Core-shell perovskite nanocrystalline composite material, preparation method, device and equipment
By coating perovskite nanocrystals with shell materials including subgroup II elements and main group IV elements, the problems of stability and photoelectric performance of perovskite nanocrystal materials are solved, and higher environmental stability is achieved. The properties and optoelectronic performance are improved, and it is suitable for a variety of optoelectronic devices.
Patent Information
- Application Number
- CN202410498810.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-29
AI Technical Summary
Perovskite nanocrystalline materials have fast crystallization rates due to their ionic properties and low lattice energy, and low formation energy of lead defects or halide vacancies, which limits their application and commercialization, and they are prone to instability under environmental influence. , such as octahedral lattice collapse, sintering and agglomeration, resulting in poor stability.
Compounds including subgroup II elements and main group IV elements are used as shell materials to coat the perovskite nanocrystal CsPbX3 core to form a core-shell perovskite nanocrystal composite material. The energy band structure is adjusted by selecting different element combinations. and optical properties, improve stability and inhibit ion migration.
Significantly improves the environmental stability and optoelectronic properties of perovskite nanocrystals, enhances surface defect passivation, reduces non-radiative recombination and surface ligand shedding, achieves efficient light conversion and emission, and is suitable for lasers, photodetectors and LED devices.
Smart Images

Figure CN118853136A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal halide nanomaterials, in particular to a core-shell perovskite nanocrystal composite material, a preparation method and a device. Background Art
[0002] Metal halide perovskite materials show great advantages in the next generation of optoelectronic devices, especially light-emitting diodes, due to their excellent optoelectronic properties such as tunable band gap, high carrier mobility, high color purity, wide color gamut, high photoluminescence quantum yield and facile solution processability.
[0003] The fast crystallization rate and low formation energy of lead defects or halide vacancies due to the intrinsic ionic nature and low lattice energy of perovskite nanocrystals severely limit its practical and commercial application. Summary of the invention
[0004] In view of the existing technical problems, the purpose of the present invention is to provide a core-shell perovskite nanocrystal composite material, a preparation method and a device with better environmental stability and excellent photoelectric performance.
[0005] To achieve the above-mentioned purpose, the technical solution provided in the first aspect of the present invention is: a core-shell perovskite nanocrystal composite material, the perovskite nanocrystal composite material includes a perovskite nanocrystal CsPbX3 core and a shell cluster material, the shell cluster material is coated on the outside of the perovskite nanocrystal CsPbX3 core, the shell cluster material includes a compound containing metal elements, the metal elements include elements of the II subgroup and / or elements of the IV main group, and compounds containing metal elements include elements of the VI main group; wherein X includes one or more of Cl, Br and I.
[0006] The present invention adopts the compound of the second group element-the VI group element, the IV group element-the VI group element as the coating layer. The compound of the second group element-the VI group element, the IV group element-the VI group element has high chemical stability and good protection effect, and can reduce or prevent the perovskite nanocrystal CsPbX3 core from being oxidized, corroded or affected by other environments, and can improve the stability of the perovskite nanocrystal CsPbX3; the perovskite nanocrystal composite material has a strong ability to inhibit ion migration, and when a halogen element different from the X-position element of the perovskite nanocrystal is added, ion exchange does not occur, thereby causing the phenomenon of the emission peak position of the nanocrystal to move. In addition, the compound of the second group element-the VI group element, the IV group element-the VI group element has an adjustable energy band structure, and the band gap size can be adjusted by selecting different element combinations. As a shell material, the optical properties of the nanocrystal can be changed by adjusting the energy band structure of the shell material. Perovskite nanocrystal composites have good optical properties, high absorption and emission efficiency, and good optical stability, which can achieve efficient light conversion and emission. The cluster shell material has low reactivity and can grow and coat the surface of the perovskite nanocrystal without destroying the surface of the perovskite nanocrystal.
[0007] The shell cluster material includes one or more of ZnS, CdSe, CdS, PbSe and PbS.
[0008] The shape of the perovskite nanocrystal composite material includes a cube or a quasi-cube, wherein the quasi-cube indicates that the shape is similar to a cube and at least has a columnar structure.
[0009] Among them, the shape of the core of the perovskite nanocrystal CsPbX3 is a cube or a quasi-cube, and the side length of the core of the perovskite nanocrystal CsPbX3 is 3-15nm; the thickness of the shell cluster material is 1-5nm.
[0010] Among them, there are obvious differences in the lattice spacing and lattice arrangement of the core and shell cluster materials of perovskite nanocrystal CsPbX3.
[0011] The second aspect of the present invention includes a method for preparing a core-shell perovskite nanocrystalline composite material, comprising:
[0012] A solution containing a perovskite nanocrystal CsPbX3 core is provided, a solution containing a shell cluster material is heated and added to a solution of the perovskite nanocrystal CsPbX3 core at a first temperature, and then cooled in an ice-water bath to obtain a perovskite nanocrystal composite material; wherein the shell cluster material includes a metal element, the metal element includes a sub-group II element or / and a main group IV element, and X of the perovskite nanocrystal CsPbX3 core includes one or more of Cl, Br and I. In the preparation method of the present invention, the cluster shell material has a very low reactivity and can grow and coat the surface of the perovskite nanocrystal without destroying the surface of the perovskite nanocrystal.
[0013] The temperature at which the solution of the shell cluster material is heated is 100°C-110°C.
[0014] The first temperature is 150°C-200°C. The synthesis of the perovskite nanocrystal CsPbX3 core should have just been completed and the solution temperature should be between 150°C-200°C. The shell cluster material solution can be injected at this time. Injecting the shell cluster material solution when the perovskite nanocrystal CsPbX3 core is at a high temperature can improve or avoid the damage of the shell material to the nanocrystal.
[0015] The solvent used in the solution containing the shell cluster material includes one or more of 1-octadecene, oleic acid, tri-n-octylphosphine (TOP) and diphenylphosphine (DPP). When the solvent is oleic acid, the oleic acid in the shell cluster material can supplement the loss of ligands on the surface of the nanocrystal.
