OLED flexible screen manufacturing process protective film and preparation method thereof

By using modified nanocellulose and graphene oxide in the OLED flexible screen protective film to enhance the tensile strength of the polyurethane pressure-sensitive adhesive, and preparing the microstructure base material layer through the molding method, the problem of the protective film being easily broken is solved and the Screen quality and productivity.

CN118853017APending Publication Date: 2024-10-29JIANGSU TOPFLY NEW MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410860796.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing OLED flexible screen protective films are easily broken when attached and removed, resulting in residual glue residue and affecting screen quality and production efficiency.

Method used

Components such as modified nanocellulose and graphene oxide are used to enhance the tensile strength of polyurethane pressure-sensitive adhesive, and a base material layer with a certain microstructure is prepared by molding method, and combined with drying and curing treatments to form a tight protective film.

Benefits of technology

It improves the tensile strength of the protective film, reduces the residual glue residue, improves the appearance quality and yield rate of the OLED screen, improves the light transmittance, and reduces the risk of damage during the production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004919144820000061
    Figure BDA0004919144820000061
  • Figure BDA0004919144820000071
    Figure BDA0004919144820000071
Patent Text Reader

Abstract

The invention relates to the technical field of protective films, and particularly discloses an OLED flexible screen manufacturing process protective film and a preparation method thereof. The OLED flexible screen manufacturing process protective film comprises a base material layer, an adhesive layer and a release layer, the adhesive layer is prepared from a polyurethane pressure-sensitive adhesive, and the polyurethane pressure-sensitive adhesive comprises the following components in parts by weight: 100-105 parts of polyurethane masterbatch, 40-45 parts of a polyurethane monomer, 25-27 parts of a curing agent, 12-15 parts of an auxiliary agent, 8-12 parts of modified nanocellulose and 2.6-4.4 parts of graphene oxide. Compared with the prior art, the OLED flexible screen manufacturing process protective film has the advantages that residual glue is not easy to generate when the OLED flexible screen manufacturing process protective film is torn off from the surface of an OLED screen, so that the influence on the appearance quality of the OLED screen is relatively small, the damage of the OLED screen in the production and processing process is reduced, and the yield of the OLED screen is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of protective films, and more specifically, to an OLED flexible screen process protective film and a preparation method thereof. Background Art

[0002] With the continuous advancement of display technology, OLED (organic light-emitting diode) has become a hot technology in the display field due to its high contrast, low power consumption and flexible display. OLED flexible screens are widely used in smart wearable devices, folding mobile phones and other fields due to their thin and bendable characteristics. However, in the production process of OLED flexible screens, the screen surface is extremely susceptible to scratches, pollution and other damages, which not only affects the quality of the product, but also increases the production cost. Therefore, the development of a protective film suitable for OLED flexible screens is of great significance to improving production efficiency and product quality.

[0003] At present, there are some problems with the traditional OLED screen protective film on the market, such as loose fit when attached to the OLED flexible screen, insufficient light transmittance, possible damage to the screen when removed, easy to cause bubbles, affecting the screen quality, etc. In the related technology, there is a protective film, which is composed of a substrate layer, an adhesive layer and a release layer from top to bottom. The substrate layer is a 75μm single-sided antistatic PET, the thickness of the adhesive layer is 75μm, and it is processed by a polyurethane pressure-sensitive adhesive layer; the release layer is a silicone double-sided antistatic release film with a thickness of 25μm.

[0004] With regard to the above-mentioned related technologies, the inventor believes that the adhesive layer in the related technologies is relatively thick, and the tensile strength of the polyurethane pressure-sensitive adhesive is limited, so it is easy to break when the protective film is torn off. The broken adhesive layer will produce residual adhesive on the surface of the OLED screen, which affects the appearance quality of the OLED screen and easily causes damage to the OLED screen. Summary of the invention

[0005] In the related art, the adhesive layer is prone to breakage, and the residual adhesive produced by the breakage will cause damage to the OLED screen. In order to improve this defect, the present application provides an OLED flexible screen process protective film and a preparation method thereof.

