Hydrogen bond self-assembled organic long afterglow material as well as preparation method and application thereof
The supramolecular grid structure formed through hydrogen bond self-assembly solves the problems of short phosphorescence lifetime and low efficiency of existing organic long-afterglow materials, achieves efficient fluorescence-room temperature phosphorescence multiple emission, and extends the phosphorescence lifetime under visible light excitation. Used for multiple encryption and decryption.
Patent Information
- Application Number
- CN202410893786.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-29
AI Technical Summary
Existing organic long-afterglow materials require external assistance to increase the intersystem jump process and reduce non-radiative transitions, resulting in short phosphorescence lifetime and low efficiency, and there are few types of intermolecular connections, resulting in loose molecular accumulation.
A one-step method is used to self-assemble phenothiazine molecules through hydrogen bonds to form a supramolecular grid structure to achieve efficient fluorescence-room temperature phosphorescence multiple emission. It forms a highly ordered spatial grid structure through hydrogen bond self-assembly to limit molecular motion and promote Intersystem jump rate.
It achieved a phosphorescence lifetime of up to 305ms, a quantum efficiency of 4%, long-life room temperature phosphorescence under visible light excitation, and was successfully used in multiple encryption and decryption applications.
Smart Images

Figure CN118852052A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic long afterglow luminescent materials, and in particular to a hydrogen bond self-assembled organic long afterglow material and a preparation method and application thereof. Background Art
[0002] At present, most organic long afterglow materials are excited by ultraviolet light, and their applications are mainly anti-counterfeiting, data encryption, sensing, etc. Compared with ultraviolet light, visible light has less phototoxicity, is more penetrating and less lethal for biological analysis and biological imaging, and is more convenient for practical application.
[0003] In order to achieve long afterglow emission, small molecule crystal long afterglow materials usually need to use external forces to increase the intersystem crossing process and reduce non-radiative transitions. For example, functional groups such as carbonyl, hydroxyl, carboxylic acid, carboxylate, sulfone, halogen heavy atoms are introduced into the molecules to increase the intersystem crossing rate. These functional groups are used to promote spin-orbit coupling and generate more triplet excitons.
[0004] However, there are few studies on compounds that do not require any external assistance, are easy to obtain, efficient and have a long life. In the early stage of research, the present invention prepared a visible light-excited organic long afterglow material, which introduced a methyl group into the molecular structure. There is no hydrogen bond between molecules, and there are only three interactions between molecules, including S=O···HC S=O···HC and CH···HC Although the intermolecular connections of these three molecules are relatively short, less than However, there are fewer types of intermolecular connections, the molecular stacking is relatively loose, and the triplet excitons will be lost through non-radiative transitions or quenched by oxygen, moisture, etc. in the surrounding environment, so their phosphorescence lifetime is shorter and the efficiency is relatively low (about 1.8%). To this end, the present invention provides a hydrogen bond self-assembled organic long afterglow material and its preparation method and application. Summary of the invention
[0005] The present invention provides a hydrogen bond self-assembled organic long afterglow material and its preparation method and application. On the one hand, it solves the technical problem that an external force is needed to increase the intersystem crossing process and reduce the non-radiative transition to achieve the long afterglow emission of small molecules. On the other hand, based on the fact that the organic long afterglow material molecules excited by visible light prepared by the present invention in the early stage of research do not have hydrogen bonds and few types of intermolecular connections, the molecules are loosely stacked, resulting in a short phosphorescence life and low phosphorescence efficiency. Based on the structural characteristics of the phenothiazine molecule itself and the effect of hydrogen bond self-assembly, the present invention adopts a one-step method to directly oxidize the phenothiazine molecule to obtain a hydrogen bond self-assembled supramolecular grid structure. This extremely simple small molecule can be self-assembled by hydrogen bonds without introducing any substituents to achieve efficient fluorescence-room temperature phosphorescence multiple emission, and the phosphorescence life is as long as 305ms, and the quantum efficiency can reach 4%. Furthermore, long-life room temperature phosphorescence can also be achieved under the excitation of easily available visible light, and the excitation wavelength range is between 350 and 475nm.
[0006] The first object of the present invention is to provide a method for preparing a hydrogen bond self-assembled organic long afterglow material, characterized in that it comprises the following steps:
[0007] Phenothiazine is added to a mixed solution of dichloromethane and glacial acetic acid, and then H2O2 is added, and a one-step oxidation reaction is performed, followed by cooling, extraction, separation and purification, and crystallization to obtain a hydrogen-bonded self-assembled organic long afterglow material.
