Noctilucent warning antiskid adhesive tape
By using the composite base material layer structure and the reflective effect of the aluminum-plated PET film layer in the luminous warning tape, the problems of low light absorption and energy storage efficiency and insufficient wear resistance and anti-skid performance are solved, and the luminous tape can achieve rapid light absorption and energy storage and long-term Glows out, improving the nighttime warning effect.
Patent Information
- Application Number
- CN202410875484.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing luminous warning tapes are inefficient in light absorption and energy storage, and have insufficient wear resistance and anti-slip properties, which are prone to safety hazards, especially when used on safety stairs.
It adopts a composite substrate layer structure, including surface coating, light-transmitting layer, luminous layer, reflective isolation layer and elastic foam layer. It accelerates light absorption and energy storage through the reflection of the aluminized PET film layer, and improves the energy storage through modified ceramsite sand. Anti-slip properties.
The luminous tape achieves rapid light absorption and energy storage and long-term luminescence, improves wear resistance and anti-slip properties, and ensures better warning effects at night.
Smart Images

Figure CN118853006A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of warning tapes, and in particular to a luminous warning anti-slip tape. Background Art
[0002] With the development of economy and the progress of science and technology, China has become a major processing manufacturer and consumer in the world's adhesive industry. Luminous tape is a kind of tape that can store light. When there is light, it absorbs light energy and stores it. When the light is dim, it naturally releases the stored light energy, thus producing a luminous effect. It can be recycled indefinitely. Luminous tape is widely used in the safety signs of public places such as subway stations, underground passages, airports, docks, and cinemas. Its location can be clearly marked at night or in the event of a power outage, which is convenient for operation and use, and plays a role in safety warning and guiding escape.
[0003] The existing luminous adhesive tapes are usually composed of two parts: a base material and a binder, and two or more unconnected objects are connected together through bonding. The luminous warning tapes on the market usually only rely on the luminous layer on the surface to absorb light, resulting in insufficient light absorption by the luminous tape within a limited time, and the disadvantage of slow light absorption and energy storage. At the same time, the existing luminous warning tapes have insufficient wear resistance and anti-slip properties, especially the luminous warning tapes used for safety stairs, which are prone to safety hazards when the anti-slip performance is insufficient.
[0004] In summary, the development of a luminous warning anti-slip tape is still a key issue that needs to be urgently addressed in the field of warning tape technology. Summary of the invention
[0005] In view of the problems existing in the prior art, the object of the present invention is to provide a luminous warning anti-slip tape.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A luminous warning anti-skid tape comprises an adhesive layer, a release layer is arranged on the lower surface of the adhesive layer, and a composite substrate layer is arranged on the upper surface of the adhesive layer, the composite substrate layer comprises a surface coating, a light-transmitting layer, a luminous layer, a reflective isolation layer, an elastic foam layer, a primer layer and a base film layer, and the surface coating comprises the following components in parts by weight: 100-200 parts of polyester polyol, 50-200 parts of hydroxyl acrylic resin, 200-450 parts of pigments and fillers, 10-20 parts of additives, 100-200 parts of modified ceramsite sand, 10-150 parts of nano oxide particles, 10-200 parts of nano particle luminous powder and 80-200 parts of deionized water.
[0008] The present invention is further configured as follows: the auxiliary agent includes one or more of a diluent, an aliphatic polyisocyanate curing agent, a accelerator, an anti-settling agent, an antistatic agent, a dispersant, a defoaming agent, an antioxidant, a leveling agent, a coupling agent, a bactericidal preservative, a foaming agent, a flame retardant, a film-forming agent and a thickener.
[0009] The present invention is further configured as follows: the adhesive layer is a pressure-sensitive adhesive, and the thickness of the adhesive layer is 85-100 μm; the light-transmitting layer is a transparent PET film layer, and the thickness of the light-transmitting layer is 15-30 μm.
[0010] The present invention is further configured as follows: the thickness of the luminous layer is 110-120 μm, the reflective isolation layer is an aluminized PET film layer, and the aluminized PET film layer includes a PET film layer and an aluminum layer on its upper surface, and the thickness of the reflective isolation layer is 20-25 μm.
