High-strength anti-cracking concrete for wet joints and its preparation process

By optimizing material ratio and using modified fibers and other technical means, high-strength anti-cracking concrete was prepared, which solved the problem of cracking in wet joints, significantly improved the crack resistance and durability of the bridge, and satisfies the bridge's high strength and High resilience demand.

CN118851676BActive Publication Date: 2024-12-06ANHUI WATER CONSERVANCY DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411320235.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-06
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

In simple support and then continuous bridges, wet joints are susceptible to factors such as temperature and load, which lead to cracks and affect the load-bearing capacity and durability of the bridge. Especially in large spans and multi-span bridges, cracking problems are prominent, and high-strength needs to be developed Anti-cracking concrete material to improve the performance and durability of wet joints.

Method used

By optimizing the material ratio, reinforcing fibers composed of modified carbon fibers, surface modified ultra-high molecular weight polyethylene fibers and nylon fibers are used to combine nanosilicon dioxide and tannin acid, and polycarboxylic acid-based water reducing agents and triethanolamine. Prepare high-strength anti-cracking concrete to enhance its crack resistance and durability.

Benefits of technology

It significantly improves the crack resistance and durability of concrete, meets the requirements of wet joints for bearing capacity, impact resistance, seepage resistance and crack resistance, and achieves dual improvements of high strength and high toughness, ensuring the safety and service life of the bridge. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses high-strength anti-cracking concrete for wet joints and a preparation process thereof, and belongs to the technical field of building materials. The high-strength anti-cracking concrete for wet joints comprises the following raw materials in parts by weight: 150-180 parts of water, 400-480 parts of cement, 960-1080 parts of coarse aggregate, 600-750 parts of fine aggregate, 50-80 parts of silica fume, 50-100 parts of fly ash, 25-45 parts of limestone, 5-12 parts of water reducer, 35-58 parts of reinforcing fiber, 10-25 parts of nano-silicon dioxide, 1.5-4.5 parts of triethanolamine, and 0.4-2.4 parts of tannic acid. The present invention not only achieves a dual improvement of high strength and high toughness by optimizing the material ratio, but also significantly improves the crack resistance of concrete, and can meet the requirements of wet joints for cement concrete bearing capacity, impact resistance, impermeability, and crack resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to high-strength anti-cracking concrete for wet joints and a preparation process thereof. Background Art

[0002] With the rapid development of modern transportation infrastructure construction, bridges, as important structures connecting different regions and roads, have become the focus of attention for their safety and durability. Among the many bridge structures, the simple-supported-first-continuous-bridge system is widely used due to its unique construction advantages. Based on prefabricated simply-supported beams, this structural system connects the simply-supported beams of adjacent spans into continuous beams through wet joints, thereby improving the overall stiffness and driving comfort of the bridge. However, as a key part of this structural system, the performance and durability of wet joints are directly related to the service life and safety of the entire bridge.

[0003] In bridges that are simply supported first and then continuous, wet joints are often affected by various factors such as temperature, load, creep, etc., and cracks are prone to occur. These cracks not only affect the aesthetics of the bridge, but more importantly, they reduce the bridge's bearing capacity and durability, and increase the subsequent maintenance costs. Especially in large-span and multi-span bridges, the cracking problem of wet joints is particularly prominent. Therefore, the development of a new type of high-strength anti-cracking concrete material is of great significance to improving the performance and durability of wet joints in simply supported and then continuous bridges. Summary of the invention

[0004] Based on the problems existing in the background technology, the present invention provides a high-strength anti-cracking concrete for wet joints and a preparation process thereof. By optimizing the material ratio, not only the dual improvement of high strength and high toughness is achieved, but also the crack resistance of concrete is significantly improved, which can meet the requirements of wet joints for the bearing capacity, impact resistance, impermeability and crack resistance of cement concrete.

[0005] The present invention is implemented by the following technical solutions:

[0006] On the one hand, the present invention provides a high-strength anti-cracking concrete for wet joints, which comprises the following raw materials in parts by weight: 150-180 parts of water, 400-480 parts of cement, 960-1080 parts of coarse aggregate, 600-750 parts of fine aggregate, 50-80 parts of silica fume, 50-100 parts of fly ash, 25-45 parts of limestone, 5-12 parts of water reducing agent, 35-58 parts of reinforcing fiber, 10-25 parts of nano silicon dioxide, 1.5-4.5 parts of triethanolamine and 0.4-2.4 parts of tannic acid.

[0007] Furthermore, the coarse aggregate is crushed stone with a particle size of 5-20 mm and continuous grading.

