Fluorine-containing resin for manufacturing pixel Bank layer, synthesis process of fluorine-containing resin and fluorine-containing resin composition
By using fluorine-containing resin and its composition in the pixel bank layer, the problems of poor liquid repellency and insufficient heat resistance of the material are solved, high liquid repellency, resolution and slope angle are improved, and OLED and QD- The problems of color overflow and color mixing during the printing process of LED displays meet the requirements of high reliability and heat resistance.
Patent Information
- Application Number
- CN202410833461.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-26
AI Technical Summary
The existing materials used for the pixel bank layer have poor liquid repellency, low resolution, low shape slope angle, and poor heat resistance, resulting in easy color overflow, color mixing, white defects, and poor reliability during the printing process of OLED and QD-LED displays. problem.
Using fluorine-containing resin and its composition, a pixel bank layer structure with high liquid repellency, high resolution, and high slope angle is prepared through free radical polymerization. Combining specific monomer ratios and process steps, it forms good adhesion and heat resistance. Good coating.
It effectively improves the problems of color overflow, color mixing, and white defects during ink printing, improves the reliability and heat resistance of the display panel, and meets the needs of high-definition pattern printing and large-size display.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photosensitive chemical materials, and in particular to a fluorine-containing resin for making a pixel bank layer, a synthesis process thereof, and a fluorine-containing resin composition. Background Art
[0002] The use of solution method to process OLED and QD-LED displays has the advantages of low cost, high production capacity, and easy to achieve large size, which is an important direction for the development of display technology. Among them, printing technology is considered to be the most effective way to achieve low cost and large size display of OLED and QD-LED. For example, when manufacturing large-size OLED panels, inkjet printing is sometimes used to make organic light-emitting layers to improve production efficiency and reduce costs; when manufacturing QD-LED panels, inkjet printing is often used to make QD layers; this type of inkjet printing process requires the formation of a high-precision pixel Bank layer on the substrate first to control the subsequent printing positions of different color inks, thereby forming a design pattern.
[0003] During the development of printing technology, the pixel bank layer has a very important influence on the printing yield and film uniformity. The surface of the bank layer needs to have a high liquid-repellent property to prevent ink overflow during printing to form color mixing or mura, and help improve the uniformity of ink film formation.
[0004] The materials currently used to make the bank layer generally have problems such as poor liquid repellency, low resolution, low shape slope angle, poor heat resistance, and high volatile matter, which lead to color mixing, white spots, foreign matter, mura, and poor reliability when making the color layer in the later stage. Summary of the invention
[0005] The purpose of the present invention is to provide a fluorine-containing resin for making a pixel bank layer.
[0006] The present invention also provides a synthesis process of fluorine-containing resin for making a pixel Bank layer.
[0007] The present invention also provides a fluorine-containing resin composition for preparing a pixel Bank layer.
[0008] The innovation of the present invention lies in the pixel Bank layer structure formed by the fluorine-containing resin and its composition in the present invention, which has the characteristics of high liquid repellency, high resolution, and high slope angle, and can effectively improve the defects such as color overflow, color mixing, and white deficiency that are prone to occur in the subsequent ink printing process; the formed pixel Bank layer structure has good adhesion and heat resistance, and meets the reliability requirements of the final display panel product.
[0009] In order to achieve the above-mentioned object of the invention, the technical solution of the present invention is:
[0010] A fluorine-containing resin used for making a pixel bank layer, the general molecular formula of which is:
[0011]
[0012] R 1 , R 2 , R 3 , R 4 are methyl or hydrogen atoms,
[0013] R 5 It is a structure in which the H atoms in the C1-C15 alkyl chain are completely or partially replaced by F atoms.
[0014] R 6 is a structure containing a glycidyl ester group,
[0015] R 7 is an auxiliary group, which is one or more of an alkyl group, an aromatic group, and an alicyclic group,
[0016] a, b, c, d are integers from 1 to 500 respectively;
[0017] The molecular weight of the fluorine-containing resin is 2,000 to 35,000.