[0006] In the first aspect, the present application provides an OLED flexible screen process protective film, which adopts the following technical solution: an OLED flexible screen process protective film, comprising a substrate layer, an adhesive layer and a release layer, wherein the adhesive layer is bonded to the surface of the substrate layer, and the release layer is attached to the surface of the adhesive layer; the material of the substrate layer comprises PET, and the adhesive layer is made of a polyurethane pressure-sensitive adhesive, and the polyurethane pressure-sensitive adhesive comprises the following components in parts by weight: 100-105 parts of a polyurethane masterbatch, 40-45 parts of a polyurethane monomer, 25-27 parts of a curing agent, 12-15 parts of an auxiliary agent, 8-12 parts of modified nanocellulose, and 2.6-4.4 parts of graphene oxide; The modified nanocellulose is prepared by heating diisocyanate, adding an organic base catalyst to the diisocyanate, and then adding nanocellulose. -1 The reaction is terminated when the isocyanate groups at the reaction site disappear, thereby obtaining a mixed solution; the mixed solution is washed with an organic solvent, and the modified nanocellulose is obtained after centrifugal separation.

[0007] By adopting the above technical solution, the present application modifies nanocellulose by diisocyanate, and obtains modified nanocellulose with good dispersibility in the polyurethane system, and the modified nanocellulose, graphene oxide, and polyurethane can form strong hydrogen bonds with each other. The formation of hydrogen bonds improves the binding force between polyurethane molecules, so that the tensile strength of the polyurethane pressure-sensitive adhesive is improved. Due to the improvement of the tensile strength of the polyurethane pressure-sensitive adhesive, the OLED flexible screen process protective film of the present application is not easy to produce residual glue when it is peeled off from the surface of the OLED screen, so the impact on the appearance quality of the OLED screen is relatively small, reducing the damage to the OLED screen during the production and processing process, and improving the yield rate of the OLED screen.

[0008] Preferably, in the method for preparing the modified nanocellulose, the organic base catalyst selected is a DABCO catalyst.

[0009] By adopting the above technical solution, the present application optimizes the specific type of organic base catalyst, which helps to achieve the modification of nanocellulose.

[0010] Preferably, the amount of the organic base catalyst is 0.7-0.9% of the weight of the nanocellulose.

[0011] By adopting the above technical solution, the present application optimizes the dosage of the organic base catalyst, which helps to achieve the modification of nanocellulose.

[0012] Preferably, the substrate layer is prepared according to the following method: (1) mixing LDPE, AC foaming agent and dicumyl peroxide and kneading them to obtain a foaming agent substrate for standby use; (2) The PET sheet and the foaming agent substrate are mixed and added to a molding machine, and then preheated to a processing temperature. The temperature is kept at the processing temperature and a molding process is performed for 270-310 seconds to obtain a substrate layer.

[0013] By adopting the above technical solution, the present application first prepares a foaming agent containing an AC foaming agent, and then mixes the foaming agent substrate and the PET sheet for molding. During the molding process, the AC foaming agent is decomposed by heat and pores are generated on the surface of the PET sheet, and finally a substrate layer with a certain microstructure on the surface is obtained. The microstructure on the surface of the substrate layer can improve the light transmittance of the protective film and reduce the impact of the manufacturing process on the OLED screen.

[0014] Preferably, in the step (2) of preparing the substrate layer, the processing temperature is set at 190-200°C.

[0015] By adopting the above technical solution, the present application optimizes the processing temperature of the molding process, and can realize the foaming process of the PET sheet.

[0016] Preferably, in step (2) of preparing the substrate layer, the pressure condition is set to 20-22 MPa.

[0017] By adopting the above technical solution, the present application optimizes the pressure conditions of the molding process, and the foaming process of the PET sheet can be achieved under the above pressure conditions.

[0018] Preferably, the preheating time of the foaming agent substrate is 220-250s.

[0019] By adopting the above technical solution, the present application optimizes the preheating time of the foaming agent substrate, which can fully realize the foaming processing of the PET sheet.

[0020] Preferably, the auxiliary agent comprises modified halloysite nanotubes, which are prepared as follows: MDI and halloysite nanotubes are mixed in a weight ratio of (19.8-20.6):1, then heated at 83-85°C for 180-185min, and the modified halloysite nanotubes are obtained after centrifugal separation and washing.