[0008] As a preferred embodiment, the molecular stacking of the hydrogen bond self-assembled organic long afterglow material presents a planar and herringbone crystal state.
[0009] As a preferred embodiment, the usage ratio of phenothiazine, dichloromethane, glacial acetic acid and H2O2 is 0.01 mol:60 mL:30 mL:0.012-0.015 mol.
[0010] As a preferred embodiment, the reaction temperature is 45°C to 60°C.
[0011] As a preferred embodiment, the reaction time is 12h to 24h.
[0012] As a preferred embodiment, after the reaction is completed, a crude product is obtained, the crude product is cooled to room temperature, and extracted three times with dichloromethane to obtain a secondary product.
[0013] As a preferred embodiment, the secondary product is separated and purified by column chromatography using dichloromethane and petroleum ether in a volume ratio of 2:1.
[0014] The second object of the present invention is to provide a hydrogen bond self-assembled organic long afterglow material prepared by the above preparation method.
[0015] The third object of the present invention is to provide an application of the above hydrogen bond self-assembled organic long afterglow material in multiple data encryption and decryption.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] The invention provides a hydrogen bond self-assembled organic long afterglow material and a preparation method and application thereof. Phenothiazine is added to a mixed solution of dichloromethane and glacial acetic acid, H2O2 is added, a one-step oxidation reaction is carried out, cooling, extraction, separation and purification, and crystallization are performed to obtain the hydrogen bond self-assembled organic long afterglow material.
[0018] Based on the structural characteristics of phenothiazine molecules and the effect of hydrogen bond self-assembly, the present invention adopts a one-step method to directly oxidize phenothiazine molecules to obtain a hydrogen bond self-assembled supramolecular grid structure. This extremely simple small molecule can be self-assembled by hydrogen bonds without introducing any substituents to achieve efficient fluorescence-room temperature phosphorescence multiple emission. The organic long afterglow material prepared by the present invention has a phosphorescence lifetime of up to 305ms and a quantum efficiency of up to 4%. In addition, the organic long afterglow material prepared by the present invention can also achieve long-life room temperature phosphorescence under the excitation of easily available visible light, such as a mobile phone flashlight or an incandescent lamp, and the excitation wavelength range is between 350-475nm. Through crystal analysis, it is found that the molecules form a highly ordered spatial grid structure through hydrogen bond self-assembly, which can not only greatly limit the movement of molecules and inhibit the non-radiative transition of triplet excitons, but also effectively promote the intersystem crossing rate, thereby achieving efficient and long-life room temperature phosphorescence. The present invention utilizes the significant characteristics of long-life organic phosphorescence under visible light excitation to successfully realize the application of multiple encryption and decryption. This new visible-light-stimulated ultralong organic phosphorescence provides a new platform for expanding the scope of pure organic phosphorescent materials and their applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The preparation route of the hydrogen bond self-assembled organic long afterglow material OP of the present invention;
[0020] Figure 2 It is a crystalline stacking diagram of the visible light-excited hydrogen bond self-assembled organic long afterglow material prepared by the present invention; wherein, Figure a is a planar crystalline state, and Figure b is a herringbone crystalline state;
[0021] Figure 3 The hydrogen bond self-assembled organic long afterglow material excited by visible light prepared by the present invention is prepared in tetrahydrofuran (10 -5 M) UV-visible absorption spectrum (a) and steady-state photoluminescence spectrum (b) in solution;
[0022] Figure 4The graph is a fluorescence lifetime decay curve of the visible light excited hydrogen bond self-assembled organic long afterglow material prepared by the present invention in tetrahydrofuran solution under room temperature; wherein, the graph a is a planar crystalline state, and the graph b is a herringbone crystalline state;
[0023] Figure 5 Steady-state photoluminescence spectrum of compound OP-P in dimethyltetrahydrofuran solution at 77K (Figure a); time-resolved decay curve at 349nm (Figure b); time-resolved decay curves at 393, 409 and 437nm (Figure c); steady-state photoluminescence spectrum of compound OP-H in dimethyltetrahydrofuran solution (Figure d); time-resolved decay curve at 349nm (Figure e); time-resolved decay curves at 391, 410 and 449nm (Figure f);