[0011] The present invention is further configured as follows: the nano oxide particles are a mixture of hafnium oxide, silicon oxide, zirconium oxide and titanium oxide in a mass ratio of 2-4:1:1-3:1-5, and the release layer includes the following components in parts by weight: 1-3 parts of a non-silicone oil release agent, 0.1-0.3 parts of a cross-linking agent, 0.1-0.2 parts of an adhesion additive, 0.1-0.4 parts of a release force regulator and 90-95 parts of a solvent.
[0012] The present invention is further configured as follows: the elastic foam layer comprises the following components by weight: 20-35 parts of polyethylene glycol butylene adipate, 5-15 parts of diethylene glycol, 20-30 parts of 1,4-bis(isocyanate methyl)cyclohexane, 10-35 parts of polytetramethylene ether glycol, 30-55 parts of propylene oxide-ethylene oxide copolyether triol, 0.5-1 parts of catalyst, 0.2-1 parts of foaming agent and 0.2-2 parts of flame retardant.
[0013] A method for preparing a luminous warning anti-slip tape comprises the following steps:
[0014] S1. Prepare release layer slurry, adhesive layer slurry and composite substrate layer slurry according to the formula, wherein the composite substrate layer slurry includes surface coating slurry, light-transmitting layer slurry, luminous layer slurry, reflective isolation layer slurry, elastic foam layer slurry, primer layer slurry and base film layer slurry, and prepare the required base film through the base film layer slurry;
[0015] S2, coating the base coating slurry on the surface of the base film, and then coating the elastic foam layer slurry, the reflective isolation layer slurry, the luminous layer slurry and the light-transmitting layer slurry in sequence after drying, and finally compounding the surface coating slurry to obtain a semi-finished base film;
[0016] S3, coating the adhesive layer slurry on the surface of the semi-finished base film, and finally compounding the release layer slurry, and obtaining the luminous warning tape after curing.
[0017] The present invention is further configured as follows: in step S1, the surface coating slurry is composed of three components A, B, and C, wherein component A is a mixture of polyester polyol, hydroxy acrylic resin, pigment, filler, additive, and solvent, component B is an aliphatic polyisocyanate curing agent, a reaction accelerator, and a solvent, and component C is modified ceramsite sand. The preparation of the surface coating slurry comprises the following steps:
[0018] F11. According to a certain formula, add hydroxy acrylic resin, dispersant and part of diluent into the material tank, disperse at high speed for 35 minutes, and continue to add pigments, fillers, antioxidants, defoamers, leveling agents and coupling agents into the material tank after uniform dispersion, disperse at high speed for 20 minutes, grind the dispersed materials with a sand mill until the fineness is less than 40μm, make up the remaining diluent in the formula, disperse at high speed for 20 minutes, and obtain component A after uniform dispersion;
[0019] F12. Add aliphatic polyisocyanate curing agent, accelerator and diluent into the material tank according to a certain formula, and disperse at high speed for 25 minutes to make the dispersion uniform to obtain component B;
[0020] F13. Mix components A, B and C in a certain mass ratio to obtain a surface coating slurry.
[0021] Beneficial Effects
[0022] Compared with the known public technology, the technical solution provided by the present invention has the following advantages:
[0023] Beneficial effects:
[0024] (1) In the present invention, a light-transmitting layer, a luminous layer and a reflective isolation layer are provided, wherein the luminous layer is located between the light-transmitting layer and the reflective isolation layer, and the reflective isolation layer is an aluminum-plated PET film layer. The aluminum foil in the reflective isolation layer has a very strong reflective effect. When the adhesive tape absorbs light, part of the light reaches the reflective isolation layer and is reflected back by the reflection effect of the aluminum foil, so that the bottom of the luminous layer can also absorb light, thereby accelerating the light absorption and energy storage process. At the same time, when the luminous layer emits light, it can also reflect light to prevent light from passing through the reflective isolation layer and causing a decrease in brightness. The reflective isolation layer can also prevent the luminous layer material and the glue from penetrating each other and destroying the luminous effect and the cohesive properties of the glue, thereby making the light absorption and energy storage of the adhesive tape better. Under the premise that the tensile strength is still maintained, the adhesive tape absorbs light quickly, stores energy quickly, and emits brighter and longer light, thereby achieving a better warning effect at night.
