are only used to distinguish similar objects, and cannot be understood as indicating or implying their relative importance, order of precedence, or implicitly indicating the number of technical features indicated. It should be understood that the data described by "first", "second", etc. can be interchangeable under appropriate circumstances.

[0033] In the present disclosure, the technical term "moth-eye nanostructure" is a microstructure composed of sub-wavelength structures. When the surface micro-nanostructure scale of the moth-eye nanostructure is smaller than the wavelength of light, the light wave is confined by the micro-nanostructure with a certain depth and size, trapped in the gap of the moth-eye structure and undergoes multiple internal reflections, thereby reducing the reflected light to a minimum level and enhancing the transmitted light. At the same time, the moth-eye nanostructure is mainly formed by the polymerization of the first monomer with low surface energy, coupled with the self-organized micro-nano protrusion structure, so it exhibits super-hydrophobic self-cleaning properties. Based on this, the present disclosure proposes a method for preparing a full-spectrum broadband anti-reflection coating with a moth-eye-shaped structure in the range of 190 to 2500nm.

[0034] Figure 1 It is an operational flow chart of a method for preparing a hydrophobic broadband anti-reflection coating according to an embodiment of the present disclosure.

[0035] Figure 3 Schematic diagram of the iCVD system in the present disclosure, wherein MFC is a mass flow controller (MFC), which is used to accurately control the flow and ratio of monomers and initiators.

[0036] In one aspect of the present disclosure, a method for preparing a hydrophobic broadband anti-reflection coating is provided, such as Figure 1 , Figure 3 As shown, including:

[0037] S1: placing the substrate in a deposition chamber with a heating device;

[0038] S2: Based on the initiated chemical vapor deposition technology, a first gas group including an initiator, a first monomer and a second monomer is introduced into a deposition chamber, and free radicals generated by thermal decomposition of the initiator and the first monomer and the second monomer diffuse and adsorb on the surface of the substrate in the deposition chamber, and the flow ratio of the first gas group and the pressure of the deposition chamber are regulated to cause a first free radical polymerization reaction of the first monomer, wherein the second monomer acts as a cross-linking agent to make the first free radical polymerization reaction tend to side chain crystallization, thereby forming a hydrophobic broadband anti-reflection coating with a moth-eye nanostructure on the surface of the substrate.

[0039] According to the embodiment of the present disclosure, the preparation method proposed in the present disclosure realizes the preparation of moth-eye nanostructures on the surface of hydrophobic broadband anti-reflective coatings through the preferential orientation and anisotropic growth principle of the first gas group. Specifically, when the flow rate of the first monomer is supersaturated (the partial pressure in the chamber exceeds its saturated vapor pressure), the first monomer molecules adsorbed on the substrate are transformed from gaseous to liquid droplets. The second monomer as a cross-linking agent is conducive to the crystallization of the side chains of the polymer, and when the competition between the crystallization of the polymer side chains and the propagation of the polymer main chain (the first monomer forms a polymer chain as the polymer main chain) is dominant, the free radical polymerization reaction occurring on the substrate tends to generate moth-eye nanostructures. The spacing and size of the moth-eye nanostructure can be controlled by controlling the deposition time. Generally, as the deposition time increases, the protrusion spacing of the moth-eye nanostructure becomes smaller and the size becomes larger. Among them, the first gas group can also be set to an initiator and a first monomer. Because there is no second monomer as a cross-linking agent, the protrusions of the moth-eye nanostructure are difficult to grow and the spacing is large.

[0040] According to the embodiment of the present disclosure, a method for preparing a hydrophobic broadband anti-reflection coating is proposed. The steam of the initiator and the reaction monomer is mixed in proportion and then enters the chamber, and the driving force for monomer polymerization is provided by using the gradient change of the flow field and the temperature field, and a free radical polymerization reaction is initiated to obtain a hydrophobic broadband anti-reflection coating with a moth-eye nanostructure. The conditions of the preparation method are mild, and the morphology of the moth-eye nanostructure is adjusted by adjusting the flow ratio of the reactants and the coating thickness, so that the hydrophobic broadband anti-reflection coating has both hydrophobic self-cleaning properties and weakens the full spectrum light reflectivity in the range of 190 to 2500nm. Furthermore, based on the multi-element co-deposition process, uniform deposition and gradient cross-linking of multiple coatings are achieved, supersaturated monomers nucleate and grow on the surface of the substrate, and the spacing and size of the surface moth-eye structure are controlled by precisely controlling the substrate temperature and deposition time, thereby achieving the hydrophobic and broadband anti-reflection properties of the coating at the same time.