[0008] Furthermore, the fine aggregate is composed of medium-coarse sand and fine sand, the fineness modulus of the medium-coarse sand is 2.6-2.8, and the fineness modulus of the fine sand is 2.2-2.5; wherein, in terms of mass fraction, the medium-coarse sand is 70-80%, and the fine sand is 20-30%.

[0009] Furthermore, the particle size of silica fume is 100-200nm, and the SiO2 content is ≥96%; the fly ash is Class I fly ash; and the average particle size distribution of limestone is 5-10mm.

[0010] Furthermore, the water reducing agent is a polycarboxylic acid-based water reducing agent, and its water reducing rate is ≥25%.

[0011] Furthermore, the reinforcing fibers are composed of modified carbon fibers, surface-modified ultra-high molecular weight polyethylene fibers and nylon fibers in a mass ratio of 1:(0.4-0.6):(0.4-0.6).

[0012] Among them, according to the proportion of carbon fiber, ultra-high molecular weight polyethylene fiber and nylon fiber, the reinforcing fiber composition data is layered and processed to obtain the data of the reinforced fiber material of the concrete to be tested, including:

[0013] Obtain the mass ratio types of carbon fiber, ultra-high molecular weight polyethylene fiber and nylon fiber from the reinforcing fiber composition data;

[0014] Obtaining the polyethylene fiber and nylon fiber ratio associated with each carbon fiber ratio as a data group to be detected;

[0015] After sorting each data group to be tested according to the carbon fiber ratio, the data corresponding to each fiber composition ratio type is stored in the corresponding data group to be tested, thereby obtaining the reinforcing fiber material data to be tested;

[0016] Obtain concrete uniformity test specification data, and obtain uniformity test standard data from the test specification data;

[0017] After noise elimination processing is performed on the inspection standard data, a data feature vector is constructed, and specification-related data is obtained from the inspection specification data;

[0018] After clustering the data feature vectors according to the standard associated data, a data group to be trained is obtained, and after the initial model is trained with the data group to be trained for uniformity detection, an unsupervised uniformity detection model is obtained;

[0019] The data of the reinforcing fiber materials to be tested are input into the preset unsupervised uniformity detection model one by one to obtain the uniformity detection benchmark of concrete reinforcing fiber, which specifically includes:

[0020] Inputting first data of the reinforcing fiber material to be detected into the unsupervised uniformity detection model, performing similarity matching on the first data to be detected in the unsupervised model, and outputting a first detection result according to the matching result;

[0021] Starting from the second reinforced fiber material data to be tested, the previous test result is input into the unsupervised uniformity test model to obtain the corresponding concrete uniformity test result, and the first test result and all the test results are integrated to obtain the uniformity test benchmark of the concrete reinforced fiber material;

[0022] The uniformity detection data is generated according to the uniformity detection benchmark and the current reinforcing fiber material composition data, and the detection data is input into the unsupervised uniformity detection model to obtain the uniformity detection result data.

[0023] Furthermore, the preparation steps of the modified carbon fiber are specifically as follows: treating the carbon fiber with a nitric acid solution to remove surface impurities, then immersing it in a silane coupling agent and keeping it in a constant temperature water bath for 2-3 hours, and washing the treated carbon fiber with deionized water and drying it; dissolving tetraethyl orthosilicate in ethanol, adding a deionized surfactant, stirring evenly, and continuously adding ammonia water to obtain a modified reaction solution; placing the treated carbon fiber into the modified reaction solution, and reacting it in a constant temperature water bath for 12-24 hours. After the reaction is completed, taking out the reactant and aging it at room temperature for 24 hours, and finally washing the product with deionized water and drying it to obtain the modified carbon fiber.

[0024] Furthermore, the preparation steps of the surface-modified ultra-high molecular weight polyethylene fiber are specifically as follows: washing the ultra-high molecular weight polyethylene fiber with ethanol and drying it; preparing an ethanol / water mixed solution containing a silane coupling agent, adjusting the pH to 4.0-5.5 with acetic acid, and soaking the dried ultra-high molecular weight polyethylene fiber in the ethanol / water mixed solution of the silane coupling agent for 1-2 hours, and drying at 100-120°C for 2-4 hours after soaking to obtain the surface-modified ultra-high molecular weight polyethylene fiber.

[0025] Furthermore, the nylon fiber is nylon 66 fiber.

[0026] Further, the carbon fiber has a length of 5-10 mm, a diameter of 7-10 μm, a tensile strength of 3.5-4.5 GPa, and an elastic modulus of 23-250 GPa;

[0027] The length of ultra-high molecular weight polyethylene fiber is 6-12mm, the diameter is 12-20μm, the tensile strength is 3.0-3.5GPa, and the elastic modulus is 100-120GPa;

[0028] The nylon fiber length is 6-12mm, the diameter is 15-30μm, the tensile strength is 0.8-1.2GPa, and the elastic modulus is 2.5-4.0GPa.

