Cobalt-doped electrochromic fiber and preparation method thereof
By depositing a cobalt-doped tungsten trioxide electrochromic layer on flexible conductive fibers, the problems of insufficient color changes and insufficient stability of existing electrochromic materials are solved, and the diversity and stability of cobalt-doped electrochromic fibers are realized. High cycling stability for smart wearable applications.
Patent Information
- Application Number
- CN202410785019.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-29
AI Technical Summary
Existing electrochromic materials do not have rich color changes under voltage changes, and lack stability and flexibility, making it difficult to meet the application needs of smart wearables and smart clothing.
Flexible conductive fiber is used as the base material, and a constant voltage electrochemical treatment is performed on the surface of the fiber through a three-electrode system to deposit a dense cobalt-doped tungsten trioxide electrochromic layer, and the cobalt ions in the sodium tungstate solution are used to form a variety of Color changes.
The prepared cobalt-doped electrochromic fiber has good flexibility, fast response time, multiple color changes and excellent cycle stability, and is suitable for smart fabrics and flexible smart wearable electronic devices.
Smart Images

Figure CN118854401A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrochromic fibers, and in particular to a cobalt-doped electrochromic fiber and a preparation method thereof. Background Art
[0002] Electrochromic technology adjusts the color effect by adjusting the voltage autonomously. It has the advantages of short response time and rich color changes. Therefore, electrochromic materials have gradually become a research hotspot. The current electrochromic materials mainly include a substrate layer, an electrochromic layer and an electrolyte layer. The electrochromic material undergoes an oxidation-reduction reaction by allowing the ions in the electrolyte to penetrate into the electrochromic layer. The electrochromic material will show different color changes in different states, thereby achieving the goal of changing the voltage to make the electrochromic material show different color changes.
[0003] The combination of electrochromic and fiber has greatly expanded the application prospects of electrochromic. As a new type of functional material, electrochromic fiber has a wide range of uses in electronics, displays, military industry, clothing and medical treatment.
[0004] Electrochromic materials can be divided into organic materials, inorganic materials and composite materials. Inorganic materials are widely studied because of their large color contrast and obvious color rendering effect. Tungsten trioxide is a cathode coloring material among inorganic electrochromic materials. It can maintain the coloring state under the stimulation of negative voltage. Tungsten trioxide has a stable structure and can be cathode colored in both crystalline and amorphous states. Therefore, tungsten trioxide is widely studied in the field of electrochromism. Summary of the invention
[0005] The purpose of the present invention is to provide a cobalt-doped electrochromic fiber and a preparation method thereof, wherein a flexible conductive fiber is used as a substrate, and an electrochromic material is deposited on the surface of the substrate at a constant voltage using a three-electrode system, so that a dense electrochromic layer is formed on the surface of the flexible conductive fiber. The electrochromic fiber prepared by the present invention has good flexibility, stable color change performance and multiple color changes, and has good application prospects in the fields of smart wearables, smart clothing and wearable sensing.
[0006] To achieve the above object, the present invention provides a method for preparing cobalt-doped electrochromic fibers, comprising the following steps:
[0007] S1, performing surface treatment and hydrophilic treatment on the conductive fiber substrate to obtain a fiber with hydroxyl groups attached to the surface;
[0008] S2, preparing a sodium tungstate solution, wherein the solvent of the sodium tungstate solution is deionized water;
[0009] S3, adding cobalt nitrate solution, hydrogen peroxide and sulfuric acid to the sodium tungstate solution prepared in step S2 to prepare a precursor solution;
[0010] S4, placing the fiber treated in step S1 in the precursor solution prepared in step S3, and performing electrochemical treatment for 30-300s using a three-electrode system; the electrochemical treatment process includes the following contents: using the fiber obtained in step S1 as the positive electrode, the platinum electrode as the negative electrode, the calomel electrode as the reference electrode, and the precursor solution prepared in step S3 as the electrolyte, and performing constant voltage electrochemical treatment;
[0011] S5, naturally drying the fiber obtained in step S4 to obtain electrochromic fiber.
[0012] Furthermore, in the precursor solution prepared in step S3, the concentration of sodium tungstate is 0.1-0.5 mol / L.
[0013] Furthermore, in step S3, the amount of cobalt nitrate added is 0.001-0.05 mol / L.
[0014] Furthermore, in step S4, the voltage of the constant voltage electrochemical treatment is -0.5V to -1V.
