All-cotton high-count heavy-twist yarn knitted pique fabric and production process thereof
By steaming and washing the yarn, combined with high-gauge looms and modified mercerizing machines, the back-twist problem of high-count and strong-twisted yarns during the weaving process was solved, improving the quality and production efficiency of the fabric, and realizing The production of high-count, strong-twisted yarn knitted pique fabrics with soft yet stiff texture and smooth surface.
Patent Information
- Application Number
- CN202411328459.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult to effectively produce knitted fabrics with high counts and strong twist yarns using existing technology. The fabrics are prone to back-twisting during the weaving process, resulting in yarn breakage, and have a hard hand feel, poor appearance and poor wearing properties.
Using 100s/2 strong twisted yarn, the twist coefficient is between 450 and 550. The yarn twist level is optimized through steaming and washing. It is woven using a high-gauge single-sided circular knitting machine and a customized detwister, combined with the modified mercerization Machinery and dyeing and finishing processes, including singeing, washing, mercerization, dyeing, tentering and preshrinking, reduce yarn stiffness and friction coefficient, improve weaving efficiency and fabric feel.
The weaving efficiency and quality are significantly improved, the texture is fine and refined, yarn twisting and breakage are reduced, the dimensional stability and feel of the fabric are improved, and the stability and adaptability of the production process are enhanced.
Smart Images

Figure CN118854531A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textile processing, and in particular relates to a pure cotton high-count strong-twisted yarn knitted pique fabric and a production process thereof. Background Art
[0002] The twist of high-twist yarn is generally about twice that of ordinary yarn. It has the advantages of good yarn uniformity and less hairiness. The fabric produced not only has the moisture absorption and skin-friendly properties of cotton fiber, but also has the crispness and smoothness of linen fiber. It also has a certain contact coolness function. The fabric has a unique style and good application prospects. However, high-twist yarn has high rigidity and high friction coefficient. When weaving on a knitting loom, it is easy to cause back twisting and yarn breakage, especially when weaving on a high-count loom, the knitting needles are seriously damaged. The market demand for high-count high-twist yarn is high, but the production feasibility is low, so it is imperative to study it.
[0003] Patent CN109487472A provides a method for preparing a high-count, high-twist, knitted double-sided fabric of pure cotton. s / 2 strong twist knitting yarn is used as raw material, and a double-sided circular machine is used as the loom. After weaving, the cloth is first scouring and bleaching, followed by mercerizing, dyeing, and shaping to obtain a cotton high-count strong twist knitted double-sided cloth. However, the article does not explain the yarn twist coefficient parameters, and it is impossible to determine whether the yarn is a strong twist yarn, so it is impossible to estimate the weaving difficulty. The machine model used is coarse and the fabric surface is poor in fineness. The mercerizing process after scouring and bleaching is used, which has a hard feel and is prone to fabric scratches during dyeing, and has poor appearance and wearing performance.
[0004] Patent CN112481788A provides a production process for strongly twisted fiber knitted clothing, which uses silver ion fiber, cotton thread and polyester fiber to twist into strongly twisted fiber, and weaves it into fabric on a flat knitting machine to make ready-made clothing. However, the article does not describe the yarn count and twist coefficient parameters, and it is impossible to determine whether the yarn is strongly twisted yarn. The loom used in production is a flat knitting machine with a low machine number, which is easy to weave, and the fabric is mostly used in protective occasions, and its use in leisure and daily scenes is limited.
[0005] Patent CN102071534A provides a high-twist yarn conveying device, patents CN102011257A, CN102011266A, and CN102121162A provide a yarn anti-knot device for a knitting machine, and patent CN217052525U discloses a high-strength polyester-cotton composite knitted grey fabric twisting device. These patented technologies belong to weaving equipment research and do not mention the specific weaving production process technology of the fabric. It is impossible to judge whether they are helpful for weaving production and have no reference value.