[0029] Another aspect of the present invention further provides a method for preparing the high-strength anti-cracking concrete for wet joints, comprising the following steps:

[0030] (1) Weigh the raw materials according to the ratio;

[0031] (2) Add cement, coarse aggregate, fine aggregate, silica fume, fly ash and limestone into a mixer and perform dry mixing first to ensure that the components are evenly mixed; then add reinforcing fiber and nano-silica to the dry-mixed powder mixture and perform dry mixing again to ensure that the components are evenly distributed to obtain a mixture A;

[0032] (3) dissolving the water reducing agent in water to obtain solution B;

[0033] (4) Mixture A, solution B, triethanolamine and tannic acid and mix them evenly to obtain high-strength anti-cracking concrete for wet joints.

[0034] Wherein, step (4) includes:

[0035] Controlling the mixer device to start a mixing program and outputting an initial temperature detection mark from the initial mixture;

[0036] Determine the current temperature data and temperature change trend obtained by the temperature monitoring device, the temperature change trend includes the initial temperature change trend and the real-time temperature change trend;

[0037] Determine and output a plurality of new temperature detection points, and determine temperature data and a temperature change trend for each new temperature detection point until the number of consecutive new temperature change trends reaches a preset change trend threshold, or the current temperature detection point is determined to be the last detection point;

[0038] Based on a preset temperature change trend threshold, adjusting the stirring rate of the mixer, returning to execute acquiring new temperature data from the initial mixture until the continuous number of new temperature change trends reaches a preset number threshold, or determining that the current temperature detection point is the last detection point;

[0039] Generate a list based on each temperature data and temperature change trend and output it;

[0040] Determining the current temperature data and change trend obtained by the temperature monitoring device includes the following steps:

[0041] Obtain the temperature monitoring data and time of the current mixture batch, where the time is the duration from the output of the current temperature detection point to the acquisition of the temperature data;

[0042] Determine the current temperature change trend based on the temperature data, where the temperature change trend includes the initial temperature change trend and the real-time temperature change trend;

[0043] If the temperature change trend reaches a set threshold, the parameters for adjusting the stirring rate are determined based on the temperature change trend;

[0044] If the temperature change trend does not reach the set threshold, the current adjustment rate is determined to be 0, and the original stirring conditions are kept unchanged.

[0045] Beneficial effects of the present invention:

[0046] The reinforcing fibers in the present invention are composed of modified carbon fibers, surface-modified ultra-high molecular weight polyethylene fibers and nylon fibers. The modified carbon fibers provide strength and stiffness support to prevent the generation of cracks; the surface-modified UHMWPE fibers prevent the expansion of cracks through their high toughness, while the nylon fibers absorb part of the tensile stress in the early stage of crack formation, further preventing the expansion of cracks. This multi-dimensional crack control mechanism significantly improves the overall crack resistance of concrete. Due to the different morphologies and characteristics of different fibers, the composite fibers can be more evenly dispersed in the concrete, reducing the aggregation phenomenon that may occur in a single fiber and ensuring the uniformity of the reinforcement effect. In the present invention, the surface modification of carbon fibers and UHMWPE fibers is also used to enhance their interfacial bonding with the cement matrix, thereby improving the stress transfer efficiency of the fibers, enabling the fibers to more effectively participate in the stress distribution of concrete and improve its long-term performance.

[0047] Tannic acid used in the present invention is a polyphenol compound, contains a large amount of hydroxyl groups, can form strong hydrogen bonds with cement paste, and improve the overall mechanical properties of concrete. The hydroxyl groups in tannic acid form hydrogen bonds with the amide groups in nylon fibers, thereby enhancing the chemical bonding between nylon fibers and cement matrix. Siloxane groups can be introduced into the surface of surface-modified UHMWPE fibers, which can also form hydrogen bonds with the hydroxyl groups in tannic acid, thereby increasing the adhesion of surface-modified UHMWPE fibers to cement matrix. Tannic acid optimizes the interface structure between reinforcing fibers and cement matrix through hydrogen bonding, optimizes the interface transition zone around reinforcing fibers, enables the mechanical properties of fibers in cement matrix to be fully utilized, and enhances the impact resistance and durability of the material.