[0021] By adopting the above technical solution, the present application uses MDI to treat the halloysite nanotubes, and obtains modified halloysite nanotubes with good dispersibility in the polyurethane system. The modified halloysite nanotubes can form hydrogen bonds with modified nanocellulose, graphene oxide, and polyurethane, which can further improve the tensile strength of the polyurethane pressure-sensitive adhesive, help reduce the amount of residual glue on the surface of the OLED screen, and improve the yield rate of the OLED screen.

[0022] Preferably, the weight of the modified halloysite nanotubes is 0.5-0.7% of the weight of the polyurethane masterbatch.

[0023] By adopting the above technical solution, the present application optimizes the dosage of modified halloysite nanotubes, which helps to improve the tensile strength of the polyurethane pressure-sensitive adhesive.

[0024] In a second aspect, the present application provides a method for preparing an OLED flexible screen process protective film, which adopts the following technical solution.

[0025] A method for preparing an OLED flexible screen process protective film comprises the following steps: (1) mixing a polyurethane masterbatch, a polyurethane monomer, a curing agent, an auxiliary agent, and modified nanocellulose to obtain a polyurethane pressure-sensitive adhesive; (2) The polyurethane pressure-sensitive adhesive is coated on the surface of the substrate layer, dried at 80-120° C., then mixed with the release film, rolled up, and then aged at 45-65° C. for 30-35 minutes to obtain a protective film.

[0026] By adopting the above-mentioned technical scheme, the present application coats a polyurethane pressure-sensitive adhesive on the surface of the substrate layer, solidifies the polyurethane pressure-sensitive adhesive by drying to form an adhesive layer, and then composites a release film on the surface of the adhesive layer. After aging treatment, an OLED flexible screen process protective film can be obtained.

[0027] In summary, this application has the following beneficial effects: 1. The OLED flexible screen process protective film of the present application is not easy to produce residual glue when peeled off from the surface of the OLED screen, so the impact on the appearance quality of the OLED screen is relatively small, reducing the damage to the OLED screen during the production and processing process, and improving the yield rate of the OLED screen.

[0028] 2. The present application prepares a substrate layer with a certain microstructure on the surface by a molding method. The microstructure on the surface of the substrate layer can improve the light transmittance of the protective film and reduce the impact of the manufacturing process on the OLED screen.

[0029] 3. In the method of the present application, a polyurethane pressure-sensitive adhesive is coated on the surface of the substrate layer, the polyurethane pressure-sensitive adhesive is cured by drying to form an adhesive layer, a release film is then compounded on the surface of the adhesive layer, and an OLED flexible screen process protective film is obtained after a aging treatment. DETAILED DESCRIPTION

[0030] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially.

[0031] Preparation Example of Base Material Layer The following is an explanation using Preparation Example 1.

[0032] Preparation Example 1 In this preparation example, the density of LDPE is 0.925 g / cm 3 , the melt index is 2.1g / 10min; the CAS number of PET sheet is 25038-59-9.

[0033] In this preparation example, the substrate layer was prepared according to the following method: (1) Using a SK-160B double-roll mill, LDPE, AC foaming agent and dicumyl peroxide were mixed in a weight ratio of 70:25:5, and then mixed at 110° C. at a rate of 20 r / min for 60 min to obtain a foaming agent substrate for later use; (2) The PET sheet and the foaming agent substrate were mixed in a weight ratio of 85:15 and added to a molding machine, and then preheated for 220 seconds to reach a processing temperature of 190° C., and heat-insulating molding was performed for 270 seconds at a processing temperature of 190° C. and a pressure of 20 MPa, and then the pressure was released to obtain a substrate layer.

[0034] As shown in Table 1, the difference between Preparation Examples 1-3 lies in the different production and processing parameters of the substrate layer.

[0035] Table 1 Production and processing parameters of substrate layer sample Processing temperature / ℃ Pressure conditions / MPa Insulation time / s Warm-up time / s Preparation Example 1 190 20 270 220 Preparation Example 2 195 21 290 235 Preparation Example 3 200 22 310 250 Preparation example of modified halloysite nanotubes The following is an explanation using Preparation Example 4.

[0036] Preparation Example 4 In this preparation example, modified halloysite nanotubes were prepared according to the following method: MDI and halloysite nanotubes (CAS: 1332-58-7) were mixed in a weight ratio of 19.8:1 (referred to as the mixing ratio), and then heated at 83° C. for 180 min. The modified halloysite nanotubes were obtained after centrifugal separation and washing.