[0016] The method for preparing a solution containing shell cluster materials comprises: mixing a simple substance of a group VI element and a solvent to form a group VI element-solvent complex;
[0017] Mixing a raw material containing a subgroup II element and / or a main group IV element, 1-octadecene and oleic acid, and heating them at a second temperature under an inert gas to react, thereby obtaining an intermediate containing a subgroup II element and / or a main group IV element;
[0018] The VI main group element-solvent complex and the intermediate having the II sub-group element and / or the IV main group element are added to react at a third temperature to obtain a shell cluster material.
[0019] The second temperature ranges from 100°C to 120°C, and the third temperature ranges from 100°C to 110°C.
[0020] The solvent in the mixture of the simple substance of the Group VI element and the solvent includes tri-n-octylphosphine (TOP) and / or diphenylphosphine (DPP), but is not limited to the above solvents.
[0021] Wherein, the molar volume ratio of the Group VI A element to the solvent is (0.1-1.0) mmol:1 mL.
[0022] Wherein, a cesium precursor, a lead precursor and a halogen precursor are mixed and reacted in a molar ratio of 0.1mmol:(0.1-0.2)mmol:(0.3-0.6)mmol to form perovskite nanocrystal CsPbX3. In the preparation method of the present invention, the cesium precursor, the lead precursor and the halogen precursor are three completely independent precursors, so that the Cs source, the Pb source and the halogen source are all independent, and the proportion and purity of each element can be well controlled.
[0023] The solvent used for the mixed reaction includes oleic acid and oleylamine, and the volume ratio of oleic acid to oleylamine is 1:(1-3). In the embodiment of the present invention, oleic acid and oleylamine are used as nanocrystal surface ligands. By controlling the ratio of oleic acid and oleylamine, the collapse of the lattice of the perovskite nanocrystal CsPbX3, the fusion of adjacent nanocrystals, and the excessive surface defects can be reduced, and the difficulty of carrier injection can be reduced.
[0024] Wherein, after cooling in an ice-water bath, purification is also included, and the solvent used for purification includes but is not limited to ethyl acetate to purify the core-shell perovskite nanocrystal composite material.
[0025] Among them, the rotation speed for removing large particles during purification is (10000-14000) rpm and the time is (1-3) min.
[0026] A third aspect of the present invention provides a light-emitting device, comprising the core-shell perovskite nanocrystal composite material described above, or the core-shell perovskite nanocrystal composite material prepared by the above preparation method.
[0027] The fourth aspect of the present invention also provides an electrical device, the above core-shell perovskite nanocrystal composite material, or the core-shell perovskite nanocrystal composite material prepared by the above preparation method.
[0028] The fifth aspect of the present invention also provides a light-emitting device, the above-mentioned core-shell perovskite nanocrystal composite material, or the core-shell perovskite nanocrystal composite material prepared by the above-mentioned preparation method, or the above-mentioned light-emitting device.
[0029] Compared with the prior art, the present invention has the following obvious outstanding substantive features and significant advantages:
[0030] 1. The core-shell perovskite nanocrystal composite material of the present invention has good stability and high photoluminescence quantum yield compared with single-core nanocrystals. Due to the coating of the cluster shell layer, the surface defects of the core-shell nanocrystals are well passivated, non-radiative recombination is inhibited, the shedding of surface ligands is reduced, and the photoelectric properties of the nanocrystals are greatly improved.
[0031] 2. The preparation method of the core-shell perovskite nanocrystal composite material of the present invention has low synthesis temperature, low synthesis cost, simple synthesis, and uniform synthesized nanocrystals. The core-shell nanocrystal composite material can be mass-produced and prepared, and the nanocrystal composite material has high stability.
[0032] 3. The core-shell perovskite nanocrystal composite material of the present invention has excellent photoelectric properties and stability, and can be applied to the fields of lasers, photodetectors, LED devices, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Schematic diagram of the growth and coating of the CsPbI3 / PbS core-shell perovskite nanocrystal composite material prepared in Example 1 of the present invention.
[0034] Figure 2 This is an emission spectrum (PL) diagram of the CsPbI3 / PbS core-shell perovskite nanocrystal composite material prepared in Example 1 of the present invention.
[0035] Figure 3 This is a graph of the UV-visible absorption spectrum (Absorbance) of the CsPbI3 / PbS core-shell perovskite nanocrystal composite material prepared in Example 1 of the present invention.
[0036] Figure 4 This is a high-resolution transmission electron microscopy (HRTEM) image of the CsPbI3 / PbS core-shell perovskite nanocrystal composite material prepared in Example 1 of the present invention.
[0037] Figure 5a The photoluminescence contour map of the two samples of CsPbI3 and CsPbBr3 perovskite nanocrystals in Comparative Example 1, which were stirred and mixed for 15 minutes;
[0038] Figure 5b The photoluminescence contour map of the CsPbI3 / PbS core-shell perovskite nanocrystal composite material CsPbBr3 perovskite nanocrystal stirred and mixed for 15 minutes in Example 1 of the present invention;
[0039] Figure 5c This is a spectrum of the two samples of CsPbI3 and CsPbBr3 perovskite nanocrystals in Comparative Example 1, which were stirred and mixed for 15 minutes;
[0040] Figure 5d This is a spectrum diagram of CsPbI3 / PbS core-shell perovskite nanocrystal composite material CsPbBr3 perovskite nanocrystal stirred and mixed for 15 minutes in Example 1 of the present invention;
[0041] Figure 5eIt is a normalized photoluminescence intensity decay diagram of two samples of CsPbI3 of comparative example 1 and CsPbI3 / PbS core-shell nanocrystal composite material of example 1 at 85°C for 300 minutes;
[0042] Figure 5f This is a normalized photoluminescence intensity attenuation graph of two samples of CsPbI3 of Comparative Example 1 and CsPbI3 / PbS core-shell nanocrystal composite material of Example 1 when irradiated with 365nm ultraviolet lamp for 300min.
[0043] Figure 6a The electroluminescence spectra of the LED devices of Comparative Example 1 and Example 1;
[0044] Figure 6b The external quantum efficiency-voltage characteristic curves of the LED devices of Comparative Example 1 and Example 1;
[0045] Figure 6c The current density-voltage characteristic curves of the LED devices of Comparative Example 1 and Example 1;
[0046] Figure 6d The brightness-voltage characteristic curves of the LED devices of Comparative Example 1 and Example 1 are shown.