[0024] Figure 6 The steady-state photoluminescence spectrum (black line) and phosphorescence spectrum (blue filled part) of the organic long afterglow material of the present invention in the crystalline state; wherein the inset is a luminescence photograph under a 365nm ultraviolet lamp (left) and a luminescence photograph after turning off the ultraviolet lamp (right), Figure a is compound OP-P, and Figure b is compound OP-H;
[0025] Figure 7 The steady-state photoluminescence spectrum of compound OP-P in the crystalline state (a); the time-resolved decay curve at 389 nm (b); the time-resolved decay curve at 434 nm and 504 nm (c); the steady-state photoluminescence spectrum of compound OP-H (d); the time-resolved decay curve at 381 nm (e); the time-resolved decay curve at 452 nm and 508 nm (f);
[0026] Figure 8 Steady-state photoluminescence spectrum of compound OP-P at 77K in the crystalline state (a); time-resolved decay curve at 367nm (b); time-resolved decay curve at 425, 437 and 468nm (c); steady-state photoluminescence spectrum of compound OP-H at 77K (d); time-resolved decay curve at 367nm (e); time-resolved decay curve at 448nm and 474nm (f);
[0027] Fig. 9 Afterglow peak excitation spectra of the crystals of compounds OP-P (a) and OP-H (b) at room temperature. Insets: luminescence photos under the LED light of a mobile phone (above) and luminescence photos after turning off the LED light (below);
[0028] Fig.10Photoluminescence spectra (a) and corresponding time-resolved fluorescence decay curves (b) of thin films of compounds OP-P and OP-H (5% concentration doped in PMMA) under 330nm excitation at room temperature;
[0029] Fig.11 The unit cell and stacking structure of compound OP-P (a) (b); the unit cell and stacking structure of compound OP-H (c) (d);
[0030] Fig.12 The crystal stacking diagram of compound OP-P. Stacking diagram of bc plane (a); stacking diagram of ac plane (b); stacking diagram of ab plane;
[0031] Fig.13 The crystal stacking diagram of compound OP-P in the ab plane. One-layer stacking diagram (a); two-layer stacking diagram (b); one-layer and two-layer stacking model diagrams (c)(d);
[0032] Fig.14 The crystal stacking diagram of compound OP-H. Stacking diagram of bc plane (a); stacking diagram of ac plane (b); stacking diagram of ab plane;
[0033] Fig.15 The intermolecular interactions of compound OP-H (a); the interactions around each molecule of OP-H (b);
[0034] Fig.16 The dimer stacking diagram of OP-P (a); the dimer stacking diagram of OP-H (b);
[0035] Fig.17 Application of ultralong phosphors excited by visible light. Application of multiple data encryption using OP-P, BrTMOPP and o-MOPP (a); Explanation of multiple encryption using OP-P, BrTMOPP and o-MOPP crystals (b). DETAILED DESCRIPTION
[0036] In order to enable those skilled in the art to better understand the technical solution of the present invention and implement it, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention. The following test methods and detection methods, unless otherwise specified, are conventional methods; the reagents and raw materials, unless otherwise specified, are commercially available.
[0037] The technical contents of the present invention are analyzed and explained in detail below.
[0038] The present invention provides a method for preparing a hydrogen bond self-assembled organic long afterglow material, comprising the following steps:
[0039] Phenothiazine is added to a mixed solution of dichloromethane and glacial acetic acid, and then H2O2 is added to perform a one-step oxidation reaction to directly oxidize the phenothiazine molecules to obtain a hydrogen-bonded self-assembled supramolecular grid structure. The structure is then cooled, extracted, separated and purified, and crystallized to obtain a visible light-excited organic long afterglow material. The molecular stacking of the hydrogen-bonded self-assembled organic long afterglow material presents a planar and herringbone crystalline state.
[0040] In order to obtain a high-purity visible light-excited hydrogen bond self-assembled organic long afterglow material, the dosage ratio of phenothiazine, dichloromethane, glacial acetic acid and H2O2 is 0.01mol:60mL:30mL:0.012-0.015mol; when the volume concentration of H2O2 used is 30%, the dosage ratio of phenothiazine, dichloromethane, glacial acetic acid and H2O2 is 2g:60mL:30mL:2mL. The molar ratio of phenothiazine to H2O2 is limited to 0.01:0.012-0.015, so that the dosage of H2O2 is slightly larger than that of phenothiazine, so that phenothiazine is fully and completely oxidized. If the dosage of phenothiazine is larger than that of H2O2, there will be by-products and incompletely reacted raw materials in the product.