[0048] The nano silicon dioxide particles in the present invention are fine and can be filled in the micropores of the concrete matrix, significantly improving the compactness of the concrete, reducing the porosity, and then enhancing the impermeability and durability of the concrete. Tannic acid forms a complex with the metal ions in the cement matrix, increasing the crosslinking degree of the matrix, and this crosslinking degree becomes more dense and stable under the filling effect of nano silicon dioxide, thereby improving the toughness and crack resistance of the concrete. Triethanolamine accelerates the hydration reaction of C3A in cement to generate early hydration products, and the presence of nano silicon dioxide further reacts these products to form more CSH, thereby further improving the early strength. Under the action of triethanolamine, the release of hydration heat is controlled, reducing the temperature cracks of large-volume concrete. This effect is combined with the effect of nano silicon dioxide filling the microstructure, significantly improving the crack resistance of the concrete. In addition, the hydration reaction accelerated by triethanolamine and the complexing effect of tannic acid complement each other, the former provides the early strength formed quickly, and the latter increases the crosslinking degree of the cement matrix, making the concrete structure more stable and uniform, and comprehensively improving the mechanical properties of the concrete. The high-strength anti-cracking concrete for wet joints prepared by the reasonable combination and synergistic effect of these components in the present invention can show excellent performance in terms of strength, toughness, crack resistance and durability, and meet the needs of practical applications. DETAILED DESCRIPTION

[0049] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the following embodiments.

[0050] The specifications of the raw materials used in the examples and comparative examples of the present invention are as follows:

[0051] Cement is silicate cement, specification: PO42.5;

[0052] The coarse aggregate is crushed stone with a particle size of 5-20 mm and continuous grading;

[0053] The fine aggregate is composed of medium-coarse sand and fine sand. The fineness modulus of the medium-coarse sand is 2.6-2.8, and the fineness modulus of the fine sand is 2.2-2.5. Among them, in terms of mass fraction, the medium-coarse sand accounts for 73% and the fine sand accounts for 27%;

[0054] Silica fume particle size is 100-200nm, SiO2 content ≥96%;

[0055] The fly ash is Class I fly ash;

[0056] The average particle size distribution of limestone is 5-10mm;

[0057] The water reducer is a polycarboxylic acid water reducer with a water reduction rate of 25% and a solid content of 20±2%;

[0058] The average particle size of nano-silicon dioxide is 30nm and the specific surface area is 295m 2 / g;

[0059] The carbon fiber is 6 mm long, 7 μm in diameter, has a tensile strength of 4.5 GPa, and an elastic modulus of 231 GPa;

[0060] The ultra-high molecular weight polyethylene fiber has a length of 8 mm, a diameter of 13 μm, a tensile strength of 3.2 GPa, and an elastic modulus of 113 GPa;

[0061] The nylon fiber has a length of 7 mm, a diameter of 17 μm, a tensile strength of 0.9 GPa, and an elastic modulus of 3.1 GPa;

[0062] The water is ordinary tap water.

[0063] Example 1

[0064] A method for preparing high-strength anti-cracking concrete for wet joints comprises the following steps:

[0065] (1) Weigh the raw materials according to the proportion: by weight, 160 parts of water, 450 parts of cement, 1038 parts of coarse aggregate, 685 parts of fine aggregate, 64 parts of silica fume, 70 parts of fly ash, 36 parts of limestone, 8 parts of water reducer, 46 parts of reinforcing fiber, 16 parts of nano-silicon dioxide, 2.8 parts of triethanolamine, and 1.7 parts of tannic acid; wherein the reinforcing fiber is composed of modified carbon fiber, surface-modified ultra-high molecular weight polyethylene fiber and nylon fiber in a mass ratio of 1:0.5:0.5;

[0066] (2) Add cement, coarse aggregate, fine aggregate, silica fume, fly ash and limestone into a mixer and perform dry mixing first to ensure that the components are evenly mixed; then add reinforcing fiber and nano-silica to the dry-mixed powder mixture and perform dry mixing again to ensure that the components are evenly distributed to obtain a mixture A;

[0067] (3) dissolving the water reducing agent in water to obtain solution B;

[0068] (4) Mixture A, solution B, triethanolamine and tannic acid and mix them evenly to obtain high-strength anti-cracking concrete for wet joints.

[0069] The specific preparation steps of the modified carbon fiber are as follows: the carbon fiber is treated with a nitric acid solution to remove surface impurities, and then immersed in a 3% mass fraction of a silane coupling agent KH550, and a constant temperature water bath at 70°C for 2-3 hours. The treated carbon fiber is washed with deionized water and dried; tetraethyl orthosilicate is dissolved in ethanol, and the volume ratio of tetraethyl orthosilicate to ethanol is 8:100, and a deionized surfactant hexadecyltrimethylammonium bromide with a solvent mass fraction of 1% is added, and stirred evenly, and ammonia water is continued to be added dropwise, and the volume ratio of ammonia water to tetraethyl orthosilicate is 1:8 to obtain a modified reaction solution; the treated carbon fiber is placed in the modified reaction solution, and reacted in a constant temperature water bath at 45°C for 12-24 hours. After the reaction is completed, the reactant is taken out and aged at room temperature for 24 hours, and finally the product is washed with deionized water and dried to obtain the modified carbon fiber.