[0006] It can be seen that the current research on high-twist yarn is mainly concentrated on loom equipment, such as yarn conveying devices, yarn anti-knot devices, etc., and there is little research on high-count high-twist yarn knitted fabrics and their production processes. Summary of the invention
[0007] The technical problem to be solved by the present invention is to provide a pure cotton high-count strong twist yarn knitted pique fabric, which has the combined advantages of cotton and linen, is soft and stiff, has a smooth surface, and has an increased cooling function.
[0008] The invention also provides a production process thereof, which improves the production efficiency of the pure cotton high-count strong-twisted yarn.
[0009] The production process of the pure cotton high-count strong-twisted yarn knitted pique fabric of the present invention comprises the following steps: Spinning → yarn steaming → washing → weaving → dyeing and finishing; The spinning process: the yarn count is 100 s / 2 Strong twist yarn, twist coefficient is 450~550; The water washing step includes adding softener for water washing; The weaving process comprises the following steps: using a high-number single-sided large circular machine for weaving, the machine number is 32G-36G, the length of one hundred turns of grey cloth is 21.5cm-22cm, the untwisting device used for weaving comprises a yarn inlet porcelain mouth, four yarn threading holes, two yarn winding shafts, and a yarn outlet porcelain mouth, and the yarn threading route is yarn inlet porcelain mouth→yarn threading hole→yarn winding shaft→yarn threading hole→yarn threading hole→yarn winding shaft→yarn threading hole→yarn outlet porcelain mouth.
[0010] The yarn twist is large, and when the tension is small, the yarn will be twisted together due to self-untwisting. In order to weave smoothly, we can start from the angle of keeping the yarn straight. Through the design of the zigzag threading path, a pulling force is added to the yarn during the weaving process to prevent the yarn from unwinding from the bobbin or the yarn twisting caused by uneven tension when the machine is stopped; the yarn threading turns use two methods: threading holes and winding shafts. The threading holes can provide force points for the yarn, and the winding shaft can make yarns with different twists wind different numbers of turns, which is more in line with the requirements of actual production.
[0011] The threading route diagram of the fabric loom untwist device is as follows Figure 2 shown.
[0012] The raw material of the spinning process is 100% long-staple cotton, and the spinning method is compact spinning.
[0013] The yarn steaming process has a temperature of 95° C. to 105° C. and a time of 25 min to 35 min.
[0014] The water washing process: the water washing temperature is 90°C to 100°C, and the water washing time is 25min to 35min.
[0015] The weaving process: the woven fabric is a single beaded fabric, and the weaving pattern of the fabric is as follows Figure 1 shown.
[0016] The softener is a silicone oil softener, and the added amount is 4% owf to 5% owf.
[0017] The dyeing and finishing process includes the following processes: Singeing → washing → mercerizing → dyeing → stretching → pre-shrinking.
[0018] The mercerizing machine used in the mercerizing process replaces the rollers with mesh belts in the needle plate area. The mesh on the mesh belt allows liquid to pass through, making it easier to remove alkali from the fabric. The comparison of the needle plate area of the mercerizing machine before and after the transformation is shown in the figure below. Figure 3 As shown in the figure, the stress changes of the fabric in the spraying part before and after the mercerizing machine transformation are compared as shown in the figure. Figure 4 shown.
[0019] The mercerizing method adopts light alkali mercerizing, the mercerizing alkali concentration is 12Be~18Be, the mercerizing machine speed is 25m / min~35m / min, the mercerizing overfeed is 20%~30%, and the mercerizing washing temperature is 50℃~70℃.
[0020] The washing process in the dyeing and finishing process: the speed is 35m / min~40m / min.
[0021] The singeing process includes: a vehicle speed of 65 m / min to 75 m / min, a cutting method for singeing, and a flame intensity of 10 mbar to 14 mbar.