[0015] Furthermore, in the precursor solution prepared in step S3, the concentration of sulfuric acid is 0.3-0.6 mol / L, and the concentration of hydrogen peroxide is 5-8 mol / L.
[0016] Furthermore, in step S1, the hydrophilic treatment refers to using the surface treated fiber as the positive electrode, the platinum electrode as the negative electrode, and the potassium hydroxide solution as the electrolyte, and obtaining the fiber with hydroxyl groups attached to the surface after the electrical treatment.
[0017] Furthermore, the electrolyte potassium hydroxide solution has a concentration of 2-3 mol / L, a power-on time of 5-6 min, and a voltage of 5-6V.
[0018] Furthermore, in step S1, the surface treatment refers to placing the fiber to be treated into a beaker containing anhydrous ethanol solution, taking it out after ultrasonic vibration for 10 to 20 minutes, and then rinsing it with deionized water and drying it to obtain a fiber with a clean surface.
[0019] Furthermore, the conductive fiber is stainless steel fiber.
[0020] To achieve the above-mentioned purpose, the present invention further provides a cobalt-doped electrochromic fiber, which is prepared by the preparation method described in any of the technical solutions in the aforementioned technical solutions.
[0021] The beneficial effects of the present invention are:
[0022] 1. The preparation method of cobalt-doped electrochromic fiber provided by the present invention is to perform surface treatment and hydrophilic treatment on the fiber substrate to make the fiber surface clean and attached with hydroxyl groups; the treated fiber is placed in a prepared sodium tungstate precursor solution doped with cobalt, and a three-electrode system is used to perform constant voltage deposition on the fiber to deposit a dense electrochromic layer on the fiber surface, thereby obtaining an electrochromic fiber. The present invention obtains a cobalt-doped tungsten trioxide electrochromic layer by doping cobalt ions in a sodium tungstate solution and electropolymerizing the fiber surface, which exhibits a variety of color changes under different voltages. The prepared electrochromic fiber has good flexibility, fast response time, multiple color changes, high color contrast and excellent cycle stability, and has broad application prospects in the fields of smart fabrics, flexible smart wearable electronic devices, etc.
[0023] 2. The electrochromic fiber prepared by the present invention can present different color changes in the electrolyte at different voltages, with high color contrast, fast coloring time and good color memory. When a constant voltage of -0.4V is applied to the electrochromic fiber, it presents blue; when a constant voltage of 0.8V is applied to the color-changing fiber, it presents transparent colorless; when a constant voltage of 1.2V is applied to the color-changing fiber, it presents yellow. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is an electron microscope image of the stainless steel substrate used in Example 1.
[0025] Figure 2 This is an electron microscope image of the electrochromic stainless steel fiber prepared in Example 1.
[0026] Figure 3 This is the CV cycle curve of the electrochromic stainless steel fiber prepared in Example 1.
[0027] Figure 4 This is a chronoamperometry cycle test curve of the electrochromic stainless steel fiber prepared in Example 1.
[0028] Figure 5 This is a color comparison chart of the electrochromic stainless steel fiber prepared in Example 1 under different voltages. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0030] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0031] The present invention provides a method for preparing a cobalt-doped electrochromic fiber, comprising the following steps:
[0032] S1, performing surface treatment and hydrophilic treatment on the conductive fiber substrate to obtain a fiber with hydroxyl groups attached to the surface;
[0033] The conductive fiber is stainless steel fiber.
[0034] Specifically, the surface treatment refers to placing the fiber to be treated in a beaker containing anhydrous ethanol solution, taking it out after ultrasonic vibration for 10 to 20 minutes, and then rinsing it with deionized water and drying it to obtain a fiber with a clean surface.
[0035] Hydrophilic treatment refers to using the surface treated fiber as the positive electrode, the platinum electrode as the negative electrode, and the potassium hydroxide solution as the electrolyte. The concentration of potassium hydroxide is 2-3 mol / L, and the treatment is carried out at a constant voltage of 5-6V for 2-3 minutes. After the power is applied, the fiber with hydroxyl groups attached to the surface is obtained. The hydrophilic treatment makes a large number of hydroxyl groups exist on the fiber surface.
