Method and device for preparing indium-tin alloy by using waste ITO (Indium Tin Oxide) target
By setting multiple through holes at the bottom of the reaction crucible, the hydrogen gas is evenly contacted with the bottom of the ITO waste target block, which solves the problem of unreacted ITO waste target powder wrapped by liquid indium tin alloy, improves the reduction rate and purity, and shortens the reaction time. Reduced energy consumption.
Patent Information
- Application Number
- CN202410905540.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing ITO waste target recycling process, the reduction rate of the hydrogen reduction method is low and the problem of unreacted waste target powder wrapped in liquid alloy is prone to occur, which results in a long reduction process and affects the production efficiency and the purity of the indium tin alloy.
A device was designed. Multiple through holes were provided at the bottom of the reaction crucible. Hydrogen passed through the through holes from the receiving crucible and contacted with the bottom of the ITO waste target block. The generated liquid indium tin alloy dropped downward through the through holes and was collected to ensure that no reaction occurred. The part continues to be in contact with hydrogen until the ITO waste target block is completely consumed.
It improves the reduction rate of ITO waste target, increases the purity of indium-tin alloy, shortens the reaction time, and reduces energy consumption.
Smart Images

Figure CN118854089A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ITO material recycling and preparation, and in particular relates to a method and a device for preparing indium tin alloy by utilizing ITO waste targets. Background Art
[0002] At present, the recycling methods of waste ITO targets mainly include wet recycling process and pyrometallurgical recycling process.
[0003] Patent CN1420184A proposes a technology for recovering indium from indium-containing materials such as indium tin oxide waste: adding the indium-containing waste to an inorganic mixed acid for dissolution, and then adding an oxidant for oxidation to separate indium and tin; adding an alkaline solution and an inorganic co-precipitant during the indium tin separation process to make tin and other impurities form a dense, fast-sedimenting, easy-to-separate solid-liquid precipitate, and then the solution is subjected to solid-liquid separation, replacement, anode casting, and electrolysis to obtain refined indium. The indium recovery rate of this technology is greater than 95%, but the process is cumbersome and involves the discharge of a large amount of acid and alkali, causing environmental pollution.
[0004] Patent CN114231743A adopts a method for preparing indium tin alloy by high-temperature reduction of ITO waste targets: the blocky ITO waste targets are crushed into particles, and then the ITO waste target particles, a reducing agent and a specific slag-forming agent are evenly mixed, and then put into an electric arc furnace for reduction smelting. The indium and tin in the ITO waste target particles enter the alloy liquid layer, and the oxygen in the ITO waste target particles is removed by reacting with the reducing agent, and impurities enter the slag layer. However, the direct recovery rate of indium tin alloy of this technology is low, and the impurity content is high.
[0005] Hydrogen reduction of ITO waste targets is one of the effective ways to recover indium resources by pyrometallurgy. The reaction byproduct is water vapor, which is environmentally friendly, but it also has the problem of low reduction rate. At the reduction temperature, indium tin alloy is usually in liquid state. In the traditional hydrogen reduction process of ITO waste targets, it is easy for the reduced liquid alloy to wrap the unreacted waste target powder, which hinders the contact between hydrogen and unreacted materials, resulting in a longer reduction process and the wrapped ITO waste targets cannot be reduced. When the amount of ITO waste target powder reduced is large, the degree of liquid alloy wrapping increases, the reduction rate is greatly reduced, and the production scale is limited. Summary of the invention
[0006] In view of this, some embodiments disclose a device for preparing indium tin alloy using ITO waste target, comprising:
[0007] A reaction crucible, the bottom of which is provided with a plurality of through holes; the reaction crucible is used for hydrogen reduction of ITO waste target to prepare indium tin alloy;
[0008] A receiving crucible, on which an air inlet hole is provided; the receiving crucible is detachably connected to the bottom of the reaction crucible and communicates with the internal volume of the reaction crucible through a plurality of through holes; the receiving crucible is used to collect the prepared indium tin alloy;
[0009] A heating jacket, which is sleeved on the outer surface of the reaction crucible and is used to heat the reaction crucible;
[0010] A gas supply assembly is arranged to be connected to the gas inlet hole of the receiving crucible and is used to provide hydrogen;
[0011] The cover plate is arranged on the top of the reaction crucible; the cover plate is provided with a gas outlet hole for discharging water vapor generated by the hydrogen reduction reaction.