[0025] (2) In the present invention, the surface coating is prepared by a surface coating slurry, polyester polyol, hydroxy acrylic resin, pigment filler, additive and solvent are mixed into component A, aliphatic polyisocyanate curing agent, reaction accelerator and solvent are mixed into component B, and component C uses modified ceramsite sand with a particle size of 250 to 380 μm as anti-skid particles, and the addition amount is 12%. The finally obtained surface coating slurry has the characteristics of low surface density, strong wear resistance, large maximum static friction coefficient and good adhesion; the tape made of the surface coating slurry improves the wear resistance and anti-skid performance of the luminous warning tape. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a structural schematic diagram of a luminous warning anti-slip tape;
[0027] Figure 2 The figure is a schematic diagram of the structure of a composite substrate layer of a luminous warning anti-slip tape.
[0028] In the figure:
[0029] 1. Release layer; 2. Adhesive layer; 3. Composite substrate layer; 31. Surface coating; 32. Light-transmitting layer; 33. Luminous layer; 34. Reflective isolation layer; 35. Elastic foam layer; 36. Primer layer; 37. Base film layer. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The present invention will be further described below in conjunction with the embodiments.
[0032] Example 1
[0033] Please refer to Figure 1 and Figure 2As shown, a luminous warning anti-slip tape comprises an adhesive layer 2, a release layer 1 is arranged on the lower surface of the adhesive layer 2, and a composite substrate layer 3 is arranged on the upper surface of the adhesive layer 2, the composite substrate layer 3 comprises a surface coating 31, a light-transmitting layer 32, a luminous layer 33, a reflective isolation layer 34, an elastic foam layer 35, a primer layer 36 and a base film layer 37, the adhesive layer 2 is a pressure-sensitive adhesive, and the thickness of the adhesive layer 2 is 85-100 μm, the light-transmitting layer 32 is a transparent PET film layer, and the thickness of the light-transmitting layer 32 is The thickness of the luminous layer 33 is 110-120 μm, the reflective isolation layer 34 is an aluminized PET film layer, and the aluminized PET film layer includes the PET film layer and the aluminum layer on its upper surface, and the thickness of the reflective isolation layer 34 is 20-25 μm; the surface coating 31 includes the following components in parts by weight: 150 parts of polyester polyol, 100 parts of hydroxyl acrylic resin, 300 parts of pigments and fillers, 15 parts of additives, 150 parts of modified ceramsite sand, 60 parts of nano oxide particles, 100 parts of nano-particle luminous powder and 100 parts of deionized water; the auxiliary agent includes one or more of a diluent, an aliphatic polyisocyanate curing agent, a accelerator, an anti-settling agent, an antistatic agent, a dispersant, a defoaming agent, an antioxidant, a leveling agent, a coupling agent, a bactericidal preservative, a foaming agent, a flame retardant, a film-forming agent and a thickener; the nano-oxide particles are a mixture of hafnium oxide, silicon oxide, zirconium oxide and titanium oxide in a mass ratio of 2:1:2:3, and the release layer 1 includes the following components in parts by weight: 2 1. The elastic foam layer 35 comprises the following components by weight: 25 parts of polyethylene adipate butanediol, 10 parts of diethylene glycol, 25 parts of 1,4-bis(isocyanate methyl)cyclohexane, 20 parts of polytetramethylene ether glycol, 40 parts of propylene oxide-ethylene oxide copolyether triol, 0.7 parts of catalyst, 0.5 parts of foaming agent and 1 part of flame retardant;
[0034] A method for preparing a luminous warning anti-slip tape comprises the following steps:
[0035] Step 1: prepare release layer slurry, adhesive layer slurry and composite substrate layer slurry according to the formula, wherein the composite substrate layer slurry includes surface coating slurry, light-transmitting layer slurry, luminous layer slurry, reflective isolation layer slurry, elastic foam layer slurry, primer layer slurry and base film layer slurry, and prepare the required base film through the base film layer slurry;
[0036] The surface coating slurry is composed of three components, namely, A, B and C. Component A is a mixture of polyester polyol, hydroxy acrylic resin, pigment, filler, additive and solvent; component B is an aliphatic polyisocyanate curing agent, a reaction accelerator and a solvent; and component C is modified ceramsite sand. The preparation of the surface coating slurry comprises the following steps:
[0037] 11) According to a certain formula, add hydroxy acrylic resin, dispersant and part of diluent into the material tank, disperse at high speed for 35 minutes, and continue to add pigments, fillers, antioxidants, defoamers, leveling agents and coupling agents into the material tank after uniform dispersion, disperse at high speed for 20 minutes, grind the dispersed materials with a sand mill to a fineness of less than 40 μm, make up the remaining diluent in the formula, disperse at high speed for 20 minutes, and obtain component A after uniform dispersion;
[0038] 12) Add aliphatic polyisocyanate curing agent, accelerator and diluent into the material tank according to a certain formula, and disperse at high speed for 25 minutes to make the dispersion uniform to obtain component B;
[0039] 13) Components A, B and C are uniformly mixed in a certain mass ratio to obtain a surface coating slurry.