[0018] Further, the following steps are included:
[0019] (1) Mixing monomers and a free radical initiator to obtain a mixed solution, wherein the monomers include fluorine-containing monomers, carboxyl-containing monomers, epoxy-containing monomers and other monomers, and the molar ratio of the fluorine-containing monomer in the monomers is
[0020] 5-40%, carboxyl monomers account for 5-20% by mole, epoxy monomers account for 20-60% by mole,
[0021] Other monomers account for 0-30%; the mass of free radical initiator accounts for 0.5-2.5% of the total monomers;
[0022] (2) Slowly adding the mixed solution dropwise into an ether ester solvent to carry out a free radical polymerization reaction to obtain a finished product.
[0023] Furthermore, the fluorine-containing monomer is one or more of tetrafluoropropyl acrylate, tetrafluoropropyl methacrylate, hexafluorobutyl acrylate, hexafluorobutyl methacrylate, octafluoropentyl acrylate, octafluoropentyl methacrylate, dodecafluoroheptyl acrylate, dodecafluoroheptyl methacrylate, tridecafluorooctyl acrylate, tridecafluorooctyl methacrylate, trifluorohydroxyethyl acrylate or trifluorohydroxyethyl methacrylate.
[0024] Furthermore, the carboxyl group-containing monomer is one or more of acrylic acid and methacrylic acid.
[0025] Furthermore, the epoxy group-containing monomer is one or more of glycidyl methacrylate, glycidyl acrylate, 3,4-epoxycyclohexyl methyl methacrylate, and 3,4-epoxycyclohexyl methyl acrylate.
[0026] Further, the other monomers are auxiliary monomers, including one or more of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, n-octyl acrylate, n-octyl methacrylate, isooctyl acrylate, isooctyl methacrylate, dodecyl acrylate, dodecyl methacrylate, tetradecyl acrylate, tetradecyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, n-decyl acrylate, n-decyl methacrylate, isodecyl acrylate, isodecyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, benzyl acrylate, benzyl methacrylate, isobornyl acrylate, isobornyl methacrylate, dicyclopentanyl acrylate, dicyclopentanyl methacrylate or maleic anhydride.
[0027] A fluorine-containing resin composition for making a pixel bank layer comprises the following raw materials in percentage by mass: 20 to 80% of a fluorine-containing resin, 10 to 70% of a photopolymerizable compound, and 5 to 15% of a photopolymerization initiator.
[0028] Furthermore, the raw materials are dissolved in a polar solvent or a diluent monomer to form a composition solution with a solid mass fraction of 5 to 60%.
[0029] Further, the photopolymerizable compound is methyl acrylate, methyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2-1,2-ethylenediyl acrylate, ethylene glycol methacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, triethylene glycol dimethacrylate, propylene glycol diacrylate, propylene glycol dimethacrylate, trimethylolpropane triacrylate, tetra(trimethylolpropane)tetraacrylate, tetra(trimethylolpropane)tetramethacrylate, pentaerythritol monoacrylate, pentaerythritol monomethacrylate, pentaerythritol tetraacrylate, pentaerythritol tetramethacrylate, polydipentaerythritol pentaacrylate, polydipentaerythritol pentamethacrylate, polydipentaerythritol hexaacrylate, polydipentaerythritol hexamethacrylate,
[0030] One or more of 1,6-hexanediol diacrylate.
[0031] Furthermore, the photopolymerization initiator is an oxime ester photoinitiator, and its general formula is:
[0032]
[0033] The molecular formula of X is
[0034]
[0035] R 8 is phenyl, C1-C20 alkyl, -CN, -NO2 or C1-C4 haloalkyl, R 9 is a C2-C12 alkyl group or a C4-C8 acyl group, R 10 -R 14 is H, a halogen atom, a C1-C12 alkyl group, a phenyl group or C6H5S-, R 15 , R 16 is H, a halogen atom, a C1-C12 alkyl group or a phenyl group.
[0036] The beneficial effects of the present invention are:
[0037] 1. The pixel Bank layer structure formed by the fluorine-containing resin and its composition in the present invention has the characteristics of high liquid repellency, high resolution and high slope angle, which can effectively improve the defects such as overflow, color mixing and white deficiency that are prone to occur in the subsequent ink printing process; the formed pixel Bank layer structure has good adhesion and heat resistance, and meets the reliability requirements of the final display panel product. DETAILED DESCRIPTION
[0038] The following will provide a clear and complete description of the technical solutions in the embodiments of the present invention.