[0041] According to an embodiment of the present disclosure, the moth-eye nanostructure has a plurality of protrusions whose size is smaller than the wavelength of light to weaken the reflection ability of the hydrophobic broadband anti-reflection coating, and the water contact angle of the moth-eye nanostructure is greater than 90°.

[0042] Figure 2It is a schematic diagram of the operating process of the method for preparing a super-hydrophobic broadband anti-reflection coating according to an embodiment of the present disclosure.

[0043] According to the embodiment of the present disclosure, Figure 2 , Figure 3 As shown, the preparation method of the above-mentioned hydrophobic broadband anti-reflection coating also includes: before the first gas group is introduced into the deposition chamber, based on the initiated chemical vapor deposition technology, a second gas group including an initiator and a second monomer is introduced into the deposition chamber, and the free radicals generated by the thermal decomposition of the initiator and the second monomer diffuse and adsorb on the surface of the substrate in the chamber and undergo a second free radical polymerization reaction to form an organic adhesive coating on the surface of the substrate; wherein the organic adhesive coating is combined with the hydrophobic broadband anti-reflection coating to promote the growth of the circular protrusions of the moth-eye nanostructure so that the water contact angle of the moth-eye nanostructure is greater than 150°.

[0044] According to the disclosed embodiment, an organic adhesive coating is added to the deposited hydrophobic broadband anti-reflection coating, which can be combined with the hydrophobic broadband anti-reflection coating to guide the moth-eye structure to grow in the longitudinal direction, causing the circular protrusions of the moth-eye nanostructure to grow in the longitudinal direction and reduce the structural spacing, so that the hydrophobic broadband anti-reflection coating reaches super-hydrophobicity, but the organic adhesive coating will slightly reduce the anti-reflection performance while increasing the hydrophobicity. When the surface micro-nanostructure scale of the moth-eye nanostructure is smaller than the wavelength of light, the light wave is confined by the micro-nanostructure with a certain depth and size, trapped in the gap between the moth-eye protrusion structures and undergoes multiple internal reflections, thereby reducing the reflected light to the minimum level and enhancing the transmitted light. At the same time, the moth-eye nanostructure is mainly formed by the polymerization of the first monomer with low surface energy, coupled with the self-organized micro-nano protrusion structure, so it exhibits super-hydrophobic self-cleaning properties.

[0045] According to the embodiments of the present disclosure, the preparation method proposed in the present disclosure does not involve any solvent throughout the process, will not cause destructive effects on the substrate, has mild reaction conditions, is fully automated, and is simple and efficient.

[0046] According to an embodiment of the present disclosure, in the operation of preparing a hydrophobic broadband anti-reflective coating, the flow ratio of the initiator to the first monomer is 1:0.5 to 1:5; the flow ratio of the first monomer to the second monomer is 1:1 to 15:1.

[0047] According to an embodiment of the present disclosure, in the operation of preparing the organic adhesive coating, the flow ratio of the initiator to the second monomer is 0.5:1 to 10:1.

[0048] According to the embodiment of the present disclosure, the bottom diameter of the protrusions ranges from 30 nm to 3 μm, the protrusion height ranges from 50 nm to 5 μm, and the spacing between adjacent protrusions ranges from 0 to 150 nm.

[0049] According to the embodiments of the present disclosure, the moth-eye nanostructure can be effectively controlled by adjusting the flow ratio and flow rate of the reaction gas group. The inventor has verified through a large number of experiments that the preparation method proposed in the present disclosure realizes the moth-eye nanostructure within the above-mentioned morphology. At the same time, this moth-eye nanostructure has excellent broadband anti-reflection and anti-transmittance and hydrophobic properties.

[0050] According to an embodiment of the present disclosure, before the substrate is placed in a deposition chamber with a heating device, the substrate is cleaned and surface activated to enhance the adhesion ability of the hydrophobic broadband anti-reflection coating or the organic adhesive coating.

[0051] According to the embodiment of the present disclosure, the temperature range of the heating device of the deposition chamber is 150-400°C; the working pressure of the deposition chamber for the induced chemical vapor deposition reaction is 100-600mTorr; and the temperature range of the substrate is 15-75°C.