[0040] Step 2: Apply the primer slurry on the surface of the base film, and then apply the elastic foam layer slurry, reflective isolation layer slurry, luminous layer slurry and light-transmitting layer slurry in sequence after drying, and finally compound the surface coating slurry to obtain a semi-finished base film.
[0041] Step 3: Coat the surface of the semi-finished base film with an adhesive layer slurry, and finally compound the release layer slurry, and obtain the luminous warning tape after curing.
[0042] Example 2
[0043] The luminous warning anti-skid tape and its preparation method provided in this embodiment are roughly the same as those in embodiment 1, and the main difference is that the surface coating 31 includes the following components in parts by weight: 100 parts of polyester polyol, 50 parts of hydroxy acrylic resin, 200 parts of pigments and fillers, 10 parts of additives, 100 parts of modified ceramsite sand, 10 parts of nano-oxide particles, 10 parts of nano-particle luminous powder and 80 parts of deionized water; the nano-oxide particles are a mixture of hafnium oxide, silicon oxide, zirconium oxide and titanium oxide in a mass ratio of 3:1:2:5, and the release layer 1 comprises the following components in parts by weight: 1 part of a non-silicone release agent, 0.1 part of a cross-linking agent, 0.1 part of an adhesion additive, 0.1 part of a release force regulator and 90 parts of a solvent; the elastic foam layer 35 comprises the following components in parts by weight: 20 parts of polyethylene adipate butanediol, 5 parts of diethylene glycol, 20 parts of 1,4-bis(isocyanatemethyl)cyclohexane, 10 parts of polytetramethylene ether glycol, 30 parts of propylene oxide-ethylene oxide copolyether triol, 0.5 parts of a catalyst, 0.2 parts of a blowing agent and 0.2 parts of a flame retardant.
[0044] Example 3
[0045] The luminous warning anti-skid tape and its preparation method provided in this embodiment are roughly the same as those in embodiment 1, with the main difference being that the surface coating 31 comprises the following components in parts by weight: 200 parts of polyester polyol, 200 parts of hydroxy acrylic resin, 450 parts of pigments and fillers, 20 parts of additives, 200 parts of modified ceramsite sand, 150 parts of nano-oxide particles, 200 parts of nano-particle luminous powder and 200 parts of deionized water; the nano-oxide particles are a mixture of hafnium oxide, silicon oxide, zirconium oxide and titanium oxide in a mass ratio of 2:1:1:5. The release layer 1 includes the following components in parts by weight: 3 parts of non-silicone release agent, 0.3 parts of cross-linking agent, 0.2 parts of adhesion additive, 0.4 parts of release force regulator and 95 parts of solvent; the elastic foam layer 35 includes the following components in parts by weight: 35 parts of polyethylene adipate butanediol, 15 parts of diethylene glycol, 30 parts of 1,4-bis(isocyanate methyl)cyclohexane, 35 parts of polytetramethylene ether glycol, 55 parts of propylene oxide-ethylene oxide copolyether triol, 1 part of catalyst, 2 parts of foaming agent and 1 part of flame retardant.
[0046] Comparative Example 1
[0047] The luminous warning anti-skid tape and its preparation method provided in this embodiment are substantially the same as those in Embodiment 1, with the main difference being that no surface coating 31 is added.
[0048] Comparative Example 2
[0049] The luminous warning anti-slip tape and its preparation method provided in this embodiment are substantially the same as those in Embodiment 1, with the main difference being that no nano oxide particles are added.
[0050] Comparative Example 3
[0051] The luminous warning anti-skid tape and its preparation method provided in this embodiment are substantially the same as those in Embodiment 1, with the main difference being that no hydroxyl acrylic resin is added.