[0039] Embodiment 1: A fluorine-containing resin for making a pixel bank layer, the general molecular formula of which is:
[0040]
[0041] R 1 , R 2 , R 3 , R 4 are methyl or hydrogen atoms,
[0042] R 5 It is a structure in which the H atoms in the C1-C15 alkyl chain are completely or partially replaced by F atoms.
[0043] R 6 is a structure containing a glycidyl ester group,
[0044] R 7 is an auxiliary group, which is one or more of an alkyl group, an aromatic group, and an alicyclic group,
[0045] a, b, c, d are integers from 1 to 500 respectively;
[0046] The molecular weight of the fluorine-containing resin is 2,000 to 35,000.
[0047] Example 2: A synthesis process of a fluorine-containing resin for making a pixel Bank layer is free radical copolymerization: heat the solvent propylene glycol methyl ether acetate to 75°C; mix the monomers and the free radical initiator to obtain a mixed solution, wherein the monomers contain 22.5% hexafluorobutyl methacrylate by mole percentage, 12.5% methacrylic acid by mole percentage, 40% methacrylate glycidyl ether by mole percentage, and 25% benzyl methacrylate by mole percentage, and the free radical initiator is azobisbutyronitrile whose mass is 1.0% of the total mass of the above monomers; slowly add the mixed solution dropwise to the propylene glycol methyl ether acetate solvent, and after the dropwise addition is completed, heat it to 95°C and react for 3 hours to obtain a fluorine-containing resin 1 with a solid content of 20%. The weight average molecular weight tested by GPC is 6519 and the PDI is 2.0.
[0048] Example 3: A synthesis process of a fluorine-containing resin for making a pixel Bank layer is free radical copolymerization: heat the solvent methyl 3-methoxypropionate to 75°C; mix the monomers and the free radical initiator to obtain a mixed solution, wherein the monomers contain 5% by mole of octafluoropentyl methacrylate, 20% by mole of methacrylic acid, 60% by mole of acrylic acid glycidyl ether, and 15% by mole of methacrylate cyclohexyl, and the free radical initiator is dibenzoyl peroxide with a mass of 0.5% of the total mass of the above monomers; slowly drop the mixed solution into the methyl 3-methoxypropionate solvent, and after the dropwise addition is completed, heat to 95°C and react for 6 hours to obtain a fluorine-containing resin 2 with a solid content of 30%. The weight average molecular weight tested by GPC is 8136 and the PDI is 1.9.
[0049] Example 4: A synthesis process of a fluorine-containing resin for making a pixel Bank layer is free radical copolymerization: heat the solvent diethylene glycol dimethyl ether to 75°C; mix monomers and free radical initiators to obtain a mixed solution, wherein the monomers contain 40% by mole of dodecafluoroheptyl methacrylate, 10% by mole of methacrylic acid, 20% by mole of 3,4-epoxycyclohexyl methyl methacrylate, and 30% by mole of cyclohexyl methacrylate, and the free radical initiator is azobisbutyronitrile whose mass is 1.5% of the total mass of the above monomers; slowly drop the mixed solution into the diethylene glycol dimethyl ether solvent, and after the dropwise addition is completed, heat to 95°C and react for 4.5 hours to obtain a fluorine-containing resin 3 with a solid content of 35%. The weight average molecular weight tested by GPC is 5869 and the PDI is 1.9.
[0050] Example 5: A synthesis process of a fluorine-containing resin for making a pixel Bank layer is free radical copolymerization: heat the solvent diethylene glycol diethyl ether to 75°C; mix monomers and free radical initiators to obtain a mixed solution, wherein the monomers contain 40% hexafluorobutyl acrylate, 5% methacrylic acid, 40% glycidyl acrylate, and 15% cyclohexyl methacrylate by mole, and the free radical initiator is azobisbutyronitrile whose mass is 1.0% of the total mass of the above monomers; slowly add the mixed solution to the diethylene glycol diethyl ether solvent, and after the addition is completed, heat it to 95°C and react for 5 hours to obtain a fluorine-containing resin 4 with a solid content of 40%. The weight average molecular weight tested by GPC is 6406 and the PDI is 2.0.