[0052] According to the embodiment of the present disclosure, in the deposition chamber, there is a certain temperature gradient between the heating device and the substrate to promote the diffusion of the reaction gas group and the free radicals. Factors affecting the diffusion of the reaction gas group and the free radicals also include concentration gradient and gravity.

[0053] According to the embodiment of the present disclosure, the initiator includes one of benzoyl peroxide, propylbenzene hydroperoxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, diisopropylbenzene peroxide, and di-tert-amyl peroxide, and the gas flow rate of the initiator is 0.3 to 10 sccm; the first monomer includes one of pentafluorophenyl methacrylate, hexafluoropropylene oxide, perfluoroacrylate, 2-(perfluorooctyl)ethyl methacrylate, 2-(perfluorohexyl)acrylate, 2-(perfluorohexyl)ethyl acrylate, and 1H,1H,2H,2H-perfluorodecyl acrylate; the second monomer includes hydroxyethyl methacrylate, diethylene glycol divinyl ether, 1-vinyl-2-pyrrolidone, 2-(dimethylamino)ethyl methacrylate, and diethylene glycol diacrylate. One of alcohol ester, ethylene glycol dimethacrylate, furfuryl methacrylate, hydroxypropyl methacrylate, cyclohexyl methacrylate, propargyl methacrylate, glycidyl methacrylate, 2,4,6-trimethyl-2,4,6-trivinylcyclotrisiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, 1,3,5-trivinyl-1,3,5-trimethylcyclotrisilazane and 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasilazane; preferably, the substrate comprises glass, silicon wafer, silicon oxide wafer, ceramic, metal sheet, quartz, mica, polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, acrylic plate, cloth.

[0054] According to the embodiments of the present disclosure, the hydrophobic broadband anti-reflective coating proposed in the present disclosure can be used in organic light-emitting diodes (OLEDs), organic solar cells (OSCs), perovskite solar cells (PSCs), copper zinc tin sulfur selenium solar cells (Cu2ZnSnS x Se 4– x Functional coating on the surface of optoelectronic devices such as solar cells (CZTSSe), copper indium gallium selenium solar cells (CIGS), printed circuit boards (PCBs), lasers, detectors, filters, glasses, photographic and video lenses, etc.

[0055] According to the embodiments of the present disclosure, the thickness of the hydrophobic broadband anti-reflection coating ranges from 0.01 to 5 μm; the thickness of the organic adhesive coating ranges from 2 to 200 nm.

[0056] According to the embodiments of the present disclosure, the range of substrate selection is wide, a large number of monomers can be selected, and the thickness and function of the film layer can be adjusted according to actual requirements.

[0057] According to the embodiment of the present disclosure, in the preparation method proposed in the present disclosure, the coating thickness is monitored by a laser interferometer thickness measuring device at the top of the deposition chamber, and the device includes a laser and a detector. The laser is incident on the substrate surface through the reserved quartz window in the chamber, and then reflected through the window and received by the detector. The periodic change of the detection light power over time corresponds to the uniform increase of the coating thickness. The excess unreacted gas is pumped out of the chamber by the vacuum pump and condensed in the exhaust gas treatment device. The device is located in the pipeline between the vacuum pump and the chamber, and is condensed by liquid nitrogen to ensure that the entire process is green and pollution-free.

[0058] It should be noted that the described embodiments are only part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the embodiments of the present disclosure, other embodiments obtained by ordinary technicians in the field without creative work are all within the scope of protection of the present disclosure.

[0059] Example 1

[0060] S1: Pre-treat the quartz glass substrate by soaking it in acetone, isopropanol, and ethanol solutions, oscillating it with an ultrasonic cleaner for 20 minutes each, and then drying it with nitrogen. Figure 3The bottom surface of the deposition chamber in the iCVD system shown in the figure uses a mass flow controller (MFC) to precisely measure and control the mass flow of each component. The reaction chamber is evacuated to 0.1 Pa, the chamber pressure is monitored in real time by a vacuum gauge and controlled by a butterfly valve, the mechanical pump of the deposition chamber is in a vacuum state throughout the process, and the temperature of the quartz glass substrate is controlled by water cooling.

[0061] S2: The heating device in the deposition chamber is heated to 300°C, and the second gas group is introduced into the deposition chamber, including tert-butyl hydroperoxide as an initiator and 2,4,6-trimethyl-2,4,6-trivinylcyclotrisiloxane as a second monomer. The substrate temperature is controlled at 20-40°C, the initiator flow rate is 3sccm, the second monomer flow rate is 2sccm, the deposition chamber pressure is 600mTorr, and the film formation rate is 15nm / min.