[0070] The specific preparation steps of the surface-modified ultra-high molecular weight polyethylene fiber are as follows: the ultra-high molecular weight polyethylene fiber is washed with ethanol and dried; an ethanol / water (volume ratio 2:1) mixed solution containing 3% by mass of silane coupling agent KH550 is prepared, the pH value is adjusted to 4.5 with acetic acid, and the dried ultra-high molecular weight polyethylene fiber is immersed in the ethanol / water mixed solution of the silane coupling agent for 2 hours. After the immersion is completed, the fiber is dried at 120°C for 3 hours to obtain the surface-modified ultra-high molecular weight polyethylene fiber.

[0071] Example 2

[0072] The difference between this embodiment and the embodiment is that the reinforcing fiber is composed of modified carbon fiber, surface modified ultra-high molecular weight polyethylene fiber and nylon fiber in a mass ratio of 1:0.6:0.4.

[0073] Example 3

[0074] The difference between this embodiment and embodiment 1 is that: the raw material ratio is calculated by weight, including 160 parts of water, 450 parts of cement, 1038 parts of coarse aggregate, 685 parts of fine aggregate, 64 parts of silica fume, 70 parts of fly ash, 36 parts of limestone, 8 parts of water reducer, 46 parts of reinforcing fiber, 20 parts of nano silicon dioxide, 3.6 parts of triethanolamine, and 2.0 parts of tannic acid; wherein the reinforcing fiber is composed of modified carbon fiber, surface modified ultra-high molecular weight polyethylene fiber and nylon fiber in a mass ratio of 1:0.5:0.5;

[0075] Comparative Example 1

[0076] The difference between this comparative example and Example 1 is that the reinforcing fiber is modified carbon fiber.

[0077] Comparative Example 2

[0078] The difference between this comparative example and Example 1 is that the reinforcing fiber is composed of modified carbon fiber and surface modified ultra-high molecular weight polyethylene fiber in a mass ratio of 1:0.5.

[0079] Comparative Example 3

[0080] The difference between this comparative example and Example 1 is that the reinforcing fiber is composed of modified carbon fiber and nylon fiber in a mass ratio of 1:0.5.

[0081] Comparative Example 4

[0082] The difference between this comparative example and Example 1 is that the carbon fiber is not modified.

[0083] Comparative Example 5

[0084] The difference between this comparative example and Example 1 is that the ultra-high molecular weight polyethylene fiber is not modified.

[0085] Comparative Example 6

[0086] The difference between this comparative example and Example 1 is that the raw material components do not include nano silicon dioxide.

[0087] Comparative Example 7

[0088] The difference between this comparative example and Example 1 is that triethanolamine is not included in the raw material components.

[0089] Comparative Example 8

[0090] The difference between this comparative example and Example 1 is that tannic acid is not included in the raw material components.

[0091] Example 4

[0092] In one embodiment, according to the carbon fiber ratio, the ultra-high molecular weight polyethylene fiber ratio and the nylon fiber ratio, the reinforcing fiber composition data is layered to obtain the concrete reinforcing fiber material data to be tested, specifically including:

[0093] Obtain the mass ratio types of carbon fiber, ultra-high molecular weight polyethylene fiber and nylon fiber from the reinforcing fiber composition data;

[0094] Obtaining the polyethylene fiber and nylon fiber ratio associated with each carbon fiber ratio as a data group to be detected;

[0095] After sorting each data group to be tested according to the carbon fiber ratio, the data corresponding to each fiber composition ratio type is stored in the corresponding data group to be tested, thereby obtaining the reinforcing fiber material data to be tested;

[0096] Obtain concrete uniformity test specification data, and obtain uniformity test standard data from the test specification data;

[0097] After noise elimination processing is performed on the inspection standard data, a data feature vector is constructed, and specification-related data is obtained from the inspection specification data;

[0098] After clustering the data feature vectors according to the standard associated data, a data group to be trained is obtained, and after the initial model is trained with the data group to be trained for uniformity detection, an unsupervised uniformity detection model is obtained;

[0099] The data of the reinforcing fiber materials to be tested are input into the preset unsupervised uniformity detection model one by one to obtain the uniformity detection benchmark of concrete reinforcing fiber, which specifically includes:

[0100] Inputting first data of the reinforcing fiber material to be detected into the unsupervised uniformity detection model, performing similarity matching on the first data to be detected in the unsupervised model, and outputting a first detection result according to the matching result;

[0101] Starting from the second reinforced fiber material data to be tested, the previous test result is input into the unsupervised uniformity test model to obtain the corresponding concrete uniformity test result, and the first test result and all the test results are integrated to obtain the uniformity test benchmark of the concrete reinforced fiber material;

[0102] The uniformity detection data is generated according to the uniformity detection benchmark and the current reinforcing fiber material composition data, and the detection data is input into the unsupervised uniformity detection model to obtain the uniformity detection result data.