[0037] As shown in Table 2, the difference between Preparation Examples 4-6 is that the production and processing parameters of the modified halloysite nanotubes are different.

[0038] Table 2 Production and processing parameters of modified halloysite nanotubes sample Mixing ratio Heating temperature / ℃ Heating time / min Preparation Example 4 19.8:1 83 180 Preparation Example 5 20.2:1 84 182 Preparation Example 6 20.6:1 85 185 Example

[0039] Examples 1-5 The following description is given by taking Example 1 as an example.

[0040] Example 1 This embodiment provides an OLED flexible screen process protective film, including a substrate layer with a thickness of 75 μm, an adhesive layer with a thickness of 75 μm, and a release layer with a thickness of 25 μm. The adhesive layer is bonded to the surface of the substrate layer, and the release layer is attached to the surface of the adhesive layer. The substrate layer is prepared according to the method of Preparation Example 1, and the adhesive layer is made of a polyurethane pressure-sensitive adhesive, which includes the following components: 100 g of polyurethane masterbatch, 40 g of polyurethane monomer, 25 g of curing agent, 12 g of auxiliary agent, 8 g of modified nanocellulose, and 2.6 g of graphene oxide (Aladdin, CAS: 7782-42-5).

[0041] In the above formula, the polyurethane monomer is polycarbonate polyol (Ube Chemical, model PH200D), the curing agent is hexamethylene diisocyanate, the curing agent is added in the form of a solution with a solid content of 75%, the solvent is a mixture of toluene, butanone and ethyl acetate in a mass ratio of 1:1:2, and the weight of the solvent is not included in the ratio; the modified nanocellulose is prepared according to the method of Preparation Example 4; the auxiliary agent is an antistatic agent (Japan Guangrong, AS400, imine salts), a polyurethane ionomer, an antioxidant (BASF, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate]), and a wetting agent (isopropyl myristate) are compounded in a weight ratio of 1:2:4:8. The polyurethane masterbatch is prepared by mixing polyether polyol (Dow, model 2000LM), polycarbonate polyol (Ube Chemical, model PH100D), and polyester polyol (Asahikawa Chemical, model XCP 1000N) in a mass ratio of 20:70:10. The preparation method is as follows: (1) dissolving polyether polyol and polyester polyol in toluene, stirring well, adding hexamethylene diisocyanate and an organic tin catalyst, and carrying out a prepolymerization reaction at 75° C. under stirring; (2) After the prepolymerization reaction is completed, a mixture of polycarbonate polyol and toluene is added, and the temperature of the reaction system is raised to 90° C. The chain extension reaction is completed under stirring conditions, and ethyl acetate is added to prepare a polyurethane masterbatch with a solid content of 70%.

[0042] The preparation method of the polyurethane ionomer used in the additive is: (1) Add MDI solid and solvent DMA to a dry four-necked flask, stir and dissolve at 40°C; slowly drop a PTMEG solution containing 0.15wt% stannous octoate catalyst (solvent is DMA, concentration 50wt%) under nitrogen protection and stirring conditions, and continue to react at 65°C for 1h after the drop is complete. Then drop a DMPA solution in DMA within 5min; continue to react at 70°C for 1.5h and then cool, slowly pour the obtained polymer solution into distilled water for precipitation, wash to remove the solvent and small molecular reactants, and dry in a 70°C oven for 2d to obtain a PU elastomer containing pendant carboxyl groups; (2) Weigh a PU elastomer containing pendant carboxyl groups, add DMF to a four-necked flask to dissolve it to a concentration of 85 g / L; add a stoichiometric amount of NaH (with a molar ratio of 1:1 to the carboxyl groups in the PU elastomer containing pendant carboxyl groups) under ice-salt cooling, react for 1 hour under nitrogen protection, then add a stoichiometric amount of γ-propane sultone (with a molar ratio of 1:1 to the carboxyl groups in the PU elastomer containing pendant carboxyl groups), react at room temperature for 0.5 hours, then heat from room temperature to 60°C, react for 1 hour, cool, and then pour into acetone for precipitation, and obtain a polyurethane ionomer after vacuum drying.