[0041] In order to make the reaction fully complete and obtain an organic long afterglow material with a high yield and purity, the reaction temperature is limited to 45-60° C. If the reaction temperature is lower than 45° C., the reaction progress will be slow and the reaction will be incomplete; if the reaction temperature is higher than 60° C., the excessively high reaction temperature will cause the rapid evaporation of dichloromethane and glacial acetic acid, thereby limiting the continuation of the reaction and inevitably affecting the yield of the product.
[0042] In order to make the reaction fully complete, the reaction time is limited to 12 to 24 hours. If it is less than 12 hours, although some organic long afterglow materials will be obtained, the reaction is not complete, and the product must be a mixture of raw materials and target products; when the reaction is 24 hours, the maximum yield of organic long afterglow materials is obtained, so there is no need to react for a longer time;
[0043] In order to purify the product after the reaction, after the reaction is completed, a crude product is obtained, the crude product is cooled to room temperature, extracted three times with dichloromethane to obtain a secondary product, and the secondary product is separated and purified by column chromatography using dichloromethane and petroleum ether in a volume ratio of 2:1, and the product is extracted and purified to remove glacial acetic acid and by-products.
[0044] The effects are described below in conjunction with specific embodiments.
[0045] Example 1
[0046] A method for preparing a hydrogen bond self-assembled organic long afterglow material comprises the following steps:
[0047] 2 g of phenothiazine was added to 60 mL of dichloromethane (analytical grade) and 30 mL of glacial acetic acid (analytical grade), and 2 mL of 30% H2O2 was slowly added dropwise. The reactants were stirred at 60°C for 24 h. After cooling to room temperature, they were extracted three times with dichloromethane, and then separated and purified by column chromatography (dichloromethane: petroleum ether = 2:1) to crystallize out two crystalline states.
[0048] The molecular stacking presents a planar crystalline state, which we named OP-P; the molecular stacking presents a herringbone crystalline state, which we named OP-H. The synthetic route of compound OP is as follows Figure 1 As shown, the stacking diagrams of the two crystalline states of OP-P and OP-H are as follows Figure 2 shown.
[0049] For OP-P, 1 H NMR (500MHz, d6-DMSO, δ [ppm]): 10.95 (s, 1H), 7.96 (d, J = 8.0Hz, 2H), 7.65-7.68 (m, 2H), 7.38 (d, J = 8.5Hz, 2H), 7.26 (t, J = 7.5Hz, 2H).
[0050] 13 C NMR(125MHz,d6-DMSO,δ[ppm]):138.64,133.75,122.94,121.87,121.18,117.49.MS[m / z]:Calcd for C 12 H9NO2S:231.04,Found 254.0237[M+Na] + .Anal.Calcd forC 12 H9NO2S: C, 62.32; H, 3.92; N, 6.06. Found: C, 62.21; H, 3.84; N, 6.15.
[0051] For OP-H, 1 H NMR (500MHz, d6-DMSO, δ [ppm]): 10.95 (s, 1H), 7.95 (d, J = 8.0 Hz, 2H), 7.65-7.68 (m, 2H), 7.37 (d, J = 8.5 Hz, 2H), 7.25-7.28 (m, 2H).
[0052] 13 C NMR(125MHz,d6-DMSO,δ[ppm]):138.64,133.77,122.96,121.91,121.18,117.50.MS[m / z]:Calcd for C 12H9NO2S:231.04,Found 254.0243[M+Na] + .Anal.Calcd forC 12 H9NO2S: C, 62.32; H, 3.92; N, 6.06. Found: C, 62.33; H, 3.86; N, 6.12.
[0053] The performance of the hydrogen bond self-assembled organic long afterglow material prepared above was tested, and the specific process and results are as follows:
[0054] 1. Study on Photophysical Properties
[0055] The absorption spectra, steady-state photoluminescence spectra, excitation spectra and time-resolved emission spectra of the compounds prepared in the embodiments of the present invention in solution and crystal state were systematically studied. -5 M) UV-visible absorption spectrum in solution Figure 3 As shown in Figure a. As can be seen from the figure, their absorption spectra are basically the same, OP-P and OP-H have stronger absorption, with absorption peaks at 270nm, 300nm, and 333nm. In addition, OP-P and OP-H also show similar steady-state photoluminescence spectra in solution ( Figure 3 (b) The emission spectra of OP-P and OP-H show slight fine vibrations, with emission peaks at 352nm, 362nm and 354nm, 362nm, respectively. At room temperature, we also tested their fluorescence lifetime decay curves in solution. The emission lifetimes of OP-P at 352nm and 362nm were 1.42ns and 1.46ns, respectively, the emission lifetimes of OP-H at 354nm and 362nm were 1.39ns and 1.38ns, respectively, and the emission lifetime of MOP at 355nm was 1.27ns. All of these emission lifetimes were in the nanosecond range, which is a typical monomer fluorescence emission.