[0051] Example 6: Reference Example 1: The fluorine-containing monomer can also be one or more of tetrafluoropropyl acrylate, tetrafluoropropyl methacrylate, hexafluorobutyl acrylate, hexafluorobutyl methacrylate, octafluoropentyl acrylate, octafluoropentyl methacrylate, dodecafluoroheptyl acrylate, dodecafluoroheptyl methacrylate, tridecafluorooctyl acrylate, tridecafluorooctyl methacrylate, trifluorohydroxyethyl acrylate or trifluorohydroxyethyl methacrylate.
[0052] The carboxyl group-containing monomer may also be one or more of acrylic acid and methacrylic acid.
[0053] The epoxy group-containing monomer may also be one or more of glycidyl methacrylate, glycidyl acrylate, 3,4-epoxycyclohexyl methyl methacrylate, and 3,4-epoxycyclohexyl methyl acrylate.
[0054] Other monomers can also be auxiliary monomers, including methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, n-octyl acrylate, n-octyl methacrylate, isooctyl acrylate, isooctyl methacrylate, dodecyl acrylate, dodecyl methacrylate, tetradecyl acrylate, tetradecyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, n-decyl acrylate, n-decyl methacrylate, isodecyl acrylate, isodecyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, benzyl acrylate, benzyl methacrylate, isobornyl acrylate, isobornyl methacrylate, dicyclopentanyl acrylate, dicyclopentanyl methacrylate or maleic anhydride or one or more thereof.
[0055] Comparative Example 1: Referring to Example 1, 22.5% of hexafluorobutyl methacrylate was replaced with methyl methacrylate to obtain a fluorine-free resin. The weight average molecular weight thereof was 6874 and the PDI was 2.0 as tested by GPC.
[0056] Example 7: A fluorine-containing resin composition for making a pixel bank layer comprises the following raw materials in percentage by mass: 20% of the fluorine-containing resin of Example 1, 70% of a photopolymerizable compound, and 10% of a photopolymerization initiator; the raw materials are dissolved in a polar solvent, diethylene glycol methyl ethyl ether, to form a composition solution having a solid mass fraction of 5%.
[0057] The photopolymerizable compound is pentaerythritol tetraacrylate;
[0058] The photopolymerization initiator is an oxime ester photoinitiator, and its general formula is:
[0059]
[0060] The molecular formula of X is
[0061]
[0062] R 8 is phenyl, R 9 is a C2-C12 alkyl group, R 10 -R 14 For H.
[0063] Embodiment 8: A fluorine-containing resin composition for making a pixel bank layer, comprising the following raw materials in percentage by mass: 80% of the fluorine-containing resin of Embodiment 2, 15% of a photopolymerizable compound, and 5% of a photopolymerization initiator; the raw materials are dissolved in a diluent monomer 1,6-hexanediol diacrylate,
[0064] A composition solution with a solid mass fraction of 30% was formed.
[0065] The photopolymerizable compound is polydipentaerythritol hexaacrylate;
[0066] The photopolymerization initiator is an oxime ester photoinitiator, and its general formula is:
[0067]
[0068] The molecular formula of X is
[0069]
[0070] R 8 is a C1-C20 alkyl group, R 9 is a C4-C8 acyl group, R 10 -R 14 A halogen atom.
[0071] Example 9: A fluorine-containing resin composition for making a pixel bank layer, comprising the following raw materials in percentage by mass: 75% of the fluorine-containing resin of Example 3, 10% of a photopolymerizable compound, and 15% of a photopolymerization initiator, the raw materials being dissolved in a polar solvent, diethylene glycol dimethyl ether, to form a composition solution having a solid mass fraction of 60%;
[0072] The photopolymerizable compound is trimethylolpropane triacrylate.
[0073] The photopolymerization initiator is an oxime ester photoinitiator, and its general formula is:
[0074]
[0075] The molecular formula of X is
[0076]
[0077] R 8 is -CN group, R 9 is a C4-C8 acyl group, R 15 , R 16 For H.
[0078] Example 10: A fluorine-containing resin composition for making a pixel bank layer comprises the following raw materials in percentage by mass: 50% of the fluorine-containing resin of Example 4, 43% of a photopolymerizable compound, and 7% of a photopolymerization initiator.