[0043] The modified nanocellulose in the above formula is prepared according to the following method: 2,4-toluene diisocyanate is heated to 75°C, and then an organic base catalyst (DABCO catalyst) is added to the 2,4-toluene diisocyanate; the amount of the organic base catalyst is 0.7% of the weight of the nanocellulose (referred to as the catalyst amount); then the nanocellulose is added, and the infrared spectrum is monitored at 2270cm -1 The reaction is terminated when the isocyanate groups at the reaction site disappear, thereby obtaining a mixed solution; the mixed solution is washed with xylene, and the modified nanocellulose is obtained after centrifugal separation.

[0044] This embodiment provides a method for preparing an OLED flexible screen process protective film, comprising the following steps: (1) mixing a polyurethane masterbatch, a polyurethane monomer, a curing agent, an auxiliary agent, and modified nanocellulose to obtain a polyurethane pressure-sensitive adhesive; (2) The polyurethane pressure-sensitive adhesive is coated on the surface of the substrate layer, dried at 80° C., mixed with the release film, rolled up, and then aged at 45° C. for 30 minutes to obtain a protective film.

[0045] As shown in Table 3, the main differences between Examples 1-5 are that the raw material ratios of the polyurethane pressure-sensitive adhesive and the production and processing parameters of the protective film are different.

[0046] Table 3 Raw material ratio of polyurethane pressure-sensitive adhesive and production and processing parameters of protective film Example 6 The difference between this embodiment and embodiment 5 is that, based on embodiment 1, the auxiliary agent is supplemented with modified halloysite nanotubes, and the modified halloysite nanotubes are prepared according to the method of preparation example 4.

[0047] Example 7 The difference between this embodiment and embodiment 6 is that the modified halloysite nanotubes are prepared according to the method of preparation example 5.

[0048] Example 8 The difference between this embodiment and embodiment 6 is that the modified halloysite nanotubes are prepared according to the method of preparation example 6.

[0049] Example 9 The difference between this embodiment and embodiment 1 is that the substrate layer is replaced with a PET film with a thickness of 75 μm and not subjected to foaming treatment, and the PET film is processed from a PET sheet, and the CAS number of the PET sheet is 25038-59-9.

[0050] Comparative Example Comparative Example 1 The protective film was prepared according to Example 1 of the Chinese patent publication number CN 111500243 A.

[0051] Comparative Example 2 The difference between this comparative example and Example 1 is that the components of the polyurethane pressure-sensitive adhesive do not include modified nanocellulose.

[0052] Comparative Example 3 The difference between this comparative example and Example 1 is that the components of the polyurethane pressure-sensitive adhesive do not include graphene oxide.

[0053] Performance testing methods 1. Tensile strength Referring to the method described in GB / T 528-2009, the polyurethane pressure-sensitive adhesive was made into a sample strip and the tensile properties were tested. After the results were measured, the tensile strength measured in Comparative Example 1 was used as the standard to calculate the ratio between the tensile strength of each embodiment and the comparative example and the tensile strength of Comparative Example 1. The ratio was recorded as the relative tensile strength. The results are shown in Table 4.

[0054] 2. Light transmittance The light transmittance of the protective film was characterized by haze, and the haze was tested according to ASTM D1003. After the test, the haze of Comparative Example 1 was used as a reference to calculate the ratio between the haze of each embodiment and the comparative example and the haze of Comparative Example 1, and the ratio was recorded as the relative haze. The results are shown in Table 4.

[0055] Table 4 Test results sample Relative tensile strength / % Relative haze / % Example 1 119 76 Example 2 122 74 Example 3 123 75 Example 4 125 76 Example 5 125 73 Example 6 131 72 Example 7 130 73 Example 8 131 72 Example 9 119 97 Comparative Example 1 100 100 Comparative Example 2 104 75 Comparative Example 3 107 76 It can be seen from Examples 1-5 and Comparative Example 1 and Table 4 that the tensile strengths measured in Examples 1-5 are all higher than those in Comparative Example 1, indicating that the polyurethane pressure-sensitive adhesive of the present application has better tensile properties and is not prone to breakage during film tearing, thereby reducing the impact of residual adhesive on the OLED screen and helping to improve the yield rate of the OLED screen.