[0047] Figure 7a The normalized photoluminescence intensity decay graph of two samples of CsPbBr3 of Comparative Example 2 and CsPbBr3 / CdSe core-shell nanocrystal composite material of Example 2 at 100°C for 300 minutes;
[0048] Figure 7b The normalized photoluminescence intensity attenuation graph of two samples of CsPbBr3 of Comparative Example 2 and CsPbBr3 / CdSe core-shell nanocrystal composite material of Example 2 when irradiated with 365nm ultraviolet lamp for 300min;
[0049] Figure 7c This is a spectrum change diagram of CsPbBr3 in comparative example 2 within 180 minutes after adding OAmI solution;
[0050] Figure 7d This is a spectrum change diagram within 180 minutes after adding OAmI solution to the CsPbBr3 / CdSe core-shell nanocrystal composite material of Example 2;
[0051] Figure 8a : are the electroluminescence spectra of the LED devices of Comparative Example 2 and Example 2;
[0052] Figure 8b The external quantum efficiency-voltage characteristic curves of the LED devices of Comparative Example 2 and Example 2;
[0053] Figure 8c 2 are the current density-voltage characteristic curves of the LED devices of Comparative Example 2 and Example 2;
[0054] Figure 8d 2 are the brightness-voltage characteristic curves of the LED devices of Comparative Example 2 and Example 2;
[0055] Fig. 9 This is a transmission electron microscope image of the control sample of Comparative Example 3. DETAILED DESCRIPTION
[0056] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments. It should be noted that these embodiments are only used to illustrate the present invention and do not limit the scope of the present invention. After reading the content of the present invention, any modification and replacement made by those skilled in the art to the present invention all fall within the scope limited by the appended claims of the application.
[0057] Due to the inherent ionic properties and low lattice energy of perovskite nanocrystals, the crystallization rate is fast and the formation energy of lead defects or halide vacancies is low. Factors such as the inherent solubility equilibrium and high dynamic binding of surface ligands lead to poor stability of nanocrystals, which makes them prone to collapse, sintering, and agglomeration of the perovskite octahedral lattice under the influence of external environmental conditions (such as light, temperature, humidity, etc.). All these instabilities make perovskite nanocrystals environmentally fragile, and when perovskite nanocrystals are integrated into optoelectronic devices, they will not only lead to nanocrystal decomposition and phase transition, but also lead to luminescence quenching and poor electron mobility.
[0058] To this end, an embodiment of the present invention provides a core-shell perovskite nanocrystal composite material, the perovskite nanocrystal composite material includes a perovskite nanocrystal CsPbX3 core and a shell cluster material, the shell cluster material is coated on the outside of the perovskite nanocrystal CsPbX3 core, the shell cluster material includes a compound containing a metal element, the metal element includes a II sub-group element or / and a IV main group element, and a compound containing a metal element includes a VI main group element; wherein X includes one or more of Cl, Br and I.
[0059] The present invention adopts the compound of the second group element-the VI group element, the IV group element-the VI group element as the coating layer. The compound of the second group element-the VI group element, the IV group element-the VI group element has high chemical stability and good protection effect, and can reduce or prevent the perovskite nanocrystal CsPbX3 core from being oxidized, corroded or affected by other environments, and can improve the stability of the perovskite nanocrystal CsPbX3; the perovskite nanocrystal composite material has a strong ability to inhibit ion migration, and when a halogen element different from the X-position element of the perovskite nanocrystal is added, ion exchange does not occur, thereby causing the phenomenon of the emission peak position of the nanocrystal to move. In addition, the compound of the second group element-the VI group element, the IV group element-the VI group element has an adjustable energy band structure, and the band gap size can be adjusted by selecting different element combinations. As a shell material, the optical properties of the nanocrystal can be changed by adjusting the energy band structure of the shell material. Perovskite nanocrystal composites have good optical properties, high absorption and emission efficiency, and good optical stability, which can achieve efficient light conversion and emission. The cluster shell material has low reactivity and can grow and coat the surface of the perovskite nanocrystal without destroying the surface of the perovskite nanocrystal.
[0060] The shell cluster material includes one or more of ZnS, CdSe, CdS, PbSe and PbS.
[0061] Among them, the shape of the perovskite nanocrystal composite material includes cube or quasi-cube.
[0062] Among them, the shape of the core of the perovskite nanocrystal CsPbX3 is a cube or a quasi-cube, and the side length of the core of the perovskite nanocrystal CsPbX3 is 3-15nm; the thickness of the shell cluster material is 1-5nm.
[0063] Among them, there are obvious differences in the lattice spacing and lattice arrangement of the core and shell cluster materials of perovskite nanocrystal CsPbX3.
[0064] The second aspect of the present invention includes a method for preparing a core-shell perovskite nanocrystalline composite material, comprising:
[0065] A solution containing a perovskite nanocrystal CsPbX3 core is provided, a solution containing a shell cluster material is heated and added to a solution of the perovskite nanocrystal CsPbX3 core at a first temperature, and then cooled in an ice-water bath to obtain a perovskite nanocrystal composite material; wherein the shell cluster material includes a metal element, the metal element includes a sub-group II element or / and a main group IV element, and X of the perovskite nanocrystal CsPbX3 core includes one or more of Cl, Br and I. In the preparation method of the present invention, the cluster shell material has a very low reactivity and can grow and coat the surface of the perovskite nanocrystal without destroying the surface of the perovskite nanocrystal.
[0066] Wherein, the temperature of the solution heated by the shell cluster material is 100°C-110°C.
[0067] The first temperature is 150°C-200°C. The synthesis of the perovskite nanocrystal CsPbX3 core should have just been completed and the solution temperature should be between 150°C-200°C. The shell cluster material solution can be injected at this time. Injecting the shell cluster material solution when the perovskite nanocrystal CsPbX3 core is at a high temperature can improve or avoid the damage of the shell material to the nanocrystal.
[0068] The solvent used in the solution containing the shell cluster material includes one or more of 1-octadecene, oleic acid, tri-n-octylphosphine (TOP) and diphenylphosphine (DPP).