[0079] The raw materials are dissolved in the diluent monomer diethylene glycol diacrylate to form a solid mass fraction of
[0080] 45% solution of the composition;
[0081] The photopolymerizable compound is polydipentaerythritol hexaacrylate;
[0082] The photopolymerization initiator is an oxime ester photoinitiator, and its general formula is:
[0083]
[0084] The molecular formula of X is
[0085]
[0086] R 8 For -NO2, R 9 It is a C2-C12 alkyl group, and R15 and R16 are halogen atoms.
[0087] Example 11: Referring to Example 7, the photopolymerizable compound is one or more of methyl acrylate, methyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2-ethylene glycol acrylate, ethylene glycol methacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, triethylene glycol dimethacrylate, propylene glycol diacrylate, propylene glycol dimethacrylate, trimethylolpropane triacrylate, tetrakis(trimethylolpropane)tetraacrylate, tetrakis(trimethylolpropane)tetramethacrylate, pentaerythritol monoacrylate, pentaerythritol monomethacrylate, pentaerythritol tetraacrylate, pentaerythritol tetramethacrylate, polydipentaerythritol pentaacrylate, polydipentaerythritol pentamethacrylate, polydipentaerythritol hexaacrylate, polydipentaerythritol hexamethacrylate, and 1,6-hexanediol diacrylate.
[0088] The photopolymerization initiator is an oxime ester photoinitiator, and its general formula is:
[0089]
[0090] The molecular formula of X is
[0091]
[0092] R 8 is phenyl, C1-C20 alkyl, -CN, -NO2 or C1-C4 haloalkyl, R 9 is a C2-C12 alkyl group or a C4-C8 acyl group, R 10 -R 14 is H, a halogen atom, a C1-C12 alkyl group, a phenyl group or C6H5S-, and R15 and R16 are H, a halogen atom, a C1-C12 alkyl group or a phenyl group.
[0093] Comparative Example 2: Referring to Example 10, 50% of the fluorine-containing resin in Example 4 was replaced by 50% of the fluorine-free resin in Comparative Example 1.
[0094] <Evaluation of liquid repellency>
[0095] The fluorine-containing resin composition was coated on a glass substrate using a spin coater (1H-36S: produced by Mikasa) and dried on a 90°C baking sheet for 2 min to form a coating film. A scanning mercury lamp exposure machine (MPA-400: produced by Canon, Japan) was used to expose the glass substrate at an irradiation dose of 50 mj / cm 2 The entire film was exposed and then baked in an oven at 230°C for 30 minutes to form a cured film with a thickness of 2 um.
[0096] Use a contact angle tester (DM-901: Kyowa) to drop PGMEA (propylene glycol methyl ether acetate, the same below) on the above-mentioned cured film for contact angle test. The amount of addition is 2 μL. Take a picture 30 seconds after the addition and measure the contact angle to obtain the PGMEA liquid contact angle value. The higher the PGMEA contact angle value, the better the liquid repellency of the coating.
[0097] <Aperture Resolution Evaluation>
[0098] The fluorine-containing resin composition was coated on a glass substrate using a spin coater (1H-36S: produced by Mikasa), dried on a baking plate at 90°C for 2 min to form a coating film, and exposed with a mask using a scanning mercury lamp exposure machine (MPA-400: produced by Canon, Japan). The mask contained circular shading areas with apertures of 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, and 20 um, thereby forming circular openings of corresponding diameters on the substrate; the exposure energy was 50 mj / cm 2 Exposure was performed; after exposure, development was performed for 60 seconds by spraying with a TMAH (tetramethylammonium hydroxide) developer having a concentration of 2.38%, and then baked in an oven at 230°C for 30 minutes.
[0099] An optical microscope (BX51TRF: Olympus) was used to observe the circular hole area of the substrate, and the hole diameters were observed from small to large. The smallest diameter circular hole with a circular shape and no residue in the hole was observed, and the corresponding mask aperture value was the aperture resolution value. The lower the aperture resolution, the easier it is for the composition to prepare finer patterns.