[0036] S2, preparing a sodium tungstate solution of a certain concentration, wherein the solvent of the sodium tungstate solution is deionized water;
[0037] S3, adding cobalt nitrate solution, hydrogen peroxide and sulfuric acid to the sodium tungstate solution prepared in step S2 to prepare a precursor solution;
[0038] Specifically, the precursor solution is a mixed solution including sodium tungstate, hydrogen peroxide, sulfuric acid and cobalt nitrate, wherein the concentration of sodium tungstate is 0.1-0.5 mol / L, the concentration of sulfuric acid is 0.3-0.6 mol / L, the concentration of hydrogen peroxide is 5-8 mol / L, and the concentration of cobalt nitrate is 0.001-0.05 mol / L.
[0039] S4, placing the fiber treated in step S1 in the sodium tungstate solution prepared in step S3, and performing electrochemical treatment for 30-300s using a three-electrode system; the electrochemical treatment process includes the following contents: using the fiber obtained in step S1 as the positive electrode (working electrode), the platinum electrode as the negative electrode (counter electrode), the calomel electrode as the reference electrode, and the precursor solution prepared in step S3 as the electrolyte, and performing constant voltage electrochemical treatment.
[0040] Specifically, the electrochemical workstation treats the fiber at a constant voltage of -0.5 to -1 V. The use of electrochemical polymerization can make the thickness of the electrochromic layer uniform and have strong adhesion to the substrate, which greatly improves the color-changing performance of the final electrochromic fiber. The voltage and deposition time both affect the structure of the electrochromic fiber.
[0041] In particular, the fiber is hydrophilically treated to increase the amount of hydroxyl groups on the fiber surface, thereby increasing the degree of electrochemical reaction and enhancing the adhesion between the electrochromic layer and the fiber substrate; cobalt ions are doped so that the cobalt ions occupy the position of tungsten atoms, forming more active sites to participate in the redox reaction, thereby improving the overall conductivity and electrochromic properties of the fiber.
[0042] S5, naturally drying the fiber obtained in step S4 to obtain electrochromic fiber.
[0043] The preparation method of the cobalt-doped electrochromic fiber provided by the present invention is described below with reference to specific embodiments.
[0044] Example 1
[0045] This embodiment provides a method for preparing a cobalt-doped electrochromic fiber, comprising the following steps:
[0046] S1, put the stainless steel fiber into anhydrous ethanol for ultrasonic cleaning for 15 minutes. After cleaning, use the clean fiber as the anode and the platinum electrode as the cathode, put it into 2.5 mol / L potassium hydroxide solution and pass 5V voltage for 2 minutes to obtain clean hydrophilic fiber, which is naturally dried and stored for later use.
[0047] S2, prepare 0.3 mol / L sodium tungstate solution, the solvent of the sodium tungstate solution is deionized water;
[0048] S3, heating the sodium tungstate solution prepared in step S2 in a water bath for 30 minutes, adding 0.5 mol / L concentrated sulfuric acid after cooling, and adding hydrogen peroxide dropwise after the reaction is complete until the sodium tungstate solution is clear, and then adding 0.005 mol / L cobalt nitrate to the solution to obtain a sodium tungstate precursor solution.
[0049] S4, take the fiber treated in step S1 as the working electrode, the platinum electrode as the counter electrode, and the calomel electrode as the reference electrode to form a three-electrode system, use the sodium tungstate precursor solution prepared in step S3 as the electrolyte, use an electrochemical workstation, and pass a constant voltage of -0.7V in a constant voltage mode for 60s to obtain a stainless steel electrochromic fiber with a layer of electrochromic material completely wrapped on the surface. After taking it out, rinse it with anhydrous ethanol and deionized water, and obtain the electrochromic fiber after drying.
[0050] See also Figure 1 , which is an electron microscope image of the stainless steel fiber substrate used in Example 1. It can be seen from the image that the stainless steel fiber has a smooth surface structure before being treated. Figure 2This is an electron microscope image of the electrochromic stainless steel fiber prepared in Example 1. It can be seen from the image that the surface of the stainless steel fiber is coated with a layer of tungsten trioxide electrochromic layer, indicating that this example successfully prepared a densely structured electrochromic stainless steel fiber.
[0051] See also Figure 3 As shown, the CV cycle performance test of the electrochromic stainless steel fiber prepared in Example 1, the curve presents the redox peak of tungsten trioxide at 0.03V, indicating that the color change of the electrochromic stainless steel fiber is mainly caused by the change of the redox state of the electrochromic material.