[0069] The method for preparing a solution containing shell cluster materials comprises: mixing a simple substance of a group VI element and a solvent to form a group VI element-solvent complex;
[0070] Mixing a raw material containing a subgroup II element and / or a main group IV element, 1-octadecene and oleic acid, and heating them at a second temperature under an inert gas to react, thereby obtaining an intermediate containing a subgroup II element and / or a main group IV element;
[0071] The VI main group element-solvent complex and the intermediate having the II sub-group element and / or the IV main group element are added to react at a third temperature to obtain a shell cluster material.
[0072] The second temperature ranges from 100°C to 120°C, and the third temperature ranges from 100°C to 110°C.
[0073] The solvent includes tri-n-octylphosphine (TOP) and / or diphenylphosphine (DPP), but is not limited to the above solvents.
[0074] Wherein, the molar volume ratio of the Group VI A element to the solvent is (0.1-1.0) mmol:1 mL.
[0075] Wherein, a cesium precursor, a lead precursor and a halogen precursor are mixed and reacted in a molar ratio of 0.1mmol:(0.1-0.2)mmol:(0.3-0.6)mmol to form perovskite nanocrystal CsPbX3. In the preparation method of the present invention, the cesium precursor, the lead precursor and the halogen precursor are three completely independent precursors, so that the Cs source, the Pb source and the halogen source are all independent, and the proportion and purity of each element can be well controlled.
[0076] Wherein, the solvent used for the mixed reaction includes oleic acid and oleylamine, and the volume ratio of oleic acid to oleylamine is 1:(1-3). In the embodiment of the present invention, oleic acid and oleylamine are used as nanocrystal surface ligands. By controlling the ratio of oleic acid and oleylamine, the collapse of the octahedral lattice of the perovskite nanocrystal CsPbX3, the fusion of adjacent nanocrystals, and the excessive surface defects can be reduced, thereby reducing the difficulty of carrier injection.
[0077] Wherein, after cooling in an ice-water bath, purification is also included, and the solvent used for purification includes but is not limited to ethyl acetate to purify the core-shell perovskite nanocrystal composite material.
[0078] Among them, the rotation speed for removing large particles during purification is (10000-14000) rpm and the time is (1-3) min.
[0079] A third aspect of the present invention provides a light-emitting device, comprising the core-shell perovskite nanocrystal composite material described above, or the core-shell perovskite nanocrystal composite material prepared by the above preparation method.
[0080] The fourth aspect of the present invention also provides an electrical device, the above core-shell perovskite nanocrystal composite material, or the core-shell perovskite nanocrystal composite material prepared by the above preparation method.
[0081] The fifth aspect of the present invention also provides a light-emitting device, the above-mentioned core-shell perovskite nanocrystal composite material, or the core-shell perovskite nanocrystal composite material prepared by the above-mentioned preparation method, or the above-mentioned light-emitting device.
[0082] It should be noted that the reaction process of the present invention is carried out under the protection of an inert gas atmosphere, wherein the inert gas includes at least one of nitrogen, argon or a rare gas.
[0083] The above scheme is further described below in conjunction with specific implementation examples. The preferred embodiments of the present invention are described in detail as follows:
[0084] Example 1
[0085] In this embodiment, if Figure 1As shown, a core-shell perovskite nanocrystal material is shown, wherein the core of the perovskite is CsPbI3 nanocrystal, and the shell material is PbS cluster. The CsPbI3 crystal core is surface coated with the PbS cluster shell to form a CsPbI3 / PbS core-shell perovskite nanocrystal.
[0086] A method for preparing a core-shell perovskite nanocrystalline material comprises the following steps:
[0087] a. Preparation of PbS shell cluster materials, the specific steps are as follows;
[0088] a-1. Synthesis of cluster shell anionic compounds:
[0089] Under nitrogen environment protection, 4 mmol of 0.1280 g of sulfur powder was added to 10 mL of tri-n-octylphosphine and stirred until the sulfur powder was completely dissolved to obtain tri-octylphosphine sulfur.
[0090] a-2. Synthesis of cluster shell cationic compounds:
[0091] 3 mmol, 0.9758 g, lead acetate, 26 mL, 1-octadecene and 4 mL, oleic acid were placed in a 50 mL three-necked flask. Under nitrogen, the mixture was heated and stirred to 120° C. and maintained for a period of time until the lead acetate was completely dissolved to obtain lead oleate.
[0092] a-3. Preparation of PbS cluster shell:
[0093] Take 1 mL of trioctylphosphine sulfide prepared in step a-1 and 4 mL of lead oleate prepared in step a-2, heat and stir to 100° C. and maintain for 3 min to obtain PbS shell clusters.
[0094] b. Preparation of perovskite nanocrystal CsPbI3 core, the specific steps are as follows;
[0095] b-1. Preparation of cesium oleate precursor:
[0096] 1.5 mmol, 0.4888 g, cesium carbonate, 26 mL of 1-octadecene and 4 mL of oleic acid were placed in a 50 mL three-necked flask, and heated and stirred to 120° C. under nitrogen flow and maintained for a period of time until the cesium carbonate was completely dissolved to obtain cesium oleate.
[0097] b-2. Preparation of CsPbI3 core:
[0098] Take 0.6 mmol, 0.2282 g of 9-octadecene iodide, 1 mL of cesium oleate and 10 mL of 1-octadecene, stir and heat to 120°C under nitrogen flow and maintain for 10 min, then add 0.2 mL of oleic acid and 0.3 mL of oleylamine, heat to 160°C and inject 1 mL of lead oleate to obtain CsPbI3 core.
[0099] c. The shell cluster material is heated to 100°C and injected into a solution of CsPbI3 core at 160°C to obtain core-shell nanocrystals:
[0100] c-1. Preparation of core-shell perovskite nanocrystals:
[0101] Take 1 mL of lead oleate in step a-2 and 1.25 mL of PbS cluster shell heated to 100°C in step a-3 and inject them into the CsPbI3 core solution at 160°C prepared in step b-2, and cool in an ice water bath after 5 seconds to obtain a core-shell perovskite nanocrystal stock solution.
[0102] It is worth noting that the PbS cluster shell needs to be heated to 100°C before injection, because the PbS shell material is synthesized in advance. During the storage process, it will cool and crystals will precipitate. It needs to be heated to dissolve and increase its reaction activity so that the shell material can easily cover the nanocrystals. However, the temperature cannot be too high, otherwise it will affect the formation of the octahedral lattice of the perovskite nanocrystals.