[0022] The dyeing includes scouring, bleaching and dyeing, using an O-type overflow dyeing machine, with a motor speed of 1000 r / min~1500 r / min, a cloth lifting speed of 80 m / min~90 m / min, a nozzle opening size of 30%~40%, soda ash 4g / L~5g / L, hydrogen peroxide 7g / L~8g / L, a leveling agent 1g / L~3g / L, alumina sulfate 8g / L~12g / L, a dyeing temperature of 55°C~65°C, and a dyeing time of 30min~50min.
[0023] The tentering speed is 35m / min~45m / min, the tentering pressure is 25bar~35bar, the tentering drying room temperature is 130℃~150℃, and the additives include neutralized acid pH regulator PH-X: 3g / L~5g / L, silicone oil softener SMI-60: 50g / L~80g / L, and the balance is water.
[0024] The pre-shrinking speed is 25m / min-30m / min, and the pre-shrinking blanket temperature is 90°C-110°C.
[0025] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention steams and washes the yarn before weaving, thereby optimizing the yarn twist level, reducing the yarn stiffness, and reducing the yarn friction coefficient, thereby significantly improving the efficiency and quality of subsequent weaving.
[0026] (2) The invention adopts high machine gauge + customized untwisting device for weaving, which not only makes the fabric texture fine, delicate and high-grade, but also improves the back-twisting phenomenon in the yarn weaving process, reduces the occurrence of defects such as yarn twisting and breakage, and the weaving efficiency and quality reach the weaving level of yarn with normal twist.
[0027] (3) The present invention uses a modified mercerizing machine, which reduces the sinking force caused by water on the fabric surface, reduces the tension of the entire machine and improves the stability of tension control, improves the longitudinal stretching of the fabric, improves the dimensional stability of the fabric, and effectively improves the feel of the fabric.
[0028] (4) The production process of the present invention has strong stability and is adaptable to the rapid production requirements of large quantities and multiple varieties. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a knitting pattern of the pique fabric knitted with all-cotton high-count and strong-twisted yarns described in the present invention; Figure 2 A yarn threading route diagram of a loom untwister for fabrics of the present invention; In the figure, 1 is the yarn inlet porcelain mouth, 2, 4, 5, 7 are the yarn threading holes, 3, 6 are the yarn winding shafts, and 8 is the yarn outlet porcelain mouth; Figure 3 This is a comparison diagram of the mercerizing machine needle plate area before and after the transformation of the present invention; In the figure, 10 is a roller, 9 is a fabric, and 11 is a support belt; Figure 4 This is a comparison diagram of the stress changes on the fabric at the spraying part of the mercerizing machine before and after the modification of the present invention; In the figure, 12 is a needle plate, 13 is a spray device, and 9 is a fabric. DETAILED DESCRIPTION
[0030] The present invention will be further described below with reference to the embodiments.
[0031] Unless otherwise specified, all raw materials used in the examples are commercially available.
[0032] Mercerizing alkali: caustic soda NaOH, hydrogen peroxide H2O2, leveling agent LARLR, sodium sulfate NA2SO4, neutralizing acid pH regulator PH-X, silicone oil softener SMI-60. The manufacturer is Zibo Lurui Fine Chemical Co., Ltd.
[0033] The cotton described in the embodiments is 100% long-staple cotton.
[0034] Example 1 The production process of knitted pique fabrics made of high-count and high-twisted cotton yarn includes the following steps: Spinning → steaming → washing → weaving → dyeing and finishing.