[0012] In the device for preparing indium tin alloy using ITO waste target disclosed in some embodiments, a temperature sensor is arranged in the reaction crucible.
[0013] In the device for preparing indium tin alloy using ITO waste target disclosed in some embodiments, a pressure sensor is arranged in the reaction crucible.
[0014] In the device for preparing indium tin alloy using ITO waste targets disclosed in some embodiments, a sealing ring is provided at the connection between the reaction crucible and the receiving crucible.
[0015] In the device for preparing indium tin alloy using ITO waste target disclosed in some embodiments, the diameter of the through hole on the reaction crucible is 5-10 mm.
[0016] In the device for preparing indium tin alloy using ITO waste target disclosed in some embodiments, the cross-sectional shape of the through hole on the reaction crucible is an inverted trapezoid.
[0017] In the device for preparing indium tin alloy using ITO waste target disclosed in some embodiments, ear handles are arranged on both side walls of the reaction crucible.
[0018] Some embodiments disclose a method for preparing an indium tin alloy using a waste ITO target, wherein the indium tin alloy is prepared using the above-mentioned device, comprising:
[0019] Taking a set amount of ITO waste target powder and pressing it into an ITO waste target block;
[0020] Putting the ITO waste target block into the reaction crucible;
[0021] Start the gas supply assembly to introduce hydrogen into the reaction crucible;
[0022] Start the heating jacket to heat the reaction crucible to the set temperature;
[0023] The hydrogen enters the receiving crucible from the air inlet of the receiving crucible, then enters the reaction crucible through the through hole at the bottom of the reaction crucible, and contacts and reacts with the bottom of the ITO waste target block at the bottom of the reaction crucible;
[0024] The bottom of the ITO waste target block reacts with hydrogen to generate liquid indium tin alloy and water vapor; the generated liquid indium tin alloy drips downward through the through hole at the bottom of the reaction crucible and is collected in the receiving crucible, and the generated water vapor flows upward through the gas outlet hole on the cover plate and is discharged from the reaction crucible;
[0025] The unreacted portion of the bottom of the ITO waste target block continues to react with the hydrogen gas until the ITO waste target block is completely consumed.
[0026] In the method for preparing indium tin alloy using ITO waste target disclosed in some embodiments, the flow rate of hydrogen is 300-1000 mL / min.
[0027] In the method for preparing indium tin alloy using ITO waste target disclosed in some embodiments, the temperature of the reaction crucible is 800-1000°C.
[0028] The method and device for preparing indium tin alloy using ITO waste targets disclosed in the embodiment of the present invention have multiple through holes in the bottom of the reaction crucible, so that hydrogen flows upward through the through holes from the receiving crucible and contacts and reacts with the bottom of the ITO waste target block set in the reaction crucible. The bottom of the ITO waste target block reacts and melts out, exposing the unreacted part to continue to react with hydrogen. The liquid indium tin alloy generated by the reaction drips downward from the through holes at the bottom of the reaction crucible to the receiving crucible for collection. The method and device for preparing indium tin alloy using ITO waste targets disclosed in the embodiment of the present invention solves the problem that the liquid indium tin alloy generated by the reaction wraps the unreacted ITO waste target powder, improves the reduction rate of the ITO waste target, improves the purity of the indium tin alloy, shortens the reaction time, and reduces energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Example 1 is a schematic diagram of the structure of an apparatus for preparing indium tin alloy using ITO waste targets;
[0030] Figure 2 Schematic diagram of the structure of the reaction crucible of Example 1;
[0031] Figure 3 Schematic diagram of the structure of the receiving crucible of Example 1;
[0032] Figure 4 Example 1 is a reaction principle diagram of a method for preparing an indium tin alloy using an ITO waste target;
[0033] Figure 5 XRD pattern of indium tin alloy of Example 2;
[0034] Figure 6 SEM image of indium tin alloy of Example 2;
[0035] Figure 7 XRD pattern of indium tin alloy of Example 3;
[0036] Figure 8 SEM image of indium tin alloy of Example 3.