[0103] c-2. Purification of core-shell perovskite nanocrystals:
[0104] Take 10 mL of perovskite nanocrystal stock solution and add 20 mL of ethyl acetate, centrifuge at 7000 rpm for 3 minutes, pour out the supernatant, disperse the precipitate in n-hexane, repeat the above steps and centrifuge again, pour out the supernatant again, disperse the precipitate in n-hexane, centrifuge at 12000 rpm for 90 seconds to remove large particles, take the supernatant, and finally obtain uniformly dispersed high-purity core-shell perovskite nanocrystals CsPbI3 / PbS.
[0105] The core-shell perovskite nanocrystal composite material CsPbI3 / PbS of the embodiment of the present application is used as a light-emitting material to make an LED light-emitting device.
[0106] The production process of LED light-emitting devices is as follows:
[0107] 1) After cleaning the indium tin oxide (ITO) glass with detergent, add deionized water, acetone and isopropanol respectively and clean it in an ultrasonic cleaner for 15 minutes each, and finally soak it in isopropanol for use.
[0108] 2) Use compressed air to blow away the residual isopropyl alcohol on the surface of the ITO glass, and then use an oxygen plasma cleaner for 15 minutes.
[0109] 3) Under atmospheric conditions, 150 μL of poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) (PEDOT:PSS) was taken and spin-coated on the patterned ITO glass using a spin coater at a process parameter of 4000 rpm / 40 s, and then placed on a magnetic stirring heating table at 150° C. for annealing for 15 min to form poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) (PEDOT:PSS) with a thickness of 40 nm.
[0110] 4) Then it was transferred to a glove box in a nitrogen environment, 120 μL of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA) was spin-coated on the HIL PEDOT:PSS at a process parameter of 2000 rpm / 40 s and annealed on a magnetic stirring heating table at 120 °C for 20 min to a thickness of 30 nm.
[0111] 5) 300 μL of CsPbI3 / PbS core-shell perovskite quantum dots with a concentration of 8 mg / mL were spin-coated on the PTAA film at a process parameter of 2000 rpm / 25 s to a thickness of 50 nm;
[0112] 6) Finally, the ITO glass is transferred to the vacuum evaporation chamber. 2nm LiF was deposited at a rate of 40 nm of 2-[3,5-bis(1-phenylbenzimidazol-2-yl)phenyl]-1-phenylbenzimidazole (TPBi) was deposited at a speed of 1 nm LiF was deposited at a rate of 100 nm of Al was deposited.
[0113] Example 2
[0114] In this embodiment, a core-shell perovskite nanocrystal material is provided, wherein the core of the perovskite is CsPbBr3 nanocrystal, and the shell material is CdSe clusters. The CsPbBr3 crystal core is surface coated with the CdSe cluster shell to form a CsPbBr3 / CdSe core-shell perovskite nanocrystal.
[0115] A method for preparing a core-shell perovskite nanocrystalline material comprises the following steps:
[0116] a. Preparation of CdSe shell cluster materials, the specific steps are as follows;
[0117] a-1. Synthesis of cluster shell anionic compounds:
[0118] Under nitrogen environment protection, 4 mmol of 0.3160 g of selenium powder was added to 10 mL of tri-n-octylphosphine and stirred until the selenium powder was completely dissolved to obtain tri-octylphosphine selenium.
[0119] a-2. Synthesis of cluster shell cationic compounds:
[0120] 3 mmol, 0.3852 g, 1-octadecene, and 4 mL of oleic acid were placed in a 50 mL three-necked flask. The mixture was heated and stirred to 240° C. under nitrogen flow and maintained for a period of time until the cadmium oxide was completely dissolved to obtain cadmium oleate.
[0121] a-3. Preparation of CdSe cluster shell:
[0122] Take 1 mL of trioctylphosphine selenide prepared in step a-1 and 8 mL of cadmium oleate prepared in step a-2, heat and stir to 100° C. and maintain for 3 min to obtain a shell CdSe cluster material.
[0123] b. Preparation of perovskite nanocrystal CsPbBr3 core, the specific steps are as follows;
[0124] b-1. Preparation of cesium oleate precursor:
[0125] 1.5 mmol, 0.4888 g, cesium carbonate, 26 mL of 1-octadecene and 4 mL of oleic acid were placed in a 50 mL three-necked flask, and heated and stirred to 120° C. under nitrogen flow and maintained for a period of time until the cesium carbonate was completely dissolved to obtain cesium oleate.
[0126] b-2. Preparation of lead oleate precursor:
[0127] 3 mmol, 0.9758 g, lead acetate, 26 mL, 1-octadecene and 4 mL, oleic acid were placed in a 50 mL three-necked flask. Under nitrogen, the mixture was heated and stirred to 120° C. and maintained for a period of time until the lead acetate was completely dissolved to obtain lead oleate.
[0128] b-3. Preparation of CsPbBr3 core:
[0129] Take 0.6mmol, 0.2090g of 9-octadecene ammonium bromide, 1mL of cesium oleate and 10mL of 1-octadecene, stir and heat to 120℃ under nitrogen flow and keep for 10min, then add 0.3mL of oleic acid and 0.3mL of oleylamine and heat to 180℃, then inject 1.2mL of lead oleate precursor to obtain CsPbBr3 core.
[0130] c. The shell cluster material is heated and injected into the solution of perovskite nanocrystal CsPbBr3 core to obtain core-shell nanocrystals:
[0131] c-1. Preparation of core-shell perovskite nanocrystals:
[0132] At 180°C, 1 mL of the CdSe cluster shell in step a-3 was injected into the solution of the CsPbBr3 core prepared in step b-3, and then cooled in an ice-water bath after 5 seconds to obtain a core-shell perovskite nanocrystal stock solution.
[0133] c-2. Purification of core-shell perovskite nanocrystals:
[0134] Take 10 mL of perovskite nanocrystal stock solution and add 20 mL of ethyl acetate, centrifuge at 7000 rpm for 3 minutes, pour out the supernatant, disperse the precipitate in n-hexane, repeat the above steps and centrifuge again, pour out the supernatant again, disperse the precipitate in n-hexane, centrifuge at 12000 rpm for 90 seconds to remove large particles, take the supernatant, and finally obtain evenly dispersed high-purity core-shell perovskite nanocrystals.