[0035] Spinning: Cotton: 100s / 2 strong twist yarn, single yarn twist direction Z twist, ply twist direction S twist, number twist coefficient 450, spinning method compact spinning; Yarn steaming: Yarn steaming temperature 95℃, yarn steaming time 25min; Washing: washing temperature 90℃, washing time 35min, adding 4% owf silicone oil softener SMI-60 during washing; Weaving: We selected a high-number single-sided circular machine for weaving, the machine number was 36G, the length of the grey fabric per hundred turns was 21.5cm, the untwisting device used included a yarn inlet porcelain mouth, four yarn threading holes, two yarn winding shafts, and a yarn outlet porcelain mouth. The yarn threading route was yarn inlet porcelain mouth → yarn threading hole → yarn winding shaft → yarn threading hole → yarn threading hole → yarn winding shaft → yarn threading hole → yarn outlet porcelain mouth; the yarn threading route of the untwisting device used is shown in the figure below: Figure 2 As shown, the weaving pattern of the fabric is as follows Figure 1 As shown; Dyeing and finishing: The production process is singeing → washing → mercerizing → dyeing → stentering → pre-shrinking; The singeing speed is 65m / min, the singeing method is cutting and burning, and the flame intensity is 14mbar; Water washing speed 35m / min; The mercerizing machine used for mercerizing replaces the roller with a mesh support belt in the needle plate area. The comparison before and after the transformation of the needle plate area of the mercerizing machine is shown in the figure below. Figure 3 As shown, the alkali concentration is 12Be, the mercerizing speed is 25m / min, the mercerizing overfeed is 20%, and the mercerizing washing temperature is 50℃; The dyeing process includes scouring, bleaching and dyeing, with a motor speed of 1000 r / min, a cloth lifting speed of 80 m / min, a nozzle opening size of 30%, soda ash 4 g / L, hydrogen peroxide 7 g / L, a leveling agent 1 g / L, sodium sulfate 8 g / L, a dyeing temperature of 55° C., a dyeing time of 30 min, a reactive blue dye of 0.0033% owf, a reactive red dye of 0.008% owf, and a reactive yellow dye of 0.007% owf; The tentering speed is 35m / min, the tentering pressure is 25bar, the tentering drying room temperature is 130℃, and the additives are: neutralized acid pH regulator PH-X: 3g / L, silicone oil softener SMI-60: 50g / L, and the balance is water; The pre-shrinking speed is 25m / min, and the pre-shrinking blanket temperature is 90℃.
[0036] Example 2 The production process of knitted pique fabrics made of high-count and high-twisted cotton yarn includes the following steps: Spinning → steaming → washing → weaving → dyeing and finishing.
[0037] Spinning: Cotton: 100 s / 2 strong twist yarn, single yarn twist direction Z twist, ply twist direction S twist, number twist coefficient 500, spinning method compact spinning; Yarn steaming: Yarn steaming temperature 100℃, washing time 30min; Washing: washing temperature 95℃, washing time 30min, adding 4.5% owf silicone oil softener SMI-60 during washing; Weaving: We selected a high-number single-sided circular machine for weaving, the machine number was 36G, the length of the grey fabric per hundred turns was 21.7cm, the untwisting device used included a yarn inlet porcelain mouth, four yarn threading holes, two yarn winding shafts, and a yarn outlet porcelain mouth, and the yarn threading route was yarn inlet porcelain mouth → yarn threading hole → yarn winding shaft → yarn threading hole → yarn threading hole → yarn winding shaft → yarn threading hole → yarn outlet porcelain mouth; the yarn threading route diagram of the untwisting device used is as follows Figure 2 As shown, the weaving pattern of the fabric is as follows Figure 1 As shown; Dyeing and finishing: The production process is singeing → washing → mercerizing → dyeing → stentering → pre-shrinking; The singeing speed is 70m / min, the singeing method is cutting and burning, and the flame intensity is 12mbar; Water washing speed 37m / min; Mercerizing uses the modified mercerizing machine. The comparison of the needle plate area of the mercerizing machine before and after the modification is as follows Figure 3 As shown, the alkali concentration is 15Be, the mercerizing speed is 30m / min, the mercerizing overfeed is 25%, and the mercerizing washing temperature is 60℃; The dyeing includes scouring, bleaching and dyeing, the motor speed is 1250r / min, the cloth lifting speed is 85m / min, the nozzle opening size is 35%, soda ash is 4.5g / L, hydrogen peroxide is 7.5g / L, leveling agent is 2g / L, sodium sulfate is 10g / L, dyeing temperature is 60°C, dyeing time is 40min, reactive blue dye is 0.0033% owf, reactive red dye is 0.065% owf, and reactive yellow dye is 0.004% owf; The tentering speed is 40m / min, the tentering pressure is 30bar, the tentering drying room temperature is 140℃, and the additives are: neutralized acid pH regulator PH-X: 4g / L, silicone oil softener SMI-60: 65g / L, and the balance is water; The pre-shrinking speed is 27m / min, and the pre-shrinking blanket temperature is 100℃.