[0062] Tert-butyl hydroperoxide is thermally decomposed at 300°C to generate free radicals that diffuse in the deposition chamber and undergo free radical polymerization with 2,4,6-trimethyl-2,4,6-trivinylcyclotrisiloxane adsorbed on the surface of the substrate, forming an organic adhesive coating with a thickness of 100 nm on the surface of the substrate.

[0063] S3: When the conditions of the deposition chamber remain unchanged, the first gas group is introduced into the deposition chamber, including tert-butyl hydroperoxide as an initiator (with a flow rate of 3 sccm), 2,4,6-trimethyl-2,4,6-trivinylcyclotrisiloxane as a second monomer (with a flow rate of 0.2 sccm), and hexafluoropropylene oxide as a first monomer (with a flow rate of 2 sccm).

[0064] Tert-butyl hydroperoxide is thermally decomposed at 300°C to generate free radicals that diffuse in the deposition chamber, and acts as an initiator to promote the free radical polymerization reaction of 2,4,6-trimethyl-2,4,6-trivinylcyclotrisiloxane and hexafluoropropylene oxide adsorbed on the surface of the substrate to generate trimethyltrivinylcyclotrisiloxane-co-tetrafluoroethylene cross-linked copolymer, forming a moth-eye nanostructured superhydrophobic broadband anti-reflection coating with a thickness of about 100 nm on the surface of the organic adhesive coating.

[0065] Example 2

[0066] S1: Pre-treat the quartz glass substrate by soaking it in acetone, isopropanol, and ethanol solutions in turn, oscillating it with an ultrasonic cleaner for 20 minutes each, and then drying it with nitrogen. Figure 3 The bottom surface of the deposition chamber in the iCVD system shown in the figure, the reaction chamber is evacuated to 0.1 Pa, the chamber pressure is monitored in real time by a vacuum gauge, the mechanical pump of the deposition chamber is in a pumping state throughout the process, and the temperature of the quartz glass substrate is controlled by water cooling.

[0067] S2: The heating device in the deposition chamber is heated to 200°C, and the first gas group is introduced into the deposition chamber, including di-tert-butyl peroxide as an initiator and 2-(perfluorohexyl) acrylate as a first monomer. The substrate temperature is controlled at 35±0.5°C, the initiator flow rate is 0.6sccm, the first monomer flow rate is 0.5sccm, the deposition chamber pressure is 200mTorr, and the film formation rate is 100nm / min.

[0068] Di-tert-butyl peroxide is thermally decomposed at 200°C to generate free radicals that diffuse in the deposition chamber, initiating a free radical polymerization reaction of 2-(perfluorohexyl) acrylate on the surface of the substrate, forming a hydrophobic broadband anti-reflection coating on the surface of the substrate with a thickness of about 130 nm.

[0069] Test Example 1

[0070] The surface morphologies of the uncoated sample (i.e., quartz glass substrate) and the super-hydrophobic broadband anti-reflection coating and the hydrophobic broadband anti-reflection coating prepared in Examples 1 and 2 of the present disclosure were observed using a scanning electron microscope.

[0071] The static water contact angle (WCA) and rolling angle (WSA) were tested using a contact angle meter. The test water drop volume was 5 μL to 20 μL. The basis for judging superhydrophobicity was WCA ≥ 150° and WSA ≤ 10°.

[0072] Figure 4 is a scanning electron microscope image of an uncoated sample of an embodiment of the present disclosure.

[0073] Figure 5 3 is a scanning electron microscope image of the super-hydrophobic broadband anti-reflection coating prepared in the embodiment of the present disclosure.

[0074] Figure 6 3 is a scanning electron microscope image of the hydrophobic broadband anti-reflection coating prepared in the embodiment of the present disclosure.

[0075] like Figure 4 As shown, the surface of the uncoated sample is smooth and flat.

[0076] like Figure 5 As shown, the surface of the super-hydrophobic broadband anti-reflection coating prepared in Example 1 of the present disclosure shows an obvious rough moth-eye nanostructure, wherein the protrusions in the moth-eye nanostructure are coarse and closely connected.