[0100] <Slope Angle Evaluation>
[0101] The fluorine-containing resin composition was coated on a glass substrate using a spin coater (1H-36S: produced by Mikasa), dried on a 90°C baking plate for 2 min to form a coating film, and exposed with a mask using a scanning mercury lamp exposure machine (MPA-400: produced by Canon, Japan). The mask contained a 20 um wide line shading area. The exposure energy was 50 mj / cm 2 Exposure was performed; after exposure, development was performed for 60 seconds by spraying with a TMAH (tetramethylammonium hydroxide) developer having a concentration of 2.38%, and then baked in an oven at 230°C for 30 minutes.
[0102] The cross section of the line is observed using a scanning electron microscope (SU8010, manufactured by Hitachi), and a trapezoidal or approximately trapezoidal cross section can be observed. The lower base angle of the trapezoid is measured to obtain the slope angle.
[0103] <Adhesion Evaluation>
[0104] The fluorine-containing resin composition was coated on a glass substrate using a spin coater (1H-36S: produced by Mikasa) and dried on a 90°C baking sheet for 2 min to form a coating film. A scanning mercury lamp exposure machine (MPA-400: produced by Canon, Japan) was used to expose the glass substrate at an irradiation dose of 50 mj / cm 2 The entire film was exposed and then baked in an oven at 230°C for 30 minutes to form a cured film with a thickness of 2 um.
[0105] After cutting out a hundred squares on the cured film with a square cutter, place it in a high temperature and high humidity chamber (EHS-211M: ESPEC) for testing. The test conditions are 120℃ / RH100% / 2atm and the test time is 24 hours. After the test is completed, the square cutter adhesion test is carried out according to GBT9286-1998. The test result level is the adhesion evaluation result.
[0106] <Heat resistance evaluation>
[0107] The fluorine-containing resin composition was coated on a glass substrate using a spin coater (1H-36S: produced by Mikasa) and dried on a 90°C baking sheet for 2 min to form a coating film. A scanning mercury lamp exposure machine (MPA-400: produced by Canon, Japan) was used to expose the glass substrate at an irradiation dose of 50 mj / cm 2 The entire film was exposed and then baked in an oven at 230°C for 30 minutes to form a cured film with a thickness of 2 um.
[0108] Heat resistance evaluation was performed using TG-DTA (TG8121: Rigaku). The coating was scraped into powder and loaded into the TGA equipment. N2 atmosphere was passed through and the temperature was raised to 400°C at a heating rate of 10°C / min. The temperature at which the mass loss was 5% was measured as the heat resistance evaluation standard. The higher the 5% thermal weight loss temperature, the better the heat resistance of the coating.
[0109] Using the above evaluation method, the evaluation results of the embodiments and comparative examples are shown in the following table:
[0110]
[0111] As can be seen from the above table, the Bank layer prepared by the embodiment has good advantages in liquid repellency, slope angle, and heat resistance, and can also maintain high adhesion and finer opening resolution. By comparison, by increasing the amount of fluorine-containing monomers in the resin synthesis process or increasing the amount of fluorine-containing resin added in the composition, the liquid repellency of the material can be improved to a certain extent.
[0112] The described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A fluorine-containing resin for making a pixel bank layer, characterized in that: Its molecular formula is: R 1 , R 2 , R 3 , R 4 are methyl or hydrogen atoms, R 5 It is a structure in which the H atoms in the C1-C15 alkyl chain are completely or partially replaced by F atoms. R 6 is a structure containing a glycidyl ester group, R 7 is an auxiliary group, which is one or more of an alkyl group, an aromatic group, and an alicyclic group, a, b, c, d are integers from 1 to 500 respectively; The molecular weight of the fluorine-containing resin is 2,000 to 35,000.
2. A synthesis process of fluorine-containing resin for making pixel bank layer, characterized in that: The following steps are involved: (1) mixing monomers and a free radical initiator to obtain a mixed solution, wherein the monomers include fluorine-containing monomers, carboxyl-containing monomers, epoxy-containing monomers and other monomers, wherein the molar proportion of the fluorine-containing monomer in the monomers is 5 to 40%, the molar proportion of the carboxyl-containing monomer is 5 to 20%, the molar proportion of the epoxy-containing monomer is 20 to 60%, and the molar proportion of other monomers is 0 to 30%; and the mass of the free radical initiator is 0.5 to 2.5% of the total amount of the monomers; (2) Slowly adding the mixed solution dropwise into an ether ester solvent to carry out a free radical polymerization reaction to obtain a finished product.