[0038] Example 3 The production process of knitted pique fabrics made of high-count and high-twisted cotton yarn includes the following steps: Spinning → yarn steaming → washing → weaving → dyeing and finishing.
[0039] Spinning: Cotton: 100 s / 2 strong twist yarn, single yarn twist direction Z twist, ply twist direction S twist, number twist coefficient 550, spinning method compact spinning; Yarn steaming: Yarn steaming temperature 105℃, washing time 35min; Washing: washing temperature 100℃, washing time 25min, adding 5% owf silicone oil softener SMI-60 during washing; Weaving: We selected a high-number single-sided circular machine for weaving, the machine number was 32G, the length of the grey fabric per hundred turns was 22cm, the untwisting device used included a yarn inlet porcelain mouth, four yarn threading holes, two yarn winding shafts, and a yarn outlet porcelain mouth. The yarn threading route was yarn inlet porcelain mouth → yarn threading hole → yarn winding shaft → yarn threading hole → yarn threading hole → yarn winding shaft → yarn threading hole → yarn outlet porcelain mouth; the yarn threading route of the untwisting device used is shown in the figure below: Figure 2 As shown, the weaving pattern of the fabric is as follows Figure 1 As shown; Dyeing and finishing: The production process is singeing → washing → mercerizing → dyeing → stentering → pre-shrinking; The singeing speed is 75m / min, the singeing method is cutting and burning, and the flame intensity is 10mbar; Water washing speed 40m / min; Mercerizing uses the modified mercerizing machine. The comparison of the needle plate area of the mercerizing machine before and after the modification is as follows Figure 3 As shown, the alkali concentration is 18Be, the mercerizing speed is 35m / min, the mercerizing overfeed is 30%, and the mercerizing washing temperature is 70℃; The dyeing process includes scouring, bleaching and dyeing, with a motor speed of 1500 r / min, a cloth lifting speed of 90 m / min, a nozzle opening size of 40%, 5 g / L soda ash, 8 g / L hydrogen peroxide, 3 g / L leveling agent, 12 g / L sodium sulfate, a dyeing temperature of 65°C, a dyeing time of 50 min, 0.0023% owf of reactive blue dye, 0.017% owf of reactive red dye, and 0.192% owf of reactive yellow dye; The tentering speed is 45m / min, the tentering pressure is 35bar, the tentering drying room temperature is 150℃, and the additives are: neutralized acid pH regulator PH-X: 5g / L, silicone oil softener SMI-60: 80g / L, and the balance is water; The pre-shrinking speed is 30m / min, and the pre-shrinking blanket temperature is 110℃.
[0040] Comparative Example 1 The production process of knitted pique fabrics made of high-count and high-twisted cotton yarn includes the following steps: Spinning → steaming → washing → weaving → dyeing and finishing. The difference between this comparative example and Example 1 is that conventional twist yarn is used.