[0135] The emission peak position of the CsPbBr3 / CdSe core-shell perovskite nanocrystal prepared in this embodiment is 517nm, and the half-peak width is 17nm. The green light core-shell perovskite nanocrystal prepared in this embodiment has a crystal structure with clear grain boundaries.
[0136] The core-shell perovskite nanocrystal composite material CsPbBr3 / CdSe of the embodiment of the present application is used as a light-emitting material to make an LED light-emitting device. The preparation method is similar to that of Example 1 and will not be repeated here.
[0137] Comparative Example 1
[0138] The preparation of perovskite nanocrystals CsPbI3, the specific steps are as follows;
[0139] Preparation of cesium oleate precursor:
[0140] 1.5 mmol, 0.4888 g, cesium carbonate, 26 mL of 1-octadecene and 4 mL of oleic acid were placed in a 50 mL three-necked flask, and heated and stirred to 120° C. under nitrogen flow and maintained for a period of time until the cesium carbonate was completely dissolved to obtain cesium oleate.
[0141] Preparation of lead oleate precursor:
[0142] 3 mmol, 0.9758 g, lead acetate, 26 mL, 1-octadecene and 4 mL, oleic acid were placed in a 50 mL three-necked flask. Under nitrogen, the mixture was heated and stirred to 120° C. and maintained for a period of time until the lead acetate was completely dissolved to obtain lead oleate.
[0143] Preparation of CsPbI3 core:
[0144] Take 0.6 mmol, 0.2282 g of 9-octadecene iodide, 1 mL of cesium oleate and 10 mL of 1-octadecene, stir and heat to 120°C under nitrogen flow and maintain for 10 min, then add 0.2 mL of oleic acid and 0.3 mL of oleylamine, heat to 160°C and inject 1 mL of lead oleate to obtain CsPbI3 core.
[0145] CsPbI3 is used as the light-emitting material to make an LED light-emitting device. The preparation method is similar to that in Example 1 and will not be repeated here.
[0146] Comparative Example 2
[0147] The preparation of perovskite nanocrystal CsPbBr3 core, the specific steps are as follows;
[0148] Preparation of cesium oleate precursor:
[0149] 1.5 mmol, 0.4888 g, cesium carbonate, 26 mL of 1-octadecene and 4 mL of oleic acid were placed in a 50 mL three-necked flask, and heated and stirred to 120° C. under nitrogen flow and maintained for a period of time until the cesium carbonate was completely dissolved to obtain cesium oleate.
[0150] Preparation of lead oleate precursor:
[0151] 3 mmol, 0.9758 g, lead acetate, 26 mL, 1-octadecene and 4 mL, oleic acid were placed in a 50 mL three-necked flask. Under nitrogen, the mixture was heated and stirred to 120° C. and maintained for a period of time until the lead acetate was completely dissolved to obtain lead oleate.
[0152] Preparation of CsPbBr3 core:
[0153] Take 0.6mmol, 0.2090g of 9-octadecene ammonium bromide, 1mL of cesium oleate and 10mL of 1-octadecene, stir and heat to 120℃ under nitrogen flow and keep for 10min, then add 0.3mL of oleic acid and 0.3mL of oleylamine and heat to 180℃, then inject 1.2mL of lead oleate precursor to obtain perovskite nanocrystals CsPbBr3.
[0154] CsPbBr3 is used as the light-emitting material to make an LED light-emitting device. The preparation method is similar to that in Example 1 and will not be repeated here.
[0155] The embodiments 1-2 of the present application and comparative examples 1 and 2 were subjected to performance tests, and were used as luminescent materials to make LED light-emitting devices, and the luminescent performance thereof was tested.
[0156] Comparative Example 3
[0157] The preparation of core-shell perovskite nanocrystals CsPbI3 / PbS, the specific steps are as follows;
[0158] Preparation of cesium oleate precursor:
[0159] 1.5 mmol, 0.4888 g, cesium carbonate, 26 mL of 1-octadecene and 4 mL of oleic acid were placed in a 50 mL three-necked flask, and heated and stirred to 120° C. under nitrogen flow and maintained for a period of time until the cesium carbonate was completely dissolved to obtain cesium oleate.
[0160] Preparation of PbS shell cluster materials:
[0161] Under nitrogen environment protection, add 4mmol of 0.1280g sulfur powder to 10mL of tri-n-octylphosphine and stir until the sulfur powder is completely dissolved to obtain trioctylphosphine sulfur. Put 3mmol of 0.9758g of lead acetate, 26mL of 1-octadecene and 4mL of oleic acid into a 50mL three-necked flask, heat and stir to 120℃ and keep for a period of time until the lead acetate is completely dissolved to obtain lead oleate. Take 1mL of trioctylphosphine sulfur and 4mL of lead oleate and heat to 30℃ and stir and keep for 3min to obtain PbS shell clusters.
[0162] Preparation of control samples:
[0163] Take 0.6 mmol, 0.2282 g of 9-octadecene iodide, 1 mL of cesium oleate and 10 mL of 1-octadecene, stir and heat to 120°C under nitrogen and keep for 10 min, then add 0.2 mL of oleic acid and 0.3 mL of oleylamine, heat to 160°C, inject 1 mL of lead oleate and 1.25 mL of PbS shell clusters at 30°C to obtain a control sample.
[0164] Table 1 Performance parameters of Example 1 and Comparative Example 1.
[0165]
[0166] Table 2 Performance parameters of Example 2 and Comparative Example 2.
[0167]
[0168] Depend on Figure 2 It can be seen that the emission peak position of the CsPbI3 / PbS core-shell perovskite nanocrystal prepared in this embodiment is 690nm and the half-peak width is 33nm. Figure 3 As shown in Figure 2, CsPbI3 / PbS core-shell perovskite nanocrystals have a typical absorption starting point at 670nm. Figure 4As shown, the red light core-shell perovskite nanocrystals prepared in this embodiment have a crystal structure with distinct grain boundaries, forming a core-shell structure. The shapes of the cores of the perovskite nanocrystals CsPbI3 include cubes and quasi-cubes. The side length of the core of the perovskite nanocrystal CsPbI3 is 14nm; the thickness of the shell cluster material is 2nm.