[0052] See also Figure 4 As shown in FIG. 1 , the 50-cycle chronoamperometry test curve of the electrochromic stainless steel fiber prepared in Example 1 is shown. The curve shows that the maximum current density of the electrochromic stainless steel fiber remains basically unchanged after 50 cycles, and is maintained at 100.00 mA / cm 2 This indicates that the electrochromic stainless steel fiber prepared in this example has good electrical cycle stability.
[0053] Figure 5 This is a color comparison diagram of the electrochromic stainless steel fiber prepared in Example 1 under different voltages. It can be seen that from left to right, when a constant voltage of -0.4V is applied to the color-changing fiber, it appears blue; when a constant voltage of 0.8V is applied to the color-changing fiber, it appears transparent and colorless; when a constant voltage of 1.2V is applied to the color-changing fiber, it appears yellow.
[0054] Comparative Example 1
[0055] Comparative Example 1 provides a method for preparing cobalt-doped electrochromic fibers. Compared with Example 1, the difference is that in step S3, no cobalt nitrate is added to the prepared sodium tungstate precursor solution, and the rest is substantially the same as Example 1 and will not be repeated here.
[0056] Example 2-3 and Comparative Example 2-3
[0057] The main difference between Example 2-3 and Comparative Example 2-3 and Example 1 is that the concentrations of sodium tungstate, sulfuric acid, hydrogen peroxide and cobalt nitrate in the sodium tungstate precursor solution in step S3 are changed, as shown in Table 1 below. The rest is roughly the same as Example 1 and will not be repeated here.
[0058] Table 1
[0059]
[0060]
[0061] Examples 4-7 and Comparative Examples 4-5
[0062] The main difference between Examples 4-7 and Comparative Examples 4-5 and Example 1 is that the process parameters in the constant voltage electrochemical treatment in step S4 are changed, as shown in Table 2 below. The rest are roughly the same as Example 1 and will not be repeated here.
[0063] Table 2
[0064] Constant voltage Constant voltage deposition time Example 1 -0.7V 60s Example 4 -0.7V 30s Example 5 -0.7V 120s Example 6 -0.5V 300s Example 7 -1V 60s Comparative Example 4 -2V 60s Comparative Example 5 1V 60s
[0065] Comparative Examples 6-7
[0066] The main difference between Comparative Example 6-7 and Example 1 is that the solvent of sodium tungstate in step S2 is changed, the solvent used in Comparative Example 6 is ethanol, and the solvent used in Comparative Example 7 is methanol. The rest is substantially the same as Example 1 and will not be repeated here.
[0067] The sensitivity and mechanical strength of the electrochromic fibers prepared in Examples 1-7 and Comparative Examples 1-11 were tested, and the results are shown in Table 3.
[0068] Table 3
[0069]
[0070]
[0071] By comparing Example 1 with Comparative Example 1, it can be seen that doping with cobalt ions improves the color change diversity. The electrochromic fiber doped with cobalt ions can respectively show blue, colorless and yellow under different voltages, while in Comparative Example 1, no cobalt ions are doped, and the electrochromic fiber only shows a change from blue to colorless under different voltages; the tensile strength of the tungsten trioxide composite electrochromic material doped with cobalt ions is slightly higher than that of the single tungsten trioxide electrochromic material; the coloring / bleaching time of the composite material doped with cobalt ions is longer than that of the single tungsten trioxide, and the deposition time will have a certain influence on the strength and coloring / bleaching time of the electrochromic fiber.
[0072] By comparing Examples 1-3 with Comparative Examples 2-3, it can be seen that if the concentration of doped cobalt ions is too high, the deposition of the color-changing layer will be too thick, resulting in slow ion interpenetration, slowing down the redox reaction of the color-changing layer and prolonging the coloring / bleaching time; if the concentration of doped cobalt ions is too low, the number of cobalt ions participating in the chemical reaction will be reduced, resulting in the color of the electrochromic fiber failing to change to yellow, but changing from blue to colorless.
[0073] By comparing Examples 1, 4-7 with Comparative Examples 4-5, it can be seen that the longer the constant voltage deposition time, the greater the deposition voltage, the thicker the electrochromic layer, the higher the tensile strength, and the longer the color change time of the fiber; by comparing Example 7 with Comparative Example 5, it can be seen that an electrochemical reaction will only occur when deposited under a negative voltage, and the electrochromic layer can be successfully deposited.