[0056] Combining Example 1 and Comparative Examples 2-3 and Table 4, it can be seen that the tensile strength of Comparative Examples 2-3 is lower than that of Example 1, indicating that when modified nanocellulose and graphene oxide are not used in combination, the improvement of the tensile properties of the protective film is relatively limited.

[0057] It can be seen from Example 5 and Examples 6-8 and Table 4 that the tensile strength of Examples 6-8 is higher than that of Example 5, indicating that the addition of modified halloysite nanotubes can further improve the tensile strength of the polyurethane pressure-sensitive adhesive, help reduce the amount of residual glue on the surface of the OLED screen, and improve the yield rate of the OLED screen.

[0058] Combining Example 1 and Comparative Example 1, Example 9 and Table 4, it can be seen that the haze of Comparative Example 1 and Comparative Example 1 is lower than that of Example 1, indicating that the substrate layer selected in the present application helps to improve the light transmittance of the protective film and reduce the impact of the manufacturing process on the OLED screen.

[0059] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An OLED flexible screen process protective film, characterized in that: It comprises a substrate layer, an adhesive layer and a release layer, wherein the adhesive layer is bonded to the surface of the substrate layer, and the release layer is attached to the surface of the adhesive layer; the substrate layer is made of PET, the adhesive layer is made of a polyurethane pressure-sensitive adhesive, and the polyurethane pressure-sensitive adhesive comprises the following components in parts by weight: 100-105 parts of a polyurethane masterbatch, 40-45 parts of a polyurethane monomer, 25-27 parts of a curing agent, 12-15 parts of an auxiliary agent, 8-12 parts of modified nanocellulose, and 2.6-4.4 parts of graphene oxide; The modified nanocellulose is prepared by heating diisocyanate, adding an organic base catalyst to the diisocyanate, and then adding nanocellulose. -1 The reaction is terminated when the isocyanate groups at the reaction site disappear, thereby obtaining a mixed solution; the mixed solution is washed with an organic solvent, and the modified nanocellulose is obtained after centrifugal separation.

2. The OLED flexible screen process protective film according to claim 1, characterized in that: In the preparation method of the modified nanocellulose, the organic base catalyst selected is a DABCO catalyst.

3. The OLED flexible screen process protective film according to claim 2, characterized in that: The amount of the organic base catalyst used is 0.7-0.9% of the weight of the nanocellulose.

4. The OLED flexible screen process protective film according to claim 1, characterized in that: The substrate layer is prepared according to the following method: (1) LDPE, AC foaming agent and dicumyl peroxide are mixed and kneaded to obtain a foaming agent base material for standby use; (2) The PET sheet and the foaming agent substrate are mixed and added to a molding machine, and then preheated to a processing temperature. The mixture is kept warm under the processing temperature and subjected to a molding process for 270-310 seconds to obtain a substrate layer.

5. The OLED flexible screen process protective film according to claim 4, characterized in that: In the step (2) of preparing the substrate layer, the processing temperature is set at 190-200°C.

6. The OLED flexible screen process protective film according to claim 4, characterized in that: In the step (2) of preparing the substrate layer, the pressure condition is set to 20-22 MPa.

7. The OLED flexible screen process protective film according to claim 4, characterized in that: The preheating time of the foaming agent substrate is 220-250s.

8. The OLED flexible screen process protective film according to claim 1, characterized in that: The auxiliary agent includes modified halloysite nanotubes, which are prepared according to the following method: MDI and halloysite nanotubes are mixed in a weight ratio of (19.8-20.6):1, then heated at 83-85°C for 180-185min, and the modified halloysite nanotubes are obtained after centrifugal separation and washing.

9. The OLED flexible screen process protective film according to claim 8, characterized in that: The weight of the modified halloysite nanotubes is 0.5-0.7% of the weight of the polyurethane masterbatch.

10. The method for preparing the OLED flexible screen process protective film according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Mixing a polyurethane masterbatch, a polyurethane monomer, a curing agent, an additive, and modified nanocellulose to obtain a polyurethane pressure-sensitive adhesive; (2) The polyurethane pressure-sensitive adhesive is coated on the surface of the substrate layer, dried at 80-120°C, then mixed with the release film, rolled up, and then aged at 45-65°C for 30-35 minutes to obtain a protective film.

Citation Information

Cited By

  • Polylactic acid aluminum laminated film and preparation method thereof

    CN119570096A