[0077] like Figure 6As shown, the surface of the hydrophobic broadband anti-reflection coating prepared in Example 2 of the present disclosure cannot form a cross-linked polymer because there is no second monomer as a cross-linking agent. At the same time, because there is no second monomer to crystallize the second monomer side chain to make the moth-eye structure grow in the longitudinal direction, the moth-eye nanostructure is smaller in size and larger in spacing.

[0078] Test Example 2

[0079] The static water contact angle (WCA) and rolling angle (WSA) of the uncoated sample (i.e., quartz glass substrate), the super-hydrophobic broadband anti-reflection coating prepared in Examples 1 and 2 of the present disclosure, and the hydrophobic broadband anti-reflection coating were tested using a contact angle meter, wherein the test water drop volume was 5 μL to 20 μL, the super-hydrophobicity was judged as WCA ≥ 150° and WSA ≤ 10°, the hydrophilic surface was judged as WCA < 90°, and the hydrophobic surface was judged as WCA > 90°.

[0080] Figure 7 This is a photograph of the water contact angle of an uncoated sample of an embodiment of the present disclosure.

[0081] Figure 8 This is a photograph of the water contact angle of a super-hydrophobic broadband anti-reflection coating prepared in an embodiment of the present disclosure.

[0082] Fig. 9 This is a photograph of the water contact angle of a hydrophobic broadband anti-reflection coating prepared in another embodiment of the present disclosure.

[0083] like Figure 7 As shown, the static water contact angle of the surface of the uncoated sample is 29.6°, which is less than 90°, and is a hydrophilic surface.

[0084] like Figure 8 As shown, the static water contact angle of the super-hydrophobic broadband anti-reflection coating prepared in Example 1 of the present disclosure reaches 161.6°, which is greater than 150°, and the rolling angle is about 5°, which is less than 10°. It is a super-hydrophobic surface, and water droplets can roll freely on its surface.

[0085] like Fig. 9 As shown, the static water contact angle of the super-hydrophobic broadband anti-reflection coating prepared in Example 1 of the present disclosure is 111.8°, which is greater than 90° but less than 150°. It is a hydrophobic surface, but it does not reach super-hydrophobicity.

[0086] Test Example 3

[0087] The transmittance and reflectivity of the uncoated sample (i.e., quartz glass substrate), the super-hydrophobic broadband anti-reflection coating prepared in Examples 1 and 2 of the present disclosure, and the hydrophobic broadband anti-reflection coating were tested using a UV-visible-near-infrared spectrophotometer, wherein the scanning range is 190 to 2500 nm, the visible light region refers to 390 nm to 780 nm, and broadband anti-reflection refers to achieving full-spectrum transmission enhancement within the range of 190-2500 nm.

[0088] Fig.10 It is a comparison chart of the transmittance curves of an uncoated sample and a super-hydrophobic broadband anti-reflection coating according to an embodiment of the present disclosure.

[0089] Fig.11 It is a comparison chart of reflectivity curves of an uncoated sample and a super-hydrophobic broadband anti-reflection coating according to an embodiment of the present disclosure.

[0090] like Fig.10 As shown, in the visible-near infrared light range of 390-2500nm, the average transmittance of the uncoated sample and the super-hydrophobic broadband anti-reflection coating in Example 1 of the present disclosure are 93.43% and 95.06%, respectively, and the average transmittance of the ARC sample is increased by 1.63%.

[0091] like Fig.11 As shown, compared with the uncoated sample, the reflectivity of the superhydrophobic broadband anti-reflection coating in Example 1 of the present disclosure is significantly reduced, indicating that the surface rough moth-eye nanostructure reduces surface reflection and improves transmittance.

[0092] Fig.12 It is a comparison chart of the transmittance curves of an uncoated sample and a hydrophobic broadband anti-reflection coating according to another embodiment of the present disclosure.

[0093] like Fig.12 As shown, in the ultraviolet-visible-near infrared spectral range of 190-2500nm, the average transmittances of the uncoated sample and the hydrophobic broadband anti-reflection coating prepared in Example 2 of the present disclosure are 93.31% and 94.54%, respectively. The transmittance of the hydrophobic broadband anti-reflection coating prepared in Example 2 of the present disclosure is enhanced in the full spectral range.

[0094] By comparison, it can be seen that in Example 2, only a hydrophobic broadband anti-reflection coating is deposited to form a moth-eye nanostructure in one step. Although it does not achieve super-hydrophobicity, its broadband anti-reflection effect is very obvious and can be used in application scenarios that focus on increasing transmittance and reducing reflection.