3. The synthesis process of fluorine-containing resin for making pixel bank layer according to claim 2, characterized in that: The fluorine-containing monomer is one or more of tetrafluoropropyl acrylate, tetrafluoropropyl methacrylate, hexafluorobutyl acrylate, hexafluorobutyl methacrylate, octafluoropentyl acrylate, octafluoropentyl methacrylate, dodecafluoroheptyl acrylate, dodecafluoroheptyl methacrylate, tridecafluorooctyl acrylate, tridecafluorooctyl methacrylate, trifluorohydroxyethyl acrylate or trifluorohydroxyethyl methacrylate.
4. The synthesis process of fluorine-containing resin for making pixel bank layer according to claim 2, characterized in that: The carboxyl group-containing monomer is one or more of acrylic acid and methacrylic acid.
5. The synthesis process of fluorine-containing resin for making pixel bank layer according to claim 2, characterized in that: The epoxy group-containing monomer is one or more of glycidyl methacrylate, glycidyl acrylate, 3,4-epoxycyclohexyl methyl methacrylate, and 3,4-epoxycyclohexyl methyl acrylate.
6. The synthesis process of fluorine-containing resin for making pixel bank layer according to claim 2, characterized in that: The other monomers are auxiliary monomers, including one or more of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, n-octyl acrylate, n-octyl methacrylate, isooctyl acrylate, isooctyl methacrylate, dodecyl acrylate, dodecyl methacrylate, tetradecyl acrylate, tetradecyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, n-decyl acrylate, n-decyl methacrylate, isodecyl acrylate, isodecyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, benzyl acrylate, benzyl methacrylate, isobornyl acrylate, isobornyl methacrylate, dicyclopentanyl acrylate, dicyclopentanyl methacrylate or maleic anhydride.
7. A fluorine-containing resin composition for making a pixel bank layer containing the fluorine-containing resin according to claim 1, characterized in that: The invention comprises the following raw materials in percentage by weight: 20 to 80% of fluorine-containing resin, 10 to 70% of photopolymerizable compound, and 5 to 15% of photopolymerization initiator.
8. The fluorine-containing resin composition for making a pixel bank layer according to claim 7, characterized in that: The raw materials are dissolved in a polar solvent or a diluent monomer to form a composition solution with a solid mass fraction of 5 to 60%.
9. The fluorine-containing resin composition for making a pixel bank layer according to claim 7, characterized in that: The photopolymerizable compound is one or more of methyl acrylate, methyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2-ethylene glycol acrylate, ethylene glycol methacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, tetraethylene glycol dimethacrylate, propylene glycol diacrylate, propylene glycol dimethacrylate, trimethylolpropane triacrylate, tetra(trimethylolpropane)tetraacrylate, tetra(trimethylolpropane)tetramethacrylate, pentaerythritol monoacrylate, pentaerythritol monomethacrylate, pentaerythritol tetraacrylate, pentaerythritol tetramethacrylate, polydipentaerythritol pentaacrylate, polydipentaerythritol pentamethacrylate, polydipentaerythritol hexaacrylate, polydipentaerythritol hexamethacrylate, and 1,6-hexanediol diacrylate.
10. The fluorine-containing resin composition for making a pixel bank layer according to claim 7, characterized in that: The photopolymerization initiator is an oxime ester photoinitiator, and its general formula is: The molecular formula of X is R 8 is phenyl, C1-C20 alkyl, -CN, -NO2 or C1-C4 haloalkyl, R 9 is a C2-C12 alkyl group or a C4-C8 acyl group, R 10 -R 14 is H, a halogen atom, a C1-C12 alkyl group, a phenyl group or C6H5S-, R 15 , R 16 is H, a halogen atom, a C1-C12 alkyl group or a phenyl group.
Citation Information
Patent Citations
Fluorine-containing epoxy acrylate oligomer for photo-curing and synthetic method thereof
CN103012660A
Light-cured resin composition and application thereof
CN109459914A