[0169] like Figure 5a , 5c As shown in the figure, after the bare core CsPbI3 and CsPbBr3 perovskite nanocrystal samples of comparative example 1 were stirred and mixed for 15 minutes, the peak positions of both samples shifted greatly. This is because a large amount of halogen ions of CsPbI3 and CsPbBr3 were exchanged, resulting in the formation of an orange-yellow light with a peak at 600nm. The new peak formed can be easily detected by the photoluminescence contour line. Figure 5a See. Figure 5b ,5d, after stirring and mixing the shell-coated CsPbI3 / PbS core-shell perovskite nanocrystal composite material of Example 1 with CsPbBr3 perovskite nanocrystals for 15 minutes, no ion migration occurred in the peak positions of both, which was manifested in that the peak positions of the two perovskite nanocrystals in the mixed solution did not move and no new peaks were generated, indicating that the shell-coated CsPbI3 / PbS core-shell perovskite nanocrystals have well fixed their own halogen I ions within the shell and blocked the entry of the halogen Br ions Br of CsPbBr3, indicating that the core-shell structure can well inhibit ion migration. At the same time, thermal stability and light stability tests were also carried out. The shell-coated CsPbI3 / PbS core-shell perovskite nanocrystals and the bare core CsPbI3 perovskite nanocrystals of Comparative Example 1 were placed on a heating table at 85°C, and the changes in their photoluminescence intensity were tested after different time periods. The results are as follows. Figure 5eIt shows that after 300 minutes, the shell-coated CsPbI3 / PbS core-shell perovskite nanocrystals can still maintain more than 90% of the original photoluminescence intensity, however, the photoluminescence intensity of the bare core CsPbI3 perovskite nanocrystals without shell coating in comparative example 1 is less than 10%. Under the same test conditions, it shows that the PbS shell significantly enhances the thermal stability of the perovskite nanocrystals. In addition, the two samples were irradiated with a 365nm ultraviolet lamp for up to 300 minutes to verify the light stability of the CsPbI3 / PbS core-shell perovskite nanocrystal composite material of comparative example 1 and the CsPbI3 of Example 1. The results showed that the standardized photoluminescence intensity of the CsPbI3 / PbS core-shell perovskite nanocrystal composite material remained at 95% after 300 minutes of ultraviolet lamp irradiation, while the standardized photoluminescence intensity of the CsPbI3 perovskite nanocrystal of comparative example 1 remained at 5% after 300 minutes of ultraviolet lamp irradiation, indicating that the light stability of the CsPbI3 / PbS core-shell perovskite nanocrystal composite material of Example 1 of the present application is far superior to that of the bare core CsPbI3 perovskite nanocrystal. The above tests all show that the stability and ion migration inhibition ability of the perovskite nanocrystal can be greatly improved after the perovskite nanocrystal is coated with a shell layer.
[0170] The CsPbI3 of Comparative Example 1 and the CsPbI3 / PbS core-shell perovskite nanocrystal of Example 1 were used as light-emitting layers to make LED devices. It can be seen from the data in Figure 6 and Table 1 that the device performance of the CsPbI3 / PbS core-shell perovskite nanocrystal composite material formed by the PbS cluster shell layer coating has been greatly improved, wherein the maximum external quantum efficiency is increased from 11.98% to 20.05% compared with that of Comparative Example 1, and the maximum brightness is increased from 184 cd / m 2 Up to 1026cd / m 2 , indicating that the photoelectric performance of the CsPbI3 / PbS core-shell perovskite nanocrystal composite material of Example 1 of the present invention is greatly improved.
[0171] exist Figure 7aIn the experiment, the bare-core CsPbBr3 perovskite nanocrystals of Comparative Example 2 and the core-shell perovskite nanocrystal composite material CsPbBr3 / CdSe of Example 2 were placed on a heating table at 100°C for 300 minutes. The results showed that the photoluminescence intensity was still able to maintain more than 80% after 300 minutes, while the photoluminescence intensity of the bare-core CsPbBr3 perovskite nanocrystals of Comparative Example 2 was only 25% of the original, indicating that the CsPbBr3 perovskite nanocrystal composite material coated with a CdSe cluster shell of Example 2 of the present application has better thermal stability. The bare-core CsPbBr3 perovskite nanocrystals of Comparative Example 2 and the core-shell perovskite nanocrystal composite material CsPbBr3 / CdSe of Example 2 were tested for light stability. The bare-core CsPbBr3 and the CsPbBr3 / CdSe core-shell perovskite nanocrystal composite materials were continuously irradiated with a 365nm ultraviolet lamp. The test results are as follows: Figure 7b As shown, after 300 minutes, the photoluminescence intensity of the CsPbBr3 / CdSe core-shell perovskite nanocrystal composite material can maintain 90% of the original, however, the bare core CsPbBr3 perovskite nanocrystal of comparative example 2 can only maintain 30% of the original, indicating that the shell perovskite nanocrystal composite material of Example 2 of the present application has good light stability. In addition, the resistance to halogen ion exchange can also well demonstrate the completeness of the shell coating in the core-shell perovskite nanocrystal. The specific testing method includes: using 9-octadecene iodide ammonium powder to dissolve in a toluene solution to form an 8 mg / mL 9-octadecene iodide ammonium solution, and then adding the 9-octadecene iodide ammonium solution to the CsPbBr3 solution of comparative example 2 and the CsPbBr3 / CdSe core-shell perovskite nanocrystal composite material solution of Example 2 to verify the resistance to halogen anion exchange of the two samples, as shown in FIG. Figure 7c As shown in Figure 7d, the photoluminescence emission peak of the bare core CsPbBr3 perovskite nanocrystals red-shifted from the original 515nm to 540nm within 180min, and its photoluminescence intensity decreased significantly. However, the CsPbBr3 / CdSe core-shell perovskite nanocrystals only red-shifted by 5nm and the photoluminescence intensity only decreased slightly. The red shift of the bare core perovskite nanocrystals is 5 times that of the core-shell perovskite nanocrystals. Such a huge difference represents that the core-shell structure has a better anti-halogen ion exchange effect. The above tests show that the stability of the core-shell perovskite nanocrystals formed by the CdSe cluster shell coating of the CsPbBr3 perovskite nanocrystals has been significantly improved, and its thermal stability, light stability and anti-halogen ion exchange performance can be improved.