[0103] The principle and beneficial effects of the above scheme are as follows: the mass ratio of carbon fiber, ultra-high molecular weight polyethylene fiber and nylon fiber is extracted from the reinforcing fiber material, and the carbon fiber ratio is classified and sorted, and it is combined with the ratio data of polyethylene fiber and nylon fiber to form a data group to be tested, and finally the reinforcing fiber material data is constructed;

[0104] Extract relevant data from the specification of concrete uniformity detection, perform noise elimination and construct data feature vectors, and at the same time, extract the associated data of the detection specification, and use these data to cluster the feature vectors to form a data group to be trained; train the initial model with the data group to be trained to generate an unsupervised uniformity detection model, which can analyze the uniformity of reinforced fiber materials;

[0105] The reinforced fiber material data are input into the unsupervised uniformity detection model one by one. First, similarity matching is performed to output preliminary detection results. Then, each detection result is integrated with the previous detection result to obtain a complete uniformity detection benchmark.

[0106] The generated uniformity test benchmark is compared with the current reinforced fiber material data to generate the final uniformity test result. This result is used to evaluate the distribution and uniformity of concrete reinforced fiber materials in actual applications.

[0107] Example 5

[0108] In one embodiment, step (4) includes:

[0109] Controlling the mixer device to start a mixing program and outputting an initial temperature detection mark from the initial mixture;

[0110] Determine the current temperature data and temperature change trend obtained by the temperature monitoring device, the temperature change trend includes the initial temperature change trend and the real-time temperature change trend;

[0111] Determine and output a plurality of new temperature detection points, and determine temperature data and a temperature change trend for each new temperature detection point until the number of consecutive new temperature change trends reaches a preset change trend threshold, or the current temperature detection point is determined to be the last detection point;

[0112] Based on a preset temperature change trend threshold, adjusting the stirring rate of the mixer, returning to execute acquiring new temperature data from the initial mixture until the continuous number of new temperature change trends reaches a preset number threshold, or determining that the current temperature detection point is the last detection point;

[0113] Generate and output a list based on each temperature data and temperature change trend;

[0114] Determining the current temperature data and change trend obtained by the temperature monitoring device includes the following steps:

[0115] Obtain the temperature monitoring data and time of the current mixture batch, where the time is the duration from the output of the current temperature detection point to the acquisition of the temperature data;

[0116] Determine the current temperature change trend based on the temperature data, where the temperature change trend includes the initial temperature change trend and the real-time temperature change trend;

[0117] If the temperature change trend reaches a set threshold, the parameters for adjusting the stirring rate are determined based on the temperature change trend;

[0118] If the temperature change trend does not reach the set threshold, the current adjustment rate is determined to be 0, and the original stirring conditions are kept unchanged.

[0119] The principle and beneficial effects of the above scheme are as follows: Preparation of initial mixture: Add mixture A, solution B, triethanolamine and tannic acid into the mixing chamber of the mixer in a predetermined proportion; Initial mixing and stirring: Start the mixer equipment and start stirring the initial mixture according to the preset stirring rate until all components are evenly mixed; Initial temperature monitoring: After the mixture starts to be stirred, the initial temperature of the mixture is obtained through the temperature monitoring device, and the initial temperature data is output; Real-time temperature data acquisition: During the stirring process, the temperature data of the current mixture is obtained from the temperature monitoring device at regular intervals, and the time and corresponding temperature value of the current temperature detection point are recorded; Temperature change trend determination: Based on the initial temperature data and real-time temperature data, the initial temperature change trend is determined; Continuously monitor the temperature change and determine the real-time temperature change trend of each new temperature detection point; Determine the number of temperature detection points: Repeat the temperature change trend monitoring until the continuous number of new temperature change trends reaches the preset change trend threshold , or reach the last temperature detection point; adjust the stirring rate: when the temperature change trend reaches the preset threshold, adjust the stirring rate of the mixer based on the trend. If the threshold is not reached, keep the stirring rate unchanged; repeat temperature monitoring and rate adjustment: based on the new stirring rate and temperature monitoring data, continue to obtain and analyze temperature data until the continuous number of new temperature change trends reaches the preset number threshold, or reaches the last detection point; generate a temperature change list: generate a list of the temperature data of each temperature detection point and the corresponding temperature change trend, and output it; final temperature monitoring confirmation: when the mixing process is over, obtain the temperature data of the last temperature detection point through the temperature monitoring device to confirm the final temperature change trend; end mixing: based on the temperature change trend and the stirring rate adjustment result, stop the operation of the mixer equipment, complete the mixing and mixing operation of the mixture A, solution B, triethanolamine and tannic acid, and obtain high-strength anti-cracking concrete for wet joints. Through real-time temperature monitoring and stirring rate adjustment, precise control of the mixing process is achieved, thereby improving the quality and performance of high-strength anti-cracking concrete for wet joints.