[0041] Spinning: Cotton: 100 s / 2 Ordinary yarn, single yarn twist direction Z twist, ply twist direction S twist, number twist coefficient 350, spinning method compact spinning; Yarn steaming: Yarn steaming temperature 95℃, washing time 25min; Washing: washing temperature 90℃, washing time 35min, adding 4% owf silicone oil softener SMI-60 during washing; Weaving: We selected a high-number single-sided circular machine for weaving, the machine number was 36G, the length of the grey fabric per hundred turns was 21.5cm, the untwisting device used included a yarn inlet porcelain mouth, four yarn threading holes, two yarn winding shafts, and a yarn outlet porcelain mouth. The yarn threading route was yarn inlet porcelain mouth → yarn threading hole → yarn winding shaft → yarn threading hole → yarn threading hole → yarn winding shaft → yarn threading hole → yarn outlet porcelain mouth; the yarn threading route of the untwisting device used is shown in the figure below: Figure 2 As shown, the weaving pattern of the fabric is as follows Figure 1 As shown; Dyeing and finishing: The production process is singeing → washing → mercerizing → dyeing → stentering → pre-shrinking; The singeing speed is 65m / min, the singeing method is cutting and burning, and the flame intensity is 14mbar; Water washing speed 35m / min; Mercerizing uses the modified mercerizing machine. The comparison of the needle plate area of the mercerizing machine before and after the modification is as follows Figure 3 As shown, the alkali concentration is 12Be, the mercerizing speed is 25m / min, the mercerizing overfeed is 20%, and the mercerizing washing temperature is 50℃; The dyeing process includes scouring, bleaching and dyeing, with a motor speed of 1000 r / min, a cloth lifting speed of 80 m / min, a nozzle opening size of 30%, soda ash 4 g / L, hydrogen peroxide 7 g / L, a leveling agent 1 g / L, sodium sulfate 8 g / L, a dyeing temperature of 55° C., a dyeing time of 30 min, a reactive blue dye of 0.0033% owf, a reactive red dye of 0.008% owf, and a reactive yellow dye of 0.007% owf; The tentering speed is 35m / min, the tentering pressure is 25bar, the tentering drying room temperature is 130℃, and the additives are: neutralized acid pH regulator PH-X 3g / L, silicone oil softener SMI-60 50g / L, and the balance is water; The pre-shrinking speed is 25m / min, and the pre-shrinking blanket temperature is 90℃.
[0042] Comparative Example 2 The production process of knitted pique fabrics made of high-count and high-twisted cotton yarn includes the following steps: Spinning → steaming → weaving → dyeing and finishing. The difference between this comparative example and Example 1 is that the yarn was not washed before weaving and the yarn of the present invention was not used. Figure 2 The untwister.
[0043] Spinning: Cotton: 100 s / 2 strong twist yarn, single yarn twist direction Z twist, ply twist direction S twist, number twist coefficient 450, spinning method compact spinning; Yarn steaming: Yarn steaming temperature 95℃, washing time 25min; Weaving: We use a high-gauge single-sided circular machine, the machine gauge is 36G, the length of the grey fabric is 21.5cm, and the weaving pattern of the fabric is as follows: Figure 1 As shown; Dyeing and finishing: The production process is singeing → washing → mercerizing → dyeing → stentering → pre-shrinking; The singeing speed is 65m / min, the singeing method is cutting and burning, and the flame intensity is 14mbar; Water washing speed 35m / min; Mercerizing uses the modified mercerizing machine. The comparison of the needle plate area of the mercerizing machine before and after the modification is as follows Figure 3 As shown, the alkali concentration is 12Be, the mercerizing speed is 25m / min, the mercerizing overfeed is 20%, and the mercerizing washing temperature is 50℃; The dyeing process includes scouring, bleaching and dyeing, with a motor speed of 1000 r / min, a cloth lifting speed of 80 m / min, a nozzle opening size of 30%, soda ash 4 g / L, hydrogen peroxide 7 g / L, a leveling agent 1 g / L, sodium sulfate 8 g / L, a dyeing temperature of 55° C., a dyeing time of 30 min, a reactive blue dye of 0.0033% owf, a reactive red dye of 0.008% owf, and a reactive yellow dye of 0.007% owf; The tentering speed is 35m / min, the tentering pressure is 25bar, the tentering drying room temperature is 130℃, and the additives are: neutralized acid pH regulator PH-X 3g / L, silicone oil softener SMI-60 50g / L, and the balance is water; The pre-shrinking speed is 25m / min, and the pre-shrinking blanket temperature is 90℃.