[0172] In addition, the bare core CsPbBr3 of Example 2 and the CsPbBr3 / CdSe core-shell perovskite nanocrystal of Example 2 were used to fabricate LED devices and perform performance tests. Figure 8a,8b and Table 2 show that the maximum external quantum efficiency and maximum brightness of CsPbBr3 / CdSe core-shell perovskite nanocrystals are much higher than those of LED devices made of CsPbBr3 bare core perovskite nanocrystals. The maximum external quantum efficiency and maximum brightness of the original bare core CsPbBr3 perovskite nanocrystal LED device are 5.10% and 3926 cd / m 2 The performance of CsPbBr3 / CdSe core-shell perovskite nanocrystal LED devices after CdSe coating has been greatly improved, with the maximum external quantum efficiency and maximum brightness of 13.75% and 27916cd / m 2 , indicating that the photoelectric performance of Example 2 of the present invention is greatly improved. The CsPbBr3 / CdSe core-shell perovskite nanocrystals prepared in the present invention have high luminescence intensity, high quantum yield, good environmental stability, and significantly improved optical properties compared to the bare core perovskite nanocrystals.
[0173] In the synthesis of the control sample of Comparative Example 3, the injection temperature of the PbS cluster shell layer is 30°C, which is a low temperature injection compared with the injection temperature of the PbS cluster shell layer in Example 1 of 100°C. Fig. 9 The high-resolution transmission electron micrograph of the control sample formed when the PbS cluster shell was injected at low temperature is shown in Figure 2. It can be seen from the figure that the PbS cluster shell cannot be seen on the surface of CsPbI3, so the PbS cluster shell cannot cover the CsPbI3 core during low-temperature injection, and the core-shell structure cannot be obtained. Therefore, the PbS cluster should be heated to a high temperature of more than 100°C when injecting the PbS cluster shell to obtain a perovskite nanocrystalline composite material with a core-shell structure.
[0174] This shows that the present application can greatly improve the environmental stability and photoelectric properties of perovskite nanocrystals by coating the surface of perovskite nanocrystals CsPbX3 with cluster shell Group II element-Group VI element compounds or Group IV element-Group VI element compounds.
[0175] Obviously, the above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, any modification, equivalent replacement, or improvement made on the basis of the above description and within the method and principle of the present invention should be included in the protection scope of the present invention. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the protection scope of the present invention.
Claims
1. A core-shell perovskite nanocrystal composite material, characterized in that: The perovskite nanocrystal composite material comprises a perovskite nanocrystal CsPbX3 core and a shell cluster material, wherein the shell cluster material is coated on the outside of the perovskite nanocrystal CsPbX3 core, and the shell cluster material comprises a compound containing a metal element, wherein the metal element comprises a sub-group II element and / or a main group IV element, and the compound containing a metal element is a main group VI element; Wherein X includes one or more of Cl, Br and I.
2. The core-shell perovskite nanocrystal composite material according to claim 1, characterized in that: The shell cluster material includes one or more of ZnS, CdSe, CdS, PbSe and PbS.
3. The core-shell perovskite nanocrystal composite material according to claim 1, characterized in that: The shape of the perovskite nanocrystal composite material includes a cube or a quasi-cube; optionally, the shape of the perovskite nanocrystal CsPbX3 core is a cube or a quasi-cube, and the side length of the perovskite nanocrystal CsPbX3 core is 3-15nm; the thickness of the shell cluster material is 1-6nm.
4. A method for preparing a core-shell perovskite nanocrystal composite material, characterized in that: include: A solution containing a perovskite nanocrystal CsPbX3 core is provided, a solution containing a shell cluster material is heated and added to a solution of the perovskite nanocrystal CsPbX3 core at a first temperature, and then cooled in an ice-water bath to obtain a perovskite nanocrystal composite material; wherein the shell cluster material includes a metal element, the metal element includes a II sub-group element or / and a IV main group element, and X of the perovskite nanocrystal CsPbX3 core includes one or more of Cl, Br and I.
5. The method for preparing the core-shell perovskite nanocrystalline composite material according to claim 4, characterized in that: The first temperature is 150°C-200°C; and / or, The temperature at which the solution of the shell cluster material is heated is 100° C.-120° C.; and / or, The solvent used in the solution containing the shell cluster material includes one or more of 1-octadecene, oleic acid, tri-n-octylphosphine and diphenylphosphine.
6. The method for preparing the core-shell perovskite nanocrystalline composite material according to claim 4 or 5, characterized in that: The method for preparing the solution containing the shell cluster material comprises: Mixing a simple substance of a Group VI element and a solvent to form a Group VI element-solvent complex; Mixing a raw material containing a subgroup II element or a main group IV element, 1-octadecene and oleic acid, and heating them at a second temperature under an inert gas to react, thereby obtaining an intermediate containing a subgroup II element or a main group IV element; The group VI element-solvent complex and the intermediate having the group II element and / or the group IV element are added to react at a third temperature to obtain a shell cluster material.
7. The Group VI element-solvent complex according to claim 6, characterized in that: The solvent in the mixture of the simple substance of the Group VI element and the solvent comprises tri-n-octylphosphine and / or diphenylphosphine; The molar volume ratio of the Group VI element to the solvent is (0.1-1.0) mmol:1 mL.
8. The method for preparing the core-shell perovskite nanocrystalline composite material according to any one of claims 5 to 7, characterized in that: A cesium precursor, a lead precursor and a halogen precursor are mixed and reacted in a molar ratio of 0.1 mmol: (0.1-0.2) mmol: (0.3-0.6) mmol to form perovskite nanocrystals CsPbX3; Optionally, the solvent used for the mixed reaction includes oleic acid and oleylamine, and the volume ratio of oleic acid to oleylamine is 1:(1-3).
9. A light emitting device, characterized in that: The invention comprises the core-shell perovskite nanocrystal composite material according to any one of claims 1 to 3, or the core-shell perovskite nanocrystal composite material prepared by the preparation method according to any one of claims 4 to 8.
10. An electrical device, characterized in that: The invention comprises the core-shell perovskite nanocrystal composite material according to any one of claims 1 to 3, or the core-shell perovskite nanocrystal composite material prepared by the preparation method according to any one of claims 4 to 8.