[0056] To further understand the photophysical properties of these compounds, we studied their steady-state photoluminescence spectra and time-resolved decay curves under cryogenic conditions, e.g. Figure 4 and Figure 5As shown, the photophysical data of compounds OP-P and OP-H in the crystal state at room temperature were detected, as shown in Table 1. Under 77K conditions, due to the suppression of the non-radiative transition process of triplet excitons, the phosphorescence intensity is greatly enhanced in the steady-state photoluminescence spectrum in solution, while the fluorescence intensity is very weak. OP-P and OP-H clearly show three emission bands. For OP-P, there is a very weak emission band at 349nm with a lifetime of nanoseconds (1.46ns), which is attributed to fluorescence emission; there is a split emission band at 393 and 409nm, with lifetimes of 450 and 437ms, respectively, which is attributed to phosphorescence emission; there is a broad emission band at 437nm with a lifetime of 438ms, which is attributed to phosphorescence emission. OP-H shows similar emission properties, with a weak emission band at 349 nm with a lifetime of 1.60 ns, which is attributed to fluorescence emission, an emission band at 391 and 410 nm with lifetimes of 451 and 430 ms, respectively, and a strong emission band at 449 nm with a lifetime of 431 ms.
[0057] Table 1 Photophysical data of compounds OP-P, OP-H and MOP in the crystalline state at room temperature
[0058]
[0059] λ F : fluorescence emission peak; τ F : fluorescence lifetime; λ P : phosphorescence emission peak; τ P : Phosphorescence lifetime; Φ P : Phosphorescence quantum efficiency; k isc : intersystem crossing rate from singlet to triplet; k r : Phosphorescence radiation rate; k nr : non-radiative transition rate; k isc =Φ Phos / τ Fluo ;k r Phos =Φ Phos / τ Phos ;k nr Phos =(1-Φ Phos ) / τ Phos
[0060] In the crystal state, OP-P and OP-H show blue-white luminescence under 365nm excitation. After turning off the excitation light source, the naked eye can observe cyan-blue and cyan-green luminescence, respectively. The afterglow can last for several seconds. Figure 6 As shown. Figure 7It can be seen that, similar to the emission spectra at low temperatures, OP-P and OP-H crystals have three distinguishable emission bands. For OP-P, the maximum emission peaks are 389, 434, and 504 nm, respectively. The lifetime at the short wavelength of 389 nm is in the nanosecond range (1.86 ns), which is attributed to fluorescence emission; the lifetimes at the long wavelengths of 434 and 504 nm are 230 and 240 ms, respectively, which are attributed to phosphorescence emission. The intensity of phosphorescence emission is comparable to or even higher than the fluorescence intensity, achieving fluorescence-phosphorescence multiple emission at room temperature. The three emission peaks of OP-H crystals are at 381, 452, and 508 nm, respectively. The strongest emission is shown at the short wavelength of 381 nm, with a lifetime of nanoseconds (1.59 ns), which is attributed to fluorescence emission; the lifetimes at the long wavelengths of 452 and 508 nm are 269 and 305 ms, respectively, which are attributed to phosphorescence emission. The fluorescence emission intensity is higher than the phosphorescence intensity, and the fluorescence-room temperature phosphorescence multiple emission characteristics are also achieved.
[0061] The present invention further tests the steady-state photoluminescence spectra and corresponding time-resolved decay curves of these compound crystals at 77K, such as Figure 8 As shown. At low temperatures, these compounds are fixed, reducing the free movement of molecules, greatly suppressing luminescence quenching and non-radiative transitions, so the phosphorescence intensity in these spectra is greatly enhanced, and they all show three obvious emission bands. The maximum emission peaks of OP-P are at 367, 425, 437, and 468 nm. The lifetime at 367 nm is 3.05 ns, and the lifetimes at 425, 437, and 468 nm are 73, 106, and 241 ms, respectively. For OP-H crystals, the short-lived emission peak is at 367 nm with a lifetime of 3.09 ns, and the long-lived emission peak is at 448, 474 nm with a lifetime of 67, 182 ms.