[0052] Performance Testing
[0053] The luminous warning anti-skid tapes prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were taken, and the relevant properties of the prepared luminous warning anti-skid tapes were tested; the dynamic friction coefficient of the luminous warning anti-skid tape was tested according to GLB 8613; the wear rate of the luminous warning anti-skid tape was tested according to GB / T 3960-2016; the adhesion of the easy-to-clean coating on the surface of the luminous warning anti-skid tape was tested according to GB / T 9286-1998; the release force of the release layer of the luminous warning anti-skid tape was tested according to GB / T 2792-2014; the obtained test results were recorded in Table 1;
[0054] Table 1 Luminous warning anti-slip tape test table
[0055]
[0056]
[0057] By analyzing the relevant data in the above table, it can be seen that by adding a surface coating 31 and using a tape made of a surface coating slurry, the wear resistance and anti-skid performance of the luminous warning tape can be effectively improved; in the present invention, the luminous warning anti-skid tape is composed of a release layer 1, an adhesive layer 2 and a composite substrate layer 3, wherein the composite substrate layer 3 is composed of a surface coating 31, a light-transmitting layer 32, a luminous layer 33, a reflective isolation layer 34, an elastic foam layer 35, a primer layer 36 and a base film layer 37;
[0058] The luminous layer 33 is located between the light-transmitting layer 32 and the reflective isolation layer 34. The thickness of the light-transmitting layer 32 is reduced, and light can more easily pass through the light-transmitting layer 32 to reach the luminous layer 33. At the same time, the reflective isolation layer 34 is added to the structure of the entire tape to compensate for the tensile strength of the tape, so that the overall tensile strength is not affected. The reflective isolation layer 34 is an aluminized PET film layer (the aluminized PET film layer is corona treated, and the aluminized PET film layer includes a PET film layer and an aluminum layer on its upper surface. The PET film layer is used for isolation, and the aluminum layer is used to increase the reflective effect. The corona treatment increases the surface adhesion). The aluminum foil has a very strong reflective effect. When the tape absorbs light, part of the light reaches the reflective isolation layer 34, and the light is reflected back by the aluminum foil, so that the bottom of the luminous layer 33 can also absorb light, which speeds up the light absorption and energy storage process. At the same time, it can also reflect light when the luminous layer 33 emits light, preventing the light from passing through the reflective isolation layer 34 and causing the brightness to decrease. The reflective isolation layer 34 can also prevent the luminous layer 33 material and the glue from penetrating each other, destroying the luminous effect and the cohesive performance of the glue; thus, the tape absorbs light and stores energy better. Under the premise that the tensile strength is still maintained, the tape absorbs light quickly, stores energy quickly, and emits brighter and longer light.
[0059] At the same time, a surface coating 31 is prepared by a surface coating slurry, wherein polyester polyol, hydroxy acrylic resin, pigment filler, additive and solvent are mixed into component A, aliphatic polyisocyanate curing agent, reaction accelerator and solvent are mixed into component B, and component C uses modified expanded clay sand with a particle size of 250 to 380 μm as anti-slip particles, and the addition amount is 12%. The final surface coating slurry has the characteristics of low surface density, strong wear resistance, large maximum static friction coefficient and good adhesion. The tape made of the surface coating slurry improves the wear resistance and anti-slip properties of the luminous warning tape.
[0060] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A luminous warning anti-slip tape, characterized in that: The invention comprises an adhesive layer (2), wherein a release layer (1) is arranged on the lower surface of the adhesive layer (2), and a composite substrate layer (3) is arranged on the upper surface of the adhesive layer (2), wherein the composite substrate layer (3) comprises a surface coating (31), a light-transmitting layer (32), a luminous layer (33), a reflective isolation layer (34), an elastic foam layer (35), a primer layer (36) and a base film layer (37), wherein the surface coating (31) comprises the following components in parts by weight: 100-200 parts of polyester polyol, 50-200 parts of hydroxyl acrylic resin, 200-450 parts of pigments and fillers, 10-20 parts of additives, 100-200 parts of modified ceramsite sand, 10-150 parts of nano oxide particles, 10-200 parts of nano particle luminous powder and 80-200 parts of deionized water.