[0044] Comparative Example 3 The production process of knitted pique fabrics made of high-count and high-twisted cotton yarn includes the following steps: Spinning → yarn steaming → washing → weaving → dyeing and finishing. The difference between this comparative example and Example 1 is that a conventional mercerizing machine without modification is used.
[0045] Spinning: Cotton: 100 s / 2 strong twist yarn, single yarn twist direction Z twist, ply twist direction S twist, number twist coefficient 450, spinning method compact spinning; Yarn steaming: Yarn steaming temperature 95℃, washing time 25min; Washing: washing temperature 90℃, washing time 35min, adding 4% owf silicone oil softener SMI-60 during washing; Weaving: We selected a high-number single-sided circular machine for weaving, the machine number was 36G, the length of the grey fabric per hundred turns was 21.5cm, the untwisting device used included a yarn inlet porcelain mouth, four yarn threading holes, two yarn winding shafts, and a yarn outlet porcelain mouth. The yarn threading route was yarn inlet porcelain mouth → yarn threading hole → yarn winding shaft → yarn threading hole → yarn threading hole → yarn winding shaft → yarn threading hole → yarn outlet porcelain mouth; the yarn threading route of the untwisting device used is shown in the figure below: Figure 2As shown, the weaving pattern of the fabric is as follows Figure 1 As shown; Dyeing and finishing: The production process is singeing → washing → mercerizing → dyeing → stentering → pre-shrinking; The singeing speed is 65m / min, the singeing method is cutting and burning, and the flame intensity is 14mbar; Water washing speed 35m / min; Mercerizing uses a conventional mercerizing machine, with an alkali concentration of 12Be, a mercerizing speed of 25m / min, mercerizing overfeed of 20%, and a mercerizing washing temperature of 50℃; The dyeing process includes scouring, bleaching and dyeing, with a motor speed of 1000 r / min, a cloth lifting speed of 80 m / min, a nozzle opening size of 30%, soda ash 4 g / L, hydrogen peroxide 7 g / L, a leveling agent 1 g / L, sodium sulfate 8 g / L, a dyeing temperature of 55° C., a dyeing time of 30 min, a reactive blue dye of 0.0033% owf, a reactive red dye of 0.008% owf, and a reactive yellow dye of 0.007% owf; The tentering speed is 35m / min, the tentering pressure is 25bar, the tentering drying room temperature is 130℃, and the additives are: neutralized acid pH regulator PH-X 3g / L, silicone oil softener SMI-60 50g / L, and the balance is water; The pre-shrinking speed is 25m / min, and the pre-shrinking blanket temperature is 90℃.
[0046] The fabrics obtained in the examples and comparative examples were subjected to performance tests, and the test standards were as follows: Flatness AATCC 124-2018t method; Washing dimensional change rate GB / T 8628-2013 method; Pilling GB / T 4802.1-2008 E method; Snagging GB / T 11047-2008; Distortion after washing GB / T 23319.2-2009 method; Cool feeling GB / T 35263 method.
[0047] The test results are shown in Table 1.
[0048] Table 1 Fabric test data obtained from the embodiments and comparative examples
[0049] In comparative example 2, the untwisting device of the present invention was not used in weaving, and the cloth surface had serious holes and yarn twisting defects, and qualified rough cloth could not be woven. In comparative example 3, the modified mercerizing machine was not used, and the fabric dimensional stability was poor due to the sinking force caused by the water on the cloth surface.