[0062] Interestingly, OP-P and OP-H crystals can be excited by light from light-emitting diodes (LEDs), such as cell phone flashlights or even incandescent lamps. Fig. 9 As shown in Figure a, for OP-P, when the LED light is turned off, the naked eye can see a blue afterglow. For another crystalline OP-H, a green afterglow is shown after the LED light is removed. In order to study why these compounds can achieve long afterglow under visible light excitation, we tested their excitation spectra, such as Fig. 9 Both OP-P and OP-H crystals can be effectively excited by visible light at room temperature, with a wavelength range of 350-475nm. The maximum excitation wavelength of OP-P is 407nm, and the maximum excitation wavelength of OP-H is 410nm.
[0063] In order to understand the effect of aggregation on organic afterglow luminescence, we conducted a set of control experiments by doping the compounds at a concentration of 5% in polymethyl methacrylate (PMMA). Fig.10 As shown, at room temperature, the doped films of these compounds only have a broad blue light emission band at about 366nm, with a lifetime of nanoseconds, and no phosphorescence peak. These results prove that the organic long afterglow of the compounds comes from aggregated molecules with strong intermolecular connections rather than single molecules.
[0064] 2. Crystal Analysis
[0065] The single crystal data and intermolecular forces of the compounds OP-P and OP-H prepared by the present invention are shown in Tables 2 and 3.
[0066] Table 2 Single crystal data of compounds OP-P and OP-H
[0067]
[0068]
[0069] a R1=Σ||F o |-|F c || / Σ|F o |. b wR2=|Σw(|F o | 2 -|F c | 2 )| / Σ|w(F o 2 ) 2 | 1 / 2 .
[0070] Table 3 Intermolecular forces of compounds OP-P and OP-H
[0071]
[0072]
[0073] Since these compounds have similar electronic structures, their different luminescence behaviors may be attributed to different stacking modes, so we have conducted a detailed analysis of their single crystal structures. Table 2 provides the single crystal data of OP-P, OP-H, and Table 3 provides their weak intermolecular interactions. The unit cell and stacking structure of the compound are shown in Figure 2. Fig.11As shown. We call the OP molecule with a planar structure OP-P. The OP-P crystal is a monoclinic P21 / n space group, and each unit cell contains four independent molecules (Z=4). We call the OP molecule with a herringbone structure OP-H. The OP-H crystal is a monoclinic P21 / c space group, and each unit cell also contains four independent molecules (Z=4). MOP also has four molecules in each unit cell (Z=4). In OP-P, the four independent molecules are arranged in parallel and staggered up and down, while in OP-H, the four molecules are arranged in a parallelogram. From their overall stacking, there are more types of interactions between OP-P and OP-H molecules, and the stacking is tighter. This is because the exposed active hydrogen of OP-P and OP-H molecules produces strong intermolecular hydrogen bonds with the oxygen atoms of neighboring molecules, and the molecules are firmly locked in a three-dimensional network through intermolecular self-assembly, which effectively reduces the stretching vibration of the molecules themselves and reduces non-radiative inactivation. In addition, the molecule has a butterfly-like shape, which has a certain rigidity and flexibility, can inhibit the π-π stacking between molecules and reduce triplet-triplet quenching (TTA).
[0074] Fig.12 The crystal stacking diagrams of OP-P in the bc plane, ac plane and ab plane are shown. It can be clearly seen from the figure that no matter which axis, the molecules are connected together through strong intermolecular interactions to form a highly ordered spatial grid structure. Such a dense stacking structure can effectively fix the molecules and form a tight stacking structure in the entire space, thereby greatly suppressing the non-radiative transition of triplet excitons. Specifically, in the a-axis direction, each phenothiazine molecule is connected by intermolecular hydrogen bonds S=O···HN It is closely connected with another adjacent phenothiazine molecule, thus forming a directional head-to-tail connection and self-assembling into a supramolecular linear chain. In the b-axis direction, CH···HC The interaction connects the benzene ring of one phenothiazine to the benzene ring of another phenothiazine shoulder to shoulder, and the molecules hold hands and are tightly connected one by one. In the c-axis direction, through two C···C(3.344, ) The back-to-back and chest-to-chest interactions connect the molecules in each layer up and down, which plays an important role in restricting molecular motion and reducing the non-radiative decay of triplet excitons.