2. The luminous warning anti-slip tape according to claim 1, characterized in that: The auxiliary agent includes one or more of a diluent, an aliphatic polyisocyanate curing agent, a accelerator, an anti-settling agent, an antistatic agent, a dispersant, a defoaming agent, an antioxidant, a leveling agent, a coupling agent, a bactericidal preservative, a foaming agent, a flame retardant, a film former and a thickener.
3. The luminous warning anti-slip tape according to claim 1, characterized in that: The adhesive layer (2) is a pressure-sensitive adhesive, and the thickness of the adhesive layer (2) is 85-100 μm; the light-transmitting layer (32) is a transparent PET film layer, and the thickness of the light-transmitting layer (32) is 15-30 μm.
4. The luminous warning anti-slip tape according to claim 1, characterized in that: The luminous layer (33) has a thickness of 110-120 μm, the reflective isolation layer (34) is an aluminum-plated PET film layer, and the aluminum-plated PET film layer includes a PET film layer and an aluminum layer on its upper surface, and the reflective isolation layer (34) has a thickness of 20-25 μm.
5. The luminous warning anti-slip tape according to claim 1, characterized in that: The nano oxide particles are a mixture of hafnium oxide, silicon oxide, zirconium oxide and titanium oxide in a mass ratio of 2-4:1:1-3:1-5, and the release layer (1) comprises the following components in parts by weight: 1-3 parts of a non-silicone oil release agent, 0.1-0.3 parts of a cross-linking agent, 0.1-0.2 parts of an adhesion additive, 0.1-0.4 parts of a release force regulator and 90-95 parts of a solvent.
6. The luminous warning anti-slip tape according to claim 1, characterized in that: The elastic foam layer (35) comprises the following components by weight: 20-35 parts of polyethylene glycol butylene adipate, 5-15 parts of diethylene glycol, 20-30 parts of 1,4-bis(isocyanate methyl)cyclohexane, 10-35 parts of polytetramethylene ether glycol, 30-55 parts of propylene oxide-ethylene oxide copolyether triol, 0.5-1 parts of catalyst, 0.2-1 parts of foaming agent and 0.2-2 parts of flame retardant.
7. A method for preparing a luminous warning anti-slip tape, characterized in that: A luminous warning anti-slip tape according to any one of claims 1 to 6 is used, comprising the following steps: S1. Prepare release layer slurry, adhesive layer slurry and composite substrate layer slurry according to the formula, wherein the composite substrate layer slurry includes surface coating slurry, light-transmitting layer slurry, luminous layer slurry, reflective isolation layer slurry, elastic foam layer slurry, primer layer slurry and base film layer slurry, and prepare the required base film through the base film layer slurry; S2, coating the base coating slurry on the surface of the base film, and then coating the elastic foam layer slurry, the reflective isolation layer slurry, the luminous layer slurry and the light-transmitting layer slurry in sequence after drying, and finally compounding the surface coating slurry to obtain a semi-finished base film; S3, coating the adhesive layer slurry on the surface of the semi-finished base film, and finally compounding the release layer slurry, and obtaining the luminous warning tape after curing.
8. The method for preparing the luminous warning anti-slip tape according to claim 7, characterized in that: In step S1, the surface coating slurry is composed of three components A, B, and C. Component A is a mixture of polyester polyol, hydroxy acrylic resin, pigment, filler, additive and solvent, component B is an aliphatic polyisocyanate curing agent, a reaction accelerator and a solvent, and component C is modified ceramsite sand. The preparation of the surface coating slurry includes the following steps: F11. According to a certain formula, add hydroxy acrylic resin, dispersant and part of diluent into the material tank, disperse at high speed for 35 minutes, and continue to add pigments, fillers, antioxidants, defoamers, leveling agents and coupling agents into the material tank after uniform dispersion, disperse at high speed for 20 minutes, grind the dispersed materials with a sand mill until the fineness is less than 40μm, make up the remaining diluent in the formula, disperse at high speed for 20 minutes, and obtain component A after uniform dispersion; F12. Add aliphatic polyisocyanate curing agent, accelerator and diluent into the material tank according to a certain formula, and disperse at high speed for 25 minutes to make the dispersion uniform to obtain component B; F13. Mix components A, B and C in a certain mass ratio to obtain a surface coating slurry.