Claims
1. A production process for knitting pique fabrics with high-count and high-twisted cotton yarns, characterized in that: Including the following processes: Spinning → yarn steaming → washing → weaving → dyeing and finishing; The spinning process: the yarn count is 100 s / 2 Strong twist yarn, twist coefficient is 450~550; The water washing step includes adding softener for water washing; The weaving process comprises: selecting a high-gauge single-sided large circular machine for weaving, the machine gauge is 32G-36G, the length of the grey cloth 100 turns is 21.5cm-22cm, the untwisting device used for weaving comprises a yarn inlet porcelain mouth, four yarn threading holes, two yarn winding shafts, and a yarn outlet porcelain mouth, and the yarn threading route is yarn inlet porcelain mouth→yarn threading hole→yarn winding shaft→yarn threading hole→yarn threading hole→yarn winding shaft→yarn threading hole→yarn outlet porcelain mouth; The dyeing and finishing process includes the following processes: Singeing → washing → mercerizing → dyeing → stentering → pre-shrinking; In the mercerizing machine used in the mercerizing process, the rollers in the needle plate area are replaced by mesh support belts.
2. The production process of knitted pique fabric made of pure cotton high count and strong twisted yarn according to claim 1, characterized in that: The raw material of the spinning process is 100% long-staple cotton, and the spinning method is compact spinning.
3. The production process of knitted pique fabric with high-count and strong-twisted cotton yarn according to claim 1, characterized in that: The yarn steaming process comprises a temperature of 95° C. to 105° C. and a time of 25 min to 35 min.
4. The production process of knitted pique fabric with high-count and strong-twisted cotton yarn according to claim 1, characterized in that: The water washing process: the water washing temperature is 90°C to 100°C, and the water washing time is 25min to 35min.
5. The production process of knitted pique fabric made of pure cotton high count and strong twisted yarn according to claim 1, characterized in that: The weaving process: the woven fabric structure is single bead ground.
6. The production process of knitted pique fabric with high-count and strong-twisted cotton yarn according to claim 1, characterized in that: The softener is a silicone oil softener, and the added amount is 4% owf to 5% owf.
7. The production process of knitted pique fabric with high-count and strong-twisted cotton yarn according to claim 1, characterized in that: The mercerizing process includes: mercerizing alkali concentration of 12Be~18Be, mercerizing machine speed of 25m / min~35m / min, mercerizing overfeed of 20%~30%, and mercerizing washing temperature of 50℃~70℃.
8. The production process of knitted pique fabric with high-count and strong-twisted cotton yarn according to claim 1, characterized in that: The singeing process includes: a vehicle speed of 65 m / min to 75 m / min, a cutting method for singeing, and a flame intensity of 10 mbar to 14 mbar.
9. The production process of knitted pique fabric with high-count and strong-twisted cotton yarn according to claim 1, characterized in that: The dyeing includes scouring, bleaching and dyeing, using an O-type overflow dyeing machine, with a motor speed of 1000 r / min~1500 r / min, a cloth lifting speed of 80 m / min~90 m / min, a nozzle opening size of 30%~40%, soda ash 4g / L~5g / L, hydrogen peroxide 7g / L~8g / L, a leveling agent 1g / L~3g / L, alumina sulfate 8g / L~12g / L, a dyeing temperature of 55°C~65°C, and a dyeing time of 30min~50min.
10. A cotton high-count strong twist yarn knitted pique fabric, characterized in that: The product is produced by the production process described in any one of claims 1 to 9.
Citation Information
Patent Citations
Method for reducing twist contraction knots of all-cotton over-twisted yarns
CN101671926A
Cool-to-touch breathable dry washable smooth all-cotton fabric and manufacture method thereof
CN102808335A
Production process of polyester-cotton anti-wrinkle easy-care high-density knitted fabric for suits
CN107419418A
Food intelligent baking system based on control of Internet of Things
CN109197927A
Weaving, printing and dyeing process of rose fiber clothing fabric
CN112080885A
Cited By
Production method of heavy-twist high-count low-hairiness yarn and yarn
CN119433776A