[0037] Reference numerals
[0038] 1 Reaction crucible 2 Receiving crucible
[0039] 3 Heating jacket 4 Cover plate
[0040] 5 Air supply assembly 6 Temperature sensor
[0041] 7 Pressure sensor 8 Ear handle
[0042] 11 through hole 21 air inlet
[0043] 22 Limiting strip 41 Vent hole
[0044] 100 ITO waste target block 200 Liquid indium tin alloy DETAILED DESCRIPTION
[0045] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0046] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0047] The terms "substantially" and "approximately" used herein are used to describe small fluctuations. For example, they can refer to less than or equal to ±5%, such as less than or equal to ±2%, such as less than or equal to ±1%, such as less than or equal to ±0.5%, such as less than or equal to ±0.2%, such as less than or equal to ±0.1%, such as less than or equal to ±0.05%. The numerical data represented or presented in the range format herein are used only for convenience and brevity, and should therefore be flexibly interpreted as including not only the values clearly listed as the limits of the range, but also all independent values or sub-ranges contained in the range. For example, the numerical range of "1-5%" should be interpreted as including not only the clearly listed values of 1% to 5%, but also the independent values and sub-ranges within the range shown. Therefore, independent values such as 2%, 3.5% and 4% and sub-ranges such as 1%-3%, 2%-4% and 3%-5% are included in this numerical range. This principle also applies to the range of only one numerical value. In addition, such an interpretation applies regardless of the width of the range or the characteristics described.
[0048] In this document, including in the claims, transitional words such as "comprises," "includes," "with," "having," "containing," "involving," "accommodating," etc. are understood to be open-ended, i.e., meaning "including but not limited to." Only the transitional words "consisting of" and "composed of" are closed transitional words.
[0049] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0050] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be arbitrarily combined, and the obtained technical solutions belong to the contents disclosed in the embodiments of the present application. It should be noted that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like mentioned in the present application indicate the orientation or position relationship based on the orientation or position relationship shown in the accompanying drawings, which is only for the convenience of describing the technical features and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention, unless it conflicts with the context. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance, unless it conflicts with the context.
[0051] In some embodiments, a device for preparing an indium tin alloy using a waste ITO target comprises:
[0052] A reaction crucible, wherein a plurality of through holes are formed through the bottom of the reaction crucible, and the plurality of through holes are evenly distributed on the bottom of the reaction crucible, so that hydrogen can evenly enter the reaction crucible and evenly contact and react with the surface of the ITO waste target block; the reaction crucible is used for hydrogen reduction of the ITO waste target to prepare indium tin alloy; generally, the material of the reaction crucible is alumina, graphite, 310s stainless steel, etc.;
[0053] A receiving crucible, wherein an air inlet hole is provided on the receiving crucible; the receiving crucible is detachably connected to the bottom of the reaction crucible and is connected to the internal volume of the reaction crucible through a plurality of through holes; the receiving crucible is used to collect the prepared indium tin alloy; in some embodiments, a circle of limiting bars is provided on the inner side wall of the receiving crucible, and when the reaction crucible is set on the receiving crucible, the reaction crucible is located on the limiting bars;
[0054] A heating jacket, which is sleeved on the outer surface of the reaction crucible and is used to heat the reaction crucible;
[0055] A gas supply assembly is arranged to be connected to the gas inlet hole of the receiving crucible and is used to provide hydrogen;
[0056] The cover plate is arranged on the top of the reaction crucible; the cover plate is provided with a gas outlet hole for discharging water vapor generated by the hydrogen reduction reaction.
[0057] In some embodiments, a temperature sensor is disposed in the reaction crucible to detect the temperature in the reaction crucible.
[0058] In some embodiments, a pressure sensor is disposed in the reaction crucible to detect the gas pressure in the reaction crucible.
[0059] In some embodiments, a solenoid valve adapted to a pressure sensor is disposed in the air outlet on the cover plate. When the pressure sensor detects that the air pressure in the reaction crucible is too high, the solenoid valve will automatically open to exhaust air, thereby reducing the air pressure in the reaction crucible, thereby avoiding danger caused by excessive air pressure in the reaction crucible.
[0060] In some embodiments, a sealing ring is provided at the connection between the reaction crucible and the receiving crucible.
[0061] In some embodiments, the through hole on the reaction crucible has a diameter of 5 to 10 mm to facilitate the passage of the generated liquid indium tin alloy.
[0062] In some embodiments, the setting density and setting position of the through holes on the reaction crucible are related to the size of the ITO waste target block, so that the hydrogen passing through the through holes can only contact and react with the ITO waste target at the bottom position of the ITO waste target block, so that the hydrogen passing through the through holes can contact and react with the bottom of the ITO waste target block evenly and fully.
[0063] In some embodiments, the cross-sectional shape of the through hole on the reaction crucible is an inverted trapezoid. The inverted trapezoidal structure is conducive to the bidirectional flow of hydrogen and liquid indium tin alloy. When hydrogen reacts with the ITO waste target block to generate liquid indium tin alloy, hydrogen flows upward from the middle position of the through hole, and the generated liquid indium tin alloy flows downward along the inner wall of the through hole.
[0064] In some embodiments, ear handles are provided on both side walls of the reaction crucible to facilitate operators to move the reaction crucible.
[0065] In some embodiments, a method for preparing an indium tin alloy using a waste ITO target, using the above-mentioned device to prepare an indium tin alloy, comprises:
[0066] A set amount of ITO waste target powder is taken and pressed into an ITO waste target block; generally, a certain amount of ITO waste target powder is taken and pre-pressed into shape in a mold by a tablet press, and then the pre-formed ITO waste target powder is vacuum-sealed and evenly pressed in a cold isostatic press to obtain a tightly combined ITO waste target block; generally, the diameter of the mold is 5 to 25 mm, and the shape of the mold is cylindrical, square, etc.; the pre-pressing pressure is 15 MPa, and the cold isostatic pressing pressure is 100 MPa;
[0067] Putting the ITO waste target block into the reaction crucible;
[0068] Start the gas supply assembly to introduce hydrogen into the reaction crucible;
[0069] Start the heating jacket to heat the reaction crucible to the set temperature;
[0070] The hydrogen enters the receiving crucible from the air inlet of the receiving crucible, then enters the reaction crucible through the through hole at the bottom of the reaction crucible, and contacts and reacts with the bottom of the ITO waste target block at the bottom of the reaction crucible;
[0071] The bottom of the ITO waste target block reacts with hydrogen to generate liquid indium tin alloy and water vapor; the generated liquid indium tin alloy drips downward through the through hole at the bottom of the reaction crucible and is collected in the receiving crucible, and the generated water vapor flows upward through the gas outlet hole on the cover plate and is discharged from the reaction crucible;
[0072] The exposed unreacted portion at the bottom of the ITO waste target block continues to react with hydrogen until the ITO waste target block is completely consumed. The liquid indium tin alloy generated by the hydrogen and ITO waste target reaction flows directly into the receiving crucible, and the liquid indium tin alloy generated by the reaction will not wrap the unreacted ITO waste target powder.
[0073] In some embodiments, the flow rate of hydrogen is 300-1000 mL / min.
[0074] In some embodiments, the temperature of the reaction crucible is 800-1000°C.
[0075] The technical details are further illustrated below in conjunction with embodiments.
[0076] Example 1
[0077] Figure 1 This is a schematic structural diagram of the device for preparing indium tin alloy using ITO waste targets disclosed in Example 1; Figure 2 It is a schematic diagram of the structure of the reaction crucible disclosed in Example 1; Figure 3 It is a schematic diagram of the structure of the receiving crucible disclosed in Example 1; Figure 4 This is a reaction principle diagram of the method for preparing indium tin alloy using ITO waste target disclosed in Example 1.
[0078] like Figures 1 to 4 As shown, the device for preparing indium tin alloy using ITO waste target includes a reaction crucible 1, a receiving crucible 2 connected to the bottom of the reaction crucible 1, a heating jacket 3 sleeved on the outer surface of the reaction crucible 1, and a cover plate 4 covered on the top of the reaction crucible 1;
[0079] Among them, a plurality of through holes 11 are opened through the bottom of the reaction crucible 1, a temperature sensor 6 and a pressure sensor 7 are arranged inside the reaction crucible 1, and an ear handle 8 is arranged on the two side walls of the reaction crucible 1 respectively; the receiving crucible 2 is connected with the internal cavity of the reaction crucible 1 through the through hole 11, a circle of limiting bars 22 for placing the reaction crucible 1 is arranged on the inner wall of the receiving crucible 2, an air inlet 21 is opened on the right side wall of the receiving crucible 2, and the air inlet 21 is connected to the air supply component 5; an air outlet 41 is opened on the cover plate 4.
[0080] The method for preparing indium tin alloy using ITO waste target includes:
[0081] Taking a set amount of ITO waste target powder and pressing it into an ITO waste target block;
[0082] Putting the ITO waste target block 100 into the reaction crucible 1;
[0083] Start the gas supply assembly 5 to introduce hydrogen into the reaction crucible 1;
[0084] Start the heating jacket 3 to heat the reaction crucible 1 to a set temperature;
[0085] Hydrogen H2 enters the receiving crucible 2 from the gas inlet 21 of the receiving crucible 2, and then enters the reaction crucible 1 upward through the through hole 11 at the bottom of the reaction crucible 1, and continuously contacts and reacts with the bottom of the ITO waste target block 100 at the bottom of the reaction crucible 1 to generate liquid indium tin alloy 200 and water vapor H2O;
[0086] The generated liquid indium-tin alloy 200 drips downward through the through hole 11 at the bottom of the reaction crucible 1 and is collected in the receiving crucible 2 , and the generated water vapor H 2 O is discharged from the reaction crucible 1 through the gas outlet 41 on the cover plate 4 .
[0087] Example 2
[0088] Figure 5 is the XRD pattern of the indium tin alloy disclosed in Example 2; Figure 6 This is a SEM image of the indium tin alloy disclosed in Example 2.
[0089] 10 grams of ITO waste target powder was placed in a mold with a diameter of 25 mm and pre-pressed with a tablet press at a molding pressure of 15 MPa. The pre-formed ITO waste target powder was then vacuum-sealed and placed in a cold isostatic press for uniform compression at a compression pressure of 100 MPa to obtain a tightly bonded ITO waste target block.
[0090] The ITO waste target block is placed in a reaction crucible, and the through hole diameter at the bottom of the reaction crucible is 5 mm;
[0091] Hydrogen was introduced into the reaction crucible at a flow rate of 1000 mL / min; the reaction crucible was heated to 800° C. and kept at this temperature for 2 hours;
[0092] Hydrogen enters the receiving crucible from the air inlet of the receiving crucible, and then enters the reaction crucible upward through the through hole at the bottom of the reaction crucible, and continuously contacts and reacts with the bottom of the ITO waste target block at the bottom of the reaction crucible to generate liquid indium tin alloy. The generated liquid indium tin alloy drips downward from the through hole at the bottom of the reaction crucible and is collected in the receiving crucible to cool and form into indium tin alloy. The obtained indium tin alloy is tested and analyzed, such as Figure 5 As shown, the phase structure of indium tin alloy is In 0.87 Sn 0.13 ;like Figure 6 As shown, the density of indium tin alloy is good. Figure 6 The spectra of points 1 to 3 are analyzed, and the analysis results are shown in Table 1 below:
[0093] Table 1 Spectral analysis results
[0094]
[0095] Example 3
[0096] Figure 7 is the XRD pattern of the indium tin alloy disclosed in Example 3; Figure 8 This is a SEM image of the indium tin alloy disclosed in Example 3.
[0097] 10 grams of ITO waste target powder was placed in a mold with a diameter of 25 mm and pre-pressed with a tablet press at a molding pressure of 15 MPa. The pre-formed ITO waste target powder was then vacuum-sealed and placed in a cold isostatic press for uniform compression at a compression pressure of 100 MPa to obtain a tightly bonded ITO waste target block.
[0098] The ITO waste target block is placed in a reaction crucible, and the through hole diameter at the bottom of the reaction crucible is 5 mm;
[0099] Hydrogen was introduced into the reaction crucible at a flow rate of 300 mL / min; the reaction crucible was heated to 1000° C. and kept at this temperature for 1 hour;
[0100] Hydrogen enters the receiving crucible from the air inlet of the receiving crucible, and then enters the reaction crucible upward through the through hole at the bottom of the reaction crucible, and continuously contacts and reacts with the bottom of the ITO waste target block at the bottom of the reaction crucible to generate liquid indium tin alloy. The generated liquid indium tin alloy drips downward from the through hole at the bottom of the reaction crucible and is collected in the receiving crucible to cool and form into indium tin alloy. The obtained indium tin alloy is tested and analyzed, such as Figure 7 As shown, the phase structure of indium tin alloy is In 0.87 Sn 0.13 ;like Figure 8 As shown, the density of indium tin alloy is good. Figure 8 The spectra of points 1 to 3 are analyzed, and the analysis results are shown in Table 2 below:
[0101] Table 2 Spectral analysis results
[0102]
[0103] The method and device for preparing indium tin alloy using ITO waste targets disclosed in the embodiment of the present invention have multiple through holes in the bottom of the reaction crucible, so that hydrogen flows upward through the through holes from the receiving crucible and contacts and reacts with the bottom of the ITO waste target block set in the reaction crucible. The bottom of the ITO waste target block reacts and melts out, exposing the unreacted part to continue to react with hydrogen. The liquid indium tin alloy generated by the reaction drips downward from the through holes at the bottom of the reaction crucible to the receiving crucible for collection. The method and device for preparing indium tin alloy using ITO waste targets disclosed in the embodiment of the present invention solves the problem that the liquid indium tin alloy generated by the reaction wraps the unreacted ITO waste target powder, improves the reduction rate of the ITO waste target, improves the purity of the indium tin alloy, shortens the reaction time, and reduces energy consumption.
[0104] The technical solutions disclosed in the present invention and the technical details disclosed in the embodiments are merely illustrative of the inventive concept of the present invention and do not constitute a limitation on the technical solutions of the present invention. Any conventional changes, substitutions or combinations of the technical details disclosed in the embodiments of the present invention have the same inventive concept as the present invention and are within the protection scope of the claims of the present invention.
Claims
1. A device for preparing indium tin alloy using ITO waste target, characterized in that: include: A reaction crucible, wherein a plurality of through holes are formed through the bottom of the reaction crucible; the reaction crucible is used for hydrogen reduction of ITO waste target to prepare indium tin alloy; A receiving crucible, wherein an air inlet is provided on the receiving crucible; the receiving crucible is detachably connected to the bottom of the reaction crucible and communicates with the internal volume of the reaction crucible through a plurality of through holes; the receiving crucible is used to collect the prepared indium tin alloy; A heating sleeve, which is sleeved on the outer surface of the reaction crucible and is used to heat the reaction crucible; A gas supply assembly, arranged to be connected to the gas inlet hole of the receiving crucible, for providing hydrogen; A cover plate is arranged on the top of the reaction crucible; the cover plate is provided with a gas outlet hole for discharging water vapor generated by the hydrogen reduction reaction.
2. The device for preparing indium tin alloy using ITO waste target according to claim 1, characterized in that: A temperature sensor is arranged in the reaction crucible.
3. The device for preparing indium tin alloy using ITO waste target according to claim 1, characterized in that: A pressure sensor is arranged in the reaction crucible.
4. The device for preparing indium tin alloy using ITO waste target according to claim 1, characterized in that: A sealing ring is provided at the connection between the reaction crucible and the receiving crucible.
5. The device for preparing indium tin alloy using ITO waste target according to claim 1, characterized in that: The diameter of the through hole on the reaction crucible is 5 to 10 mm.
6. The device for preparing indium tin alloy using ITO waste target according to claim 1, characterized in that: The cross-sectional shape of the through hole on the reaction crucible is an inverted trapezoid.
7. The device for preparing indium tin alloy using ITO waste target according to claim 1, characterized in that: Ear handles are arranged on both side walls of the reaction crucible.
8. A method for preparing indium tin alloy using waste ITO targets, using the device as claimed in any one of claims 1 to 7 to prepare indium tin alloy, characterized in that: include: Taking a set amount of ITO waste target powder and pressing it into an ITO waste target block; Putting the ITO waste target block into the reaction crucible; Start the gas supply assembly to introduce hydrogen into the reaction crucible; Start the heating jacket to heat the reaction crucible to the set temperature; The hydrogen enters the receiving crucible from the air inlet of the receiving crucible, then enters the reaction crucible through the through hole at the bottom of the reaction crucible, and contacts and reacts with the bottom of the ITO waste target block at the bottom of the reaction crucible; The bottom of the ITO waste target block reacts with hydrogen to generate liquid indium tin alloy and water vapor; the generated liquid indium tin alloy drips downward through the through hole at the bottom of the reaction crucible and is collected in the receiving crucible, and the generated water vapor flows upward through the gas outlet hole on the cover plate and is discharged from the reaction crucible; The unreacted portion of the bottom of the ITO waste target block continues to react with the hydrogen gas until the ITO waste target block is completely consumed.
9. The method for preparing indium tin alloy using ITO waste target according to claim 8, characterized in that: The flow rate of the hydrogen is 300-1000 mL / min.
10. The method for preparing indium tin alloy using ITO waste target according to claim 8, characterized in that: The temperature of the reaction crucible is 800-1000°C.
Citation Information
Patent Citations
Method for recycling indium from waste ITO target material through reduction method
CN105420756A
Method of recovering metal indium from ITO waste target
CN109762993A
Process method for extracting indium and tin from indium tin oxide (ITO) waste target
CN109957655A
Method for preparing single crystal tungsten powder by reducing tungsten oxide through hydrogen homodromous diffusion
CN116921666A
Device for recovering indium tin alloy in ITO waste target
CN218502934U