[0095] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.

Claims

1. A method for preparing a hydrophobic broadband anti-reflection coating, comprising: placing the substrate in a deposition chamber with a heating device; Based on the initiated chemical vapor deposition technology, a first gas group including an initiator, a first monomer and a second monomer is introduced into the deposition chamber, and the free radicals generated by the thermal decomposition of the initiator and the first monomer and the second monomer are diffused and adsorbed on the surface of the substrate in the deposition chamber, and the flow ratio of the first gas group and the pressure of the deposition chamber are regulated to cause the first monomer to undergo a first free radical polymerization reaction, wherein the second monomer serves as a cross-linking agent to cause the first free radical polymerization reaction to tend to side chain crystallization, thereby forming a hydrophobic broadband anti-reflection coating with a moth-eye nanostructure on the surface of the substrate.

2. The preparation method according to claim 1, wherein The moth-eye nanostructure has a plurality of protrusions whose size is smaller than the wavelength of light to weaken the reflection ability of the hydrophobic broadband anti-reflection coating, and the water contact angle of the moth-eye nanostructure is greater than 90°.

3. The preparation method according to claim 1, further comprising: Before the first gas group is introduced into the deposition chamber, a second gas group including an initiator and a second monomer is introduced into the deposition chamber based on an initiated chemical vapor deposition technique, and the free radicals generated by the thermal decomposition of the initiator and the second monomer diffuse and adsorb on the surface of the substrate in the chamber and undergo a second free radical polymerization reaction, thereby forming an organic adhesive coating on the surface of the substrate; wherein, The organic adhesive coating is combined with the hydrophobic broadband anti-reflection coating to promote the growth of the circular protrusions of the moth-eye nanostructure so that the water contact angle of the moth-eye nanostructure is greater than 150°.

4. The preparation method according to any one of claims 1 to 3, wherein: The bottom diameter of the protrusions ranges from 30 nm to 3 μm, the protrusion height ranges from 50 nm to 5 μm, and the spacing between adjacent protrusions ranges from 0 to 150 nm.

5. The preparation method according to any one of claims 1 to 3, wherein: Before the substrate is placed in a deposition chamber with a heating device, the substrate is cleaned and surface activated to enhance the adhesion ability of the hydrophobic broadband anti-reflection coating or the organic adhesive coating.

6. The preparation method according to any one of claims 1 to 3, wherein: The temperature range of the deposition chamber heating device is 150-400°C; The working pressure of the deposition chamber for the induced chemical vapor deposition reaction is 100-600 mTorr; The temperature of the substrate is in the range of 15 to 75°C.

7. The preparation method according to any one of claims 1 to 3, wherein: In the process of preparing the hydrophobic broadband anti-reflection coating, the flow ratio of the initiator to the first monomer is 1:0.5 to 1:5; the flow ratio of the first monomer to the second monomer is 1:1 to 15:

1.

8. The preparation method according to claim 2, wherein: In the process of preparing the organic adhesive coating, the flow ratio of the initiator to the second monomer is 0.5:1 to 10:

1.

9. The preparation method according to claim 1 or 2, wherein: The initiator includes one of benzoyl peroxide, propylbenzene hydroperoxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, diisopropylbenzene peroxide, and di-tert-amyl peroxide, and the gas flow rate of the initiator is 0.3 to 10 sccm; The first monomer includes one of pentafluorophenyl methacrylate, hexafluoropropylene oxide, perfluoroacrylate, 2-(perfluorooctyl)ethyl methacrylate, 2-(perfluorohexyl)acrylate, 2-(perfluorohexyl)ethyl acrylate, and 1H,1H,2H,2H-perfluorodecyl acrylate; The second monomer comprises one of hydroxyethyl methacrylate, diethylene glycol divinyl ether, 1-vinyl-2-pyrrolidone, 2-(dimethylamino)ethyl methacrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, furfuryl methacrylate, hydroxypropyl methacrylate, cyclohexyl methacrylate, propargyl methacrylate, glycidyl methacrylate, 2,4,6-trimethyl-2,4,6-trivinylcyclotrisiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, 1,3,5-trivinyl-1,3,5-trimethylcyclotrisilazane and 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasilazane; Preferably, the substrate comprises glass, silicon wafer, silicon oxide wafer, ceramic, metal sheet, quartz, mica, polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, acrylic plate, cloth.