[0075] In addition, we extracted the ab plane in the crystal structure, such as Fig.13 As shown, there is a very strong intermolecular hydrogen bond S=O···HN in the ab plane, and the distance is very close. This strong intermolecular electronic coupling is conducive to promoting the intersystem crossing rate, thereby enhancing the phosphorescence quantum efficiency. Therefore, the intersystem crossing rate of OP-P is the largest, which is 2.1×107s-1 , the phosphorescence efficiency reaches 4%. On the other hand, the strong CH···HC double hydrogen bonds and S=O···HN hydrogen bonds between molecules connect the molecules in a highly orderly manner on the two-dimensional plane, forming a compact monolayer stacking structure, similar to a large π system, which further enhances the phosphorescence emission. More interestingly, taking the two-layer stacking structure as an example, each of the six-membered rings of the upper and lower phenothiazines are staggered, effectively avoiding the triplet-triplet quenching (TTA) that may be caused by molecular aggregation. Such a highly ordered grid structure can not only limit the movement of molecules and inhibit the non-radiative transition of triplet excitons, but also promote the intersystem crossing rate, thereby achieving efficient and long-lived room temperature phosphorescence. In addition, the mutual staggering of the luminophores between layers is conducive to avoiding quenching caused by molecular aggregation, further extending the life of room temperature phosphorescence.
[0076] Fig.14 The stacking diagrams of OP-H in the bc plane, ac plane, and ab plane are shown. Unlike OP-P, the stacking of OP-H crystals is more complex, with a herringbone arrangement. There are ten different short and strong interactions between molecules, including S=O···HN S=O···N S=O···HC S=O···HC S=O···HC CH···HN CH···N CH···C CH···C C···C Among these intermolecular connections, only the C···C interconnection is greater than The remaining intermolecular connections are very short, less than This shows that there is a strong interaction between molecules, which can provide the system with a more rigid spatial environment, restrict the movement of molecules, reduce the energy loss caused by non-radiative transitions, and thus extend the lifetime of phosphorescence.
[0077] Fig.15 The specific molecular interactions of OP-H crystals are shown. As can be seen from the figure, the S=O part of a molecule forms a strong intermolecular hydrogen bond with the active hydrogen of the NH of the adjacent molecule, S=O···HN The S=O part of the molecule also forms other types of intermolecular connections, such as S=O···N, S=O···HC, and S=O···HN. In addition, the benzene ring of one phenothiazine and the NH part of another phenothiazine will also form intermolecular CH···HN and CH···N connections. In addition, the molecules are closely connected to the surrounding molecules through CH···C and C···C. In this way, the CH sites of each molecule almost interact with the surrounding molecules (except sites 1 and 7) and are fixed in the middle by the surrounding molecules. This self-limiting crystal stacking greatly increases the rigidity of the molecule, helps to lock the conformation of the molecule and restrict the movement within the molecule, thereby reducing the non-radiative decay of triplet excitons. OP-H has a minimum radiative transition rate of 0.06s -1 , the minimum non-radiative transition rate is 3.2s -1 The phosphorescence lifetime is also relatively longer at 305ms.
[0078] In addition, we also studied the π-π interactions of their dimers. Fig.16 As shown, OP-P exhibits strong interlayer π-π interactions, and the layers interact with each other through chest-to-chest and back-to-back π-π interactions ( and ) connects the molecules in each layer up and down. Similarly, OP-H also exhibits strong π-π interactions, with the distance between two adjacent molecules being These strong π-π interactions effectively limit the non-radiative transitions of the molecules, stabilize the triplet excitons, and extend the lifetime of the phosphorescence. All of these crystal data are consistent with the photophysical data we tested, proving that the tighter the crystal stacking, the more conducive to the generation of room temperature phosphorescence. In the system of the present invention, the molecules self-assemble through hydrogen bonds to form a tightly packed three-dimensional network structure, which can effectively limit the non-radiative loss of triplet excitons to suppress luminescence quenching, and promote the intersystem crossing rate, which plays a vital role in achieving efficient and long-life room temperature phosphorescence.
[0079] 3. Application of Compounds OP-P and OP-H in Data Multiple Encryption
[0080] The present invention utilizes the significant characteristics of long-life organic phosphorescence under visible light excitation to construct a simple multiple encryption model. Fig.17As shown in the figure, we used different luminescent materials (OP-P, BrTMOPP and o-MOPP) to prepare a digital pattern "8", which emits blue light under ultraviolet light. OP-P molecules are used to mark the black character (a) "L". The afterglow emission of OP-P can be excited by both ultraviolet light and visible light. The afterglow under ultraviolet light is blue-green, and the afterglow under LED light is blue. The dark gray part of the number "8" (b) is marked with BrTMOPP crystals. BrTMOPP is a long-lived organic phosphorescent material, and the afterglow under ultraviolet light is green. The light gray part of the number "8" (c) is marked with o-MOPP molecules. o-MOPP is an organic phosphorescent material with a relatively short lifetime, and the afterglow is green.
[0081] Under the excitation of 365nm UV light, the pattern appears as a blue number "8". When the 365nm UV light is turned off, since the afterglow colors of these three materials are all green, the naked eye can see a green number "8". After about 1 second, due to the short afterglow lifetime of o-MOPP, the luminescent pattern turns into a green letter "E". Most organic long afterglow materials can achieve such data security protection, and for our system, under the excitation of LED light, an obvious blue letter "L" appears. This simple time-resolved technology not only includes the encryption of pattern codes from numbers to letters, but also includes the encryption of luminescent colors, realizing multiple encryption and decryption of data.
[0082] In summary, the present invention is based on the structural characteristics of the phenothiazine molecule itself and the possible role of hydrogen bond self-assembly, and adopts a one-step method to directly oxidize the phenothiazine molecule to obtain a hydrogen bond self-assembled supramolecular grid structure. This extremely simple small molecule can be self-assembled by hydrogen bonds without introducing any substituents to achieve efficient fluorescence-room temperature phosphorescence multiple emission. The phosphorescence lifetime is up to 305ms, and the quantum efficiency can reach 4%. In addition, they can also achieve long-life room temperature phosphorescence under the excitation of easily available visible light (mobile phone flashlight or incandescent lamp), and the excitation wavelength range is between 350-475nm. Crystal analysis found that the molecules form a highly ordered spatial grid structure through hydrogen bond self-assembly, which can not only greatly limit the movement of molecules and inhibit the non-radiative transition of triplet excitons, but also effectively promote the intersystem crossing rate, thereby achieving efficient and long-life room temperature phosphorescence. In addition, we use the significant characteristics of long-life organic phosphorescence under visible light excitation to successfully realize the application of multiple encryption and decryption. This new visible light-excited ultra-long organic phosphorescence may provide a new platform for expanding the scope of pure organic phosphorescent materials and their applications.
[0083] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing a hydrogen bond self-assembled organic long afterglow material, characterized in that: The following steps are involved: Phenothiazine is added to a mixed solution of dichloromethane and glacial acetic acid, and then H2O2 is added to perform a one-step oxidation reaction to oxidize the phenothiazine to form a hydrogen-bonded self-assembled supramolecular grid structure, thereby obtaining a hydrogen-bonded self-assembled organic long afterglow material.
2. The preparation method according to claim 1, characterized in that: The molecular stacking of the hydrogen bond self-assembled organic long afterglow material presents a planar and herringbone crystal state.
3. The preparation method according to claim 1, characterized in that: The usage ratio of phenothiazine, dichloromethane, glacial acetic acid and H2O2 is 0.01mol:60mL:30mL:0.012-0.015mol.
4. The preparation method according to claim 1, characterized in that: The reaction temperature is 45°C to 60°C.
5. The preparation method according to claim 1, characterized in that: The reaction time is 12h~24h.
6. The preparation method according to claim 1, characterized in that: After the reaction is completed, a crude product is obtained, which is cooled to room temperature and extracted with dichloromethane to obtain a secondary product.
7. The preparation method according to claim 6, characterized in that: The secondary product is separated and purified by column chromatography using dichloromethane and petroleum ether to obtain a visible light excited organic long afterglow material.
8. A hydrogen bond self-assembled organic long afterglow material prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the hydrogen bond self-assembled organic long afterglow material according to claim 8 in multiple data encryption and decryption.
Citation Information
Patent Citations
New emitter materials and matrix materials for optoelectronic and electronic components, in particular organic light-emitting diodes (OLEDS)
CN108604644A
Fused heterocyclic aromatic hydrocarbon derivative as well as preparation and application thereof
CN111349090A