[0120] Test example

[0121] The concrete of the above-mentioned Examples 1-3 and Comparative Examples 1-8 were respectively subjected to performance tests according to the following test method standards.

[0122] Compressive strength: The compressive strength of concrete is tested according to GB / T 50081-2019 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete". The specimen size is a cube of 150mm×150mm×150mm.

[0123] Flexural strength: The flexural strength of concrete was tested according to GB / T 50081-2019 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete". The specimen size was a small beam specimen of 150mm×150mm×550mm.

[0124] Split tensile strength: The splitting tensile strength of concrete is tested according to GB / T 50081-2019 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete". The specimen size is a cube of 150mm×150mm×150mm.

[0125] Elastic modulus: The elastic modulus of concrete was tested according to GB / T 50081-2019 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete". The specimen size was a prism of 150mm×150mm×300mm.

[0126] Crack resistance: The total crack area per unit area is measured according to GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete". The specimen size is a flat thin plate specimen of 800mm×600mm×100mm.

[0127] Flexural toughness index: The flexural toughness index of concrete is tested according to the "Fiber Concrete Test Method Standard" CECS13:2009. The specimen size is a small beam specimen of 150mm×150mm×550mm.

[0128] Chloride ion diffusion coefficient: The chloride ion diffusion coefficient of concrete is tested according to the Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete GB / T50082-2009. The specimen size is a cylinder of Φ100×50mm.

[0129] The performance data of Examples 1-3 and Comparative Examples 1-8 obtained according to the above test methods are shown in Table 1.

[0130] Table 1 Concrete performance test results of Examples 1-3 and Comparative Examples 1-8

[0131]

[0132] As can be seen from the data in Table 1, the concrete prepared by Examples 1-3 of the present invention not only has good compactness and mechanical properties, but also has better crack resistance than the concrete in the comparative example. In Comparative Example 1, only a single modified carbon fiber is used, resulting in a significant reduction in the tensile strength, flexural strength and bending toughness of the concrete. The use of a variety of fiber combinations in the present invention can provide a wider range of reinforcement effects, and the morphology and characteristics of different fibers are different, and the composite fiber can be more evenly dispersed in the concrete, reducing the aggregation phenomenon that may occur in a single fiber, and ensuring the uniformity of the reinforcement effect. The use of a single fiber cannot provide this multi-faceted reinforcement effect, resulting in a decrease in overall performance. In Comparative Examples 2 and 3, two types of reinforcing fibers are used, and it is found that the overall performance of the concrete is still reduced. In Comparative Example 4, carbon fiber is directly used without modification. The interface transition zone between the unmodified carbon fiber and the cement matrix is ​​not dense, and the interface bonding is weak, which is not conducive to the carbon fiber transferring the bridging stress to the matrix, and is not conducive to the performance of the composite material. The silicon dioxide on the surface of the modified carbon fiber has high activity and can react with calcium hydroxide in the cement matrix to form CSH gel, so that the interface of the modified carbon fiber and the cement matrix is ​​more compact, the bonding strength is higher, and the overall mechanical properties of the concrete are enhanced. In comparative example 5, ultra-high molecular weight polyethylene fiber is directly used without surface modification. The interface transition zone between the unmodified fiber and the cement group is not dense, and the interface bonding force is insufficient, thereby affecting the overall performance of the concrete. In comparative example 6, nano-silicon dioxide is not used, and the concrete lacking nano-silicon dioxide exhibits lower compressive strength, flexural strength, elastic modulus and resistance to chloride ion penetration. In comparative example 7, triethanolamine is not contained. Triethanolamine is a commonly used early strength agent. By accelerating the cement hydration reaction, the early strength is improved. The lack of triethanolamine causes the early strength of the concrete to develop slowly, and the compressive strength and flexural strength are lower than those in the embodiment. In comparative example 8, tannic acid is not contained. Tannic acid, as an organic additive, can improve the bonding force between the fiber and the matrix, enhance the crack resistance and toughness of the concrete, and its absence causes the role of the fiber in the matrix to be weakened, and cracks are more likely to form and expand. The high-strength anti-cracking concrete for wet joints prepared by the reasonable combination and synergistic effect of these components in the present invention can show excellent performance in terms of strength, toughness, crack resistance and durability, and meet the needs of practical applications.