[0074] Comparing Example 1 with Comparative Examples 6-7, it can be seen that sodium tungstate is not soluble in ethanol and methanol, and cannot be electrochemically deposited on the fiber surface, thereby failing to obtain electrochromic fibers.
[0075] Comparing Example 1 with Comparative Examples 8 to 11, it can be seen that the concentrations of sulfuric acid and hydrogen peroxide are too high or too low, resulting in an oversaturated solution reaction in the precursor solution to form tungstic acid precipitation, or an insufficient reaction resulting in the inability to deposit the electrochromic material on the fiber surface.
[0076] In summary, the present invention provides a method for preparing cobalt-doped electrochromic fibers, using flexible conductive fibers as substrates, using a three-electrode system to deposit electrochromic materials on the surface of the fiber substrate, so that a dense electrochromic layer is formed on the surface of the flexible conductive fibers; the prepared electrochromic fibers have good flexibility, diverse color changes, and excellent cycle stability. The present invention adopts an electrochemical polymerization method, and uses a constant voltage method to perform electropolymerization in a sodium tungstate solution doped with a small amount of cobalt nitrate, so that a dense electrochromic film can be formed on the fiber surface. The prepared electrochromic fibers can display different color changes under different voltages, have bright colors, excellent color change performance, long-term color memory, and other characteristics, and can have broad application prospects in wearable devices, visual sensing, and smart fabrics.
[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing cobalt-doped electrochromic fibers, characterized in that: The following steps are involved: S1, performing surface treatment and hydrophilic treatment on the conductive fiber substrate to obtain a fiber with hydroxyl groups attached to the surface; S2, preparing a sodium tungstate solution, wherein the solvent of the sodium tungstate solution is deionized water; S3, adding cobalt nitrate solution, hydrogen peroxide and sulfuric acid to the sodium tungstate solution prepared in step S2 to prepare a precursor solution; S4, placing the fiber treated in step S1 in the precursor solution prepared in step S3, and performing electrochemical treatment for 30-300s using a three-electrode system; the electrochemical treatment process includes the following contents: using the fiber obtained in step S1 as the positive electrode, the platinum electrode as the negative electrode, the calomel electrode as the reference electrode, and the precursor solution prepared in step S3 as the electrolyte, and performing constant voltage electrochemical treatment; S5, naturally drying the fiber obtained in step S4 to obtain electrochromic fiber.
2. The method for preparing cobalt-doped electrochromic fiber according to claim 1, characterized in that: In the precursor solution prepared in step S3, the concentration of sodium tungstate is 0.1-0.5 mol / L.
3. The method for preparing cobalt-doped electrochromic fiber according to claim 1, characterized in that: In step S3, the amount of cobalt nitrate added is 0.001-0.05 mol / L.
4. The method for preparing cobalt-doped electrochromic fiber according to claim 1, characterized in that: In step S4, the voltage of the constant voltage electrochemical treatment is -0.5V to -1V.
5. The method for preparing cobalt-doped electrochromic fiber according to claim 1, characterized in that: In the precursor solution prepared in step S3, the concentration of sulfuric acid is 0.3-0.6 mol / L, and the concentration of hydrogen peroxide is 5-8 mol / L.
6. The method for preparing cobalt-doped electrochromic fiber according to claim 1, characterized in that: In step S1, the hydrophilic treatment refers to using the surface treated fiber as the positive electrode, the platinum electrode as the negative electrode, and the potassium hydroxide solution as the electrolyte, and obtaining the fiber with hydroxyl groups attached to the surface after the electrical treatment.
7. The method for preparing cobalt-doped electrochromic fibers according to claim 6, characterized in that: The electrolyte potassium hydroxide solution has a concentration of 2-3 mol / L, a power-on time of 5-6 min, and a voltage of 5-6V.
8. The method for preparing cobalt-doped electrochromic fiber according to claim 1, characterized in that: In step S1, the surface treatment refers to placing the fiber to be treated into a beaker containing anhydrous ethanol solution, taking it out after ultrasonic vibration for 10 to 20 minutes, and then rinsing it with deionized water and drying it to obtain a fiber with a clean surface.
9. The method for preparing cobalt-doped electrochromic fiber according to claim 1, characterized in that: The conductive fibers are stainless steel fibers.