[0133] Finally, it should be noted that the above-mentioned embodiments only express several implementation methods of the present invention and are not intended to limit the invention. For those skilled in the art, any modification, equivalent replacement, improvement, etc. made without departing from the concept of the present invention should be included in the protection scope of the invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A high-strength anti-cracking concrete for wet joints, characterized in that: The invention comprises the following raw materials in parts by weight: 150-180 parts of water, 400-480 parts of cement, 960-1080 parts of coarse aggregate, 600-750 parts of fine aggregate, 50-80 parts of silica fume, 50-100 parts of fly ash, 25-45 parts of limestone, 5-12 parts of water reducing agent, 35-58 parts of reinforcing fiber, 10-25 parts of nano silicon dioxide, 1.5-4.5 parts of triethanolamine and 0.4-2.4 parts of tannic acid; The reinforcing fiber is composed of modified carbon fiber, surface modified ultra-high molecular weight polyethylene fiber and nylon fiber in a mass ratio of 1: (0.4-0.6): (0.4-0.6); The preparation steps of the modified carbon fiber are as follows: treating the carbon fiber with a nitric acid solution to remove surface impurities, then immersing it in a silane coupling agent, and placing it in a constant temperature water bath for 2-3 hours. The treated carbon fiber is washed with deionized water and dried; dissolving tetraethyl orthosilicate in ethanol, adding a deionized surfactant, stirring evenly, and continuously dropping ammonia water to obtain a modified reaction solution; placing the treated carbon fiber in the modified reaction solution, and reacting it in a constant temperature water bath for 12-24 hours. After the reaction is completed, the reactant is taken out and aged at room temperature for 24 hours. Finally, the product is washed with deionized water and dried to obtain the modified carbon fiber; The specific preparation steps of the surface modified ultra-high molecular weight polyethylene fiber are as follows: the ultra-high molecular weight polyethylene fiber is washed with ethanol and dried; an ethanol / water mixed solution containing a silane coupling agent is prepared, the pH value is adjusted to 4.0-5.5 with acetic acid, and the dried ultra-high molecular weight polyethylene fiber is immersed in the ethanol / water mixed solution of the silane coupling agent for 1-2 hours, and after the immersion is completed, it is dried at 100-120°C for 2-4 hours to obtain the surface modified ultra-high molecular weight polyethylene fiber.

2. The high-strength anti-cracking concrete for wet joints according to claim 1, characterized in that: The coarse aggregate is crushed stone with a particle size of 5-20 mm and continuous grading.

3. The high-strength anti-cracking concrete for wet joints according to claim 1, characterized in that: The fine aggregate is composed of medium-coarse sand and fine sand. The fineness modulus of the medium-coarse sand is 2.6-2.8, and the fineness modulus of the fine sand is 2.2-2.5; among them, in terms of mass fraction, the medium-coarse sand is 70-80%, and the fine sand is 20-30%.

4. The high-strength anti-cracking concrete for wet joints according to claim 1, characterized in that: The particle size of silica fume is 100-200nm, and the SiO2 content is ≥96%; the fly ash is Class I fly ash; and the average particle size distribution of limestone is 5-10mm.

5. The high-strength anti-cracking concrete for wet joints according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid-based water reducing agent, and its water reducing rate is ≥25%.

6. The high-strength anti-cracking concrete for wet joints according to claim 1, characterized in that: The nylon fiber is nylon 66 fiber.

7. A method for preparing high-strength anti-cracking concrete for wet joints as claimed in any one of claims 1 to 6, characterized in that: The steps include: (1) Weigh the raw materials according to the ratio; (2) Add cement, coarse aggregate, fine aggregate, silica fume, fly ash and limestone into a mixer and perform dry mixing first to ensure that the components are evenly mixed; then add reinforcing fiber and nano-silica to the dry-mixed powder mixture and perform dry mixing again to ensure that the components are evenly distributed, thereby obtaining a mixture A; (3) dissolving the water reducing agent in water to obtain solution B; (4) Mixture A, solution B, triethanolamine and tannic acid and mix them evenly to obtain high-strength anti-cracking